A high carbon steel and its ultra-clean smelting process

Through the vacuum induction furnace double furnace smelting process and the use of high-purity raw materials, the content of alumina inclusions in high-carbon steel was successfully reduced, the problem of high-pulse wire breaking rate was solved, and the production of high-quality diamond wire busbars was realized .

CN118480747BActive Publication Date: 2024-11-26INST OF RES OF IRON & STEEL JIANGSU PROVINCE +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410926290.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-26
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

现有技术中高碳钢盘条在拉拔过程中因非金属夹杂物氧化铝导致断丝现象,降低成材率并提高生产成本,且现有真空感应熔炼工艺难以有效控制氧化铝夹杂物。

Method used

The vacuum induction furnace is used to perform the double furnace smelting process. The first furnace is dealuminized through the aluminum oxide reaction, and the second furnace is dealuminized through the carbon oxygen reaction during the manganese alloying process to produce an aluminum content of less than 0.0005% and a low oxygen content. At 0.001% high-carbon steel, high-purity raw materials such as industrial pure iron, polysilicon and metal chromium are used, and a crucible refractory material with low Al2O3 content is designed to avoid pollution.

Benefits of technology

It significantly reduces the pulling and wire breaking rate of the diamond wire busbar, and produces ultra-clean high-carbon steel with very small amounts of alumina inclusions. It is suitable for the preparation of high-quality diamond wire busbars, which improves the yield rate and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention provides a high carbon steel and an ultra-clean smelting process thereof, which relates to the field of steel smelting; a double-furnace smelting process is adopted, the first furnace is dealuminated by oxygen-aluminum reaction, and the second furnace is deoxidized by carbon-oxygen reaction while completing manganese alloying, so as to produce ultra-clean high carbon steel with an aluminum content of less than 0.0005% and an oxygen content of less than 0.001%; ​​the high carbon steel includes the following components in mass percentage: C1.0-1.1%, Si 0.4-0.5%, Mn 0.6-0.7%, Cr 0.3-0.4%, Al≤0.0005%, O≤0.001%, N≤0.001%, S≤0.005%, P≤0.005%, and the remainder is Fe and unavoidable impurity elements. The present invention can effectively solve the problem of high wire breakage rate caused by excessive number and oversize of alumina inclusions in the drawing process of high carbon steel wire rod for diamond wire busbar.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel smelting, and in particular to high-carbon steel and an ultra-clean smelting process thereof. Background Art

[0002] In recent years, the photovoltaic industry has developed rapidly, and the demand for its upstream silicon wafers has shown an explosive growth trend. The production of silicon wafers is inseparable from cutting. Diamond cutting wire (referred to as diamond wire) saw cutting technology has a dominant position in silicon wafer cutting technology due to its advantages of high efficiency, low cost and low pollution. Competition within the photovoltaic industry is becoming increasingly fierce. Silicon wafer processing companies hope to reduce production costs and material losses, and require diamond wire refinement. In the process of diamond wire refinement technology development, the refinement of diamond wire busbar plays a decisive role. Diamond wire busbar is made of high-carbon steel wire rod through a series of processes such as heat treatment, drawing, and electroplating. Wire breakage will occur during the drawing process, reducing the yield rate and increasing production costs. There are many factors that affect wire breakage during drawing, and non-metallic inclusions are the most important reason. The hard and brittle aluminum oxide in non-metallic inclusions has a particularly obvious effect on wire breakage during drawing. Therefore, in order to reduce the wire breakage rate of high-carbon steel wire rods used for diamond wire busbars, the control of aluminum oxide inclusions is very important.

[0003] The prior art adopts vacuum induction melting / vacuum induction melting furnace (VIM / VIDP) → vacuum arc remelting (VAR) → forging → high wire rolling process to produce high carbon steel wire rod for diamond wire busbar, wherein the VIM / VIDP process is the key step for inclusion control. Patent CN108866433A in the prior art discloses a high carbon, low aluminum, low oxygen cutting wire steel and its vacuum induction melting method, the chemical composition of which includes, by mass percentage: C 0.9-0.94%, Si 0.12-0.3%, Mn 0.3-0.65%, Cr 0.1-0.3%, Al≤0.004%, O≤0.003%, N≤0.0025%, S≤0.01%, P≤0.01%, the remainder is Fe and unavoidable impurity elements. By controlling the order and timing of carbon addition, the chamber pressure at different smelting stages, and low-temperature refining at 1540±5℃, the purpose of using a vacuum induction furnace alumina crucible to melt high-carbon, low-aluminum, and low-oxygen steel for cutting wire is achieved. Summary of the invention

[0004] The object of the present invention is to provide a high carbon steel and an ultra-clean smelting process thereof, using a vacuum induction furnace, selecting raw materials, and adopting a double-furnace smelting process. The first furnace is dealuminated by oxygen-aluminum reaction, and the second furnace is deoxidized by carbon-oxygen reaction while completing manganese alloying, so as to produce ultra-clean high carbon steel with an aluminum content of less than 0.0005% and an oxygen content of less than 0.001%.

[0005] To achieve the above object, the present invention proposes the following technical solutions:

[0006] In a first aspect, a high carbon steel is proposed, comprising the following components in mass percentage: C 1.0-1.1%, Si 0.4-0.5%, Mn 0.6-0.7%, Cr 0.3-0.4%, Al<0.0005%, O<0.001%, N≤0.001%, S≤0.005%, P≤0.005%, and the balance is Fe and unavoidable impurity elements.

[0007] Furthermore, the raw materials for preparing the high carbon steel include: industrial pure iron, polysilicon, electrolytic manganese and metallic chromium, wherein the mass percentage of the main element of any raw material is greater than 99.9%, and the mass percentage of the aluminum element is less than 0.001%.

[0008] Furthermore, the average size of the aluminum oxide inclusions in the high carbon steel does not exceed 1.3 μm, and the number of aluminum oxide inclusions does not exceed 0.4 / mm. 2 .

[0009] Secondly, an ultra-clean smelting process for high carbon steel is proposed, in which a vacuum induction furnace is used for double-furnace smelting. The first furnace smelting is carried out for dealumination through oxygen-aluminum reaction, and the second furnace smelting is carried out for manganese alloying and deoxidation through carbon-oxygen reaction, to produce high carbon steel with an aluminum mass percentage of less than 0.0005% and an oxygen mass percentage of less than 0.001%.

[0010] Furthermore, the process of dealumination by oxygen-aluminum reaction in the first smelting heat comprises the following steps:

[0011] Put the raw materials of industrial pure iron, polysilicon and metallic chromium into the crucible of the vacuum induction furnace, and extract the air in the furnace to reduce the pressure in the furnace to 10-20Pa;

[0012] Power is supplied to the vacuum induction furnace according to the process curve, and when the power supply reaches 70-80% of the rated power, oxygen is filled into the furnace to make the pressure inside the furnace reach 20000-25000Pa, and the raw materials are melted in the oxygen atmosphere to carry out oxygen-aluminum reaction;

[0013] After the raw materials are fully melted, they are kept warm for 20 to 30 minutes, and the power supply is controlled to be 50 to 60% of the rated power to discharge the aluminum oxide produced by the oxygen-aluminum reaction;

[0014] After the heat preservation is completed, the oxygen in the furnace is extracted to reduce the pressure in the furnace to 10-20 Pa, and after the temperature of the molten steel is controlled to reach the first preset target, carbon particles accounting for 0.01-0.02% of the total weight of the raw materials for smelting high-carbon steel are added to the molten steel to perform the first micro-carbon alloying and complete the first deoxidation;

[0015] Control the pressure in the furnace to 10-20Pa for refining, the refining temperature to 1580-1590℃, and the refining time to 20-25min to complete the second deoxidation;

[0016] The power is turned off until the surface of the molten steel forms a film, and after the film forms, carbon particles accounting for 0.02-0.03% of the total weight of the raw materials for smelting high-carbon steel are added to the molten steel to perform a second micro-carbon alloying and complete the third deoxidation;

[0017] After the carbon particles are fully melted, the temperature of the molten steel is controlled at 1535-1545°C, and low-temperature vacuum carbon-oxygen reaction deoxidation is carried out for 20-25 minutes to complete the fourth deoxidation;

[0018] After the low-temperature vacuum carbon-oxygen reaction is completed, the temperature of the molten steel rises to the pouring temperature of 1560-1570°C and is poured into steel ingots.

[0019] Furthermore, the process of performing manganese alloying and deoxidation by carbon-oxygen reaction in the second heat smelting comprises the following steps:

[0020] The first smelting product and carbon particles accounting for 0.05-0.07% of the total raw material weight of smelting high carbon steel are loaded into the crucible of the vacuum induction furnace, and the air in the furnace is evacuated to reduce the pressure in the furnace to 10-20 Pa;

[0021] According to the process curve, the vacuum induction furnace is powered, and the initial charge is melted under relative vacuum conditions to carry out carbon-oxygen reaction and complete the first deoxidation;

[0022] When the temperature of the molten steel rises to a second preset target, carbon particles are added at a weight percentage of 1.03-1.05% of the total raw material weight of the smelting high-carbon steel to perform carbon alloying and complete the second deoxidation;

[0023] Control the pressure in the furnace to 10-20Pa for refining, the refining temperature to 1550-1560℃, and the refining time to 15-20min to complete the third deoxidation;

[0024] Cut off the power supply until the steel liquid surface forms a film, and fill the furnace with argon gas to raise the pressure inside the furnace to 18000-20000Pa;

[0025] Adding raw material metal manganese into the furnace filled with argon to carry out manganese alloying reaction;

[0026] After the composition of the molten steel is determined to meet the target composition requirements, high carbon steel is cast when the temperature of the molten steel is reduced to a pouring temperature of 1540-1560°C.

[0027] Furthermore, the crucible of the vacuum induction furnace includes the following chemical components in mass percentage: CaO ≥97%, MgO ≤1%, SiO2 ≤0.2%, Al2O3 ≤0.05%, and CeO2 0.8-1.75%.

[0028] Furthermore, the target composition is required to include the following components in mass percentage: C 1.0-1.1%, Si 0.4-0.5%, Mn 0.6-0.7%, Cr 0.3-0.4%, Al<0.0005%, O<0.001%, N≤0.001%, S≤0.005%, P≤0.005%, and the balance is Fe and unavoidable impurity elements.

[0029] Furthermore, during the first furnace smelting process, the raw materials are melted at a melting speed of 2 to 3 kg / min in an oxygen atmosphere by adjusting the power supply.

[0030] Furthermore, during the second furnace smelting process, the melting rate of the initial charge is controlled to be 3-4 kg / min by adjusting the power supply.

[0031] It can be seen from the above technical solutions that the technical solutions of the present invention have the following beneficial effects:

[0032] The high carbon steel and the ultra-clean smelting process disclosed in the present invention include the following components in mass percentage: C 1.0-1.1%, Si 0.4-0.5%, Mn 0.6-0.7%, Cr 0.3~0.4%, Al<0.0005%, O<0.001%, N≤0.001%, S≤0.005%, P≤0.005%, and the balance is Fe and inevitable impurity elements; the process adopts a vacuum induction furnace for double-furnace smelting, the first furnace smelting is dealumened by oxygen-aluminum reaction, and the second furnace smelting is manganese alloyed and deoxidized by carbon-oxygen reaction to obtain high-carbon steel with an aluminum mass percentage of less than 0.0005% and an oxygen mass percentage of less than 0.001%; ​​the present invention uses a vacuum induction furnace to explore the control process of aluminum and oxygen content in ultra-clean high-carbon steel, the high-carbon steel obtained by the process has extremely low oxygen and aluminum contents, and a small number of alumina inclusions, which effectively reduces its drawing breakage rate, and is suitable for preparing ultra-high-quality diamond wire busbars.

[0033] In addition, the present invention designs a special crucible refractory material based on the technical characteristics of ultra-clean high-carbon steel. The Al2O3 content of this crucible refractory material is extremely low, thus avoiding the contamination of molten steel by Al2O3 in the crucible refractory material.

[0034] It should be appreciated that all combinations of the foregoing concepts, as well as additional concepts described in greater detail below, may be considered to be part of the inventive subject matter of the present disclosure, provided such concepts are not mutually inconsistent.

[0035] The foregoing and other aspects, embodiments and features of the present invention can be more fully understood from the following description in conjunction with the embodiments. Other additional aspects of the present invention, such as the features and / or beneficial effects of the exemplary embodiments, will be apparent from the following description or learned from the practice of the specific embodiments according to the present invention. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme of the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the described embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be the common meanings understood by people with general skills in the field to which the present invention belongs.

[0037] The words "first", "second" and similar words used in the patent application specification and claims of the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, unless the context clearly indicates otherwise, the singular form of "a", "an" or "the" and other similar words do not indicate a quantitative limitation, but indicate the existence of at least one. "Include" or "comprises" and other similar words mean that the elements or objects appearing before "include" or "comprises" include the features, wholes, steps, operations, elements and / or components listed after "include" or "comprises", and do not exclude the existence or addition of one or more other features, wholes, steps, operations, elements, components and / or their collections.

[0038] In the prior art, the diamond wire busbar is made of high carbon steel wire rod through a series of process steps such as heat treatment, drawing, and electroplating. Due to the influence of hard and brittle alumina as non-metallic inclusions, the diamond wire busbar may break during the drawing process, which reduces the yield rate, increases the production cost, and further affects the silicon wafer production efficiency. The present invention aims to propose a high carbon steel and an ultra-clean melting process thereof, which adopts a double-furnace melting process to reduce the amount of alumina inclusions in the high carbon steel wire rod for the diamond wire busbar and reduce its wire breakage rate during drawing.

[0039] Specifically, the high carbon steel includes the following components in mass percentage: C 1.0-1.1%, Si 0.4-0.5%, Mn 0.6-0.7%, Cr 0.3-0.4%, Al<0.0005%, O<0.001%, N≤0.001%, S≤0.005%, P≤0.005%, and the balance is Fe and unavoidable impurity elements; the ultra-clean smelting process of the high carbon steel is as follows: a vacuum induction furnace is used for double-furnace smelting, the first furnace smelting is dealuminated by oxygen-aluminum reaction, and the second furnace smelting is performed for manganese alloying and deoxidation by carbon-oxygen reaction, so as to obtain high carbon steel with an aluminum mass percentage of less than 0.0005% and an oxygen mass percentage of less than 0.001%.

[0040] Specifically, the process of dealumination through oxygen-aluminum reaction in the first furnace smelting includes the following steps: loading raw materials of industrial pure iron, polysilicon and metallic chromium into the crucible of the vacuum induction furnace, and extracting the air in the furnace to reduce the pressure in the furnace to 10-20Pa; supplying power to the vacuum induction furnace according to the process curve, and when the power supply reaches 70-80% of the rated power, filling oxygen into the furnace to make the pressure in the furnace reach 20000-25000Pa, oxygen is used as an oxygenating agent, and the power supply is adjusted in an oxygen atmosphere to control the melting speed to 2-3 kg / min to melt the raw materials, ensuring that oxygen is fully dissolved in the molten steel for oxygen-aluminum reaction; after the raw materials are fully melted, they are kept warm for 20-30 minutes, and the power supply is controlled to be 50-60% of the rated power to fully discharge the aluminum oxide product of the oxygen-aluminum reaction; after the insulation is completed, the oxygen in the furnace is extracted to reduce the pressure in the furnace to 10-20 Pa, and after the temperature of the molten steel reaches the first preset target, carbon particles accounting for 0.01-0.02% of the total weight and mass percentage of the raw materials for smelting high carbon steel are added to the molten steel to perform the first micro-carbon alloying and complete the first deoxidation; the pressure in the furnace is controlled to be 10-20Pa for refining, the refining temperature is 1580-1590℃, and the refining time is 20-25 min to complete the second deoxidation; the power is turned off until the surface of the molten steel forms a film, and after the film forms, carbon particles accounting for 0.02-0.03% of the total weight and mass percentage of the raw materials for smelting high carbon steel are added to the molten steel to perform the second micro-carbon alloying and complete the third deoxidation; low-temperature vacuum carbon-oxygen reaction deoxidation is performed for 20-25 min to complete the fourth deoxidation; after the low-temperature vacuum carbon-oxygen reaction is completed, the temperature of the molten steel is raised to the pouring temperature of 1560-1570℃, and it is poured into a steel ingot.

[0041] The process of performing manganese alloying and deoxidation by carbon-oxygen reaction in the second smelting process comprises the following steps: loading the smelting product of the first smelting process and carbon particles accounting for 0.05-0.07% of the total weight of the raw materials for smelting high-carbon steel into a crucible of a vacuum induction furnace, and extracting the air in the furnace to reduce the pressure in the furnace to 10-20 Pa; supplying power to the vacuum induction furnace according to the process curve, and melting the initial charge under relative vacuum conditions, and controlling the melting speed of the initial charge to 3-4 by adjusting the power supply; kg / min, carbon oxygen reaction is carried out to complete the first deoxidation; when the temperature of the molten steel rises to the second preset target, carbon particles accounting for 1.03-1.05% of the total weight mass percentage of the raw materials for smelting high carbon steel are added to carry out carbon alloying to complete the second deoxidation; the pressure in the furnace is controlled to be 10-20Pa for refining, the refining temperature is 1550-1560℃, and the refining time is 15-20min to complete the third deoxidation; the power is turned off until the surface of the molten steel forms a film, and argon is filled into the furnace to increase the pressure in the furnace to 18000-20000Pa; raw material metal manganese is added into the furnace after argon is filled to carry out manganese alloying reaction; after the composition of the molten steel is determined to meet the target composition requirements, when the temperature of the molten steel is reduced to the pouring temperature of 1540-1560℃, high carbon steel is cast.

[0042] The contamination of molten steel by Al2O3 in the crucible of the vacuum induction furnace is avoided. Aiming at this type of steel, the present invention designs a special crucible refractory material, the chemical composition of which is shown in Table 1 below. The Al2O3 content of the crucible refractory material is extremely low.

[0043] Table 1 Mass percentage of each chemical component of crucible refractory

[0044]

[0045] At the same time, in order to avoid introducing more impurities into the molten steel, the present invention selects raw materials, which are industrial pure iron, polysilicon, electrolytic manganese and metallic chromium. The mass percentage of the main elements of each raw material is greater than 99.9%, and the mass percentage of aluminum element is less than 0.0010%.

[0046] The high carbon steel and the ultra-clean smelting process thereof disclosed in the present invention will be further specifically introduced below in conjunction with specific embodiments.

[0047] Example 1

[0048] A vacuum induction furnace is used, and a double-furnace melting process is adopted. In the first furnace, oxygen is used as an oxygenating agent to dealuminate through oxygen-aluminum reaction. The specific steps are:

[0049] (1) Charging: All the purified industrial pure iron, polysilicon and metallic chromium are loaded into the crucible. The mass percentage of the chemical components in the crucible is CaO 97.5%, MgO 0.8%, SiO2 0.1%, Al2O3 0.04%, CeO2 1.56%.

[0050] (2) Vacuuming: Extract the air in the furnace so that the pressure inside the furnace reaches 10 Pa.

[0051] (3) Power on: Power is supplied according to the process curve.

[0052] (4) Oxygen supply: When the power supply reaches 75% of the rated power, oxygen is filled into the furnace to make the pressure inside the furnace reach 25000Pa.

[0053] (5) Melting of initial charge: Melt the initial charge in an oxygen atmosphere, adjust the power supply, and control the melting speed to 2.5 kg / min to ensure that oxygen is fully dissolved in the molten steel and complete the oxygen-aluminum reaction.

[0054] (6) Insulation: After the initial charge is fully melted, the heat is maintained for 23 minutes. At this time, the power transmission reaches 57% of the rated power, and the aluminum oxide product of the oxygen-aluminum reaction is fully discharged.

[0055] (7) Vacuuming: After complete melting, the oxygen in the furnace is extracted to reduce the pressure in the furnace to 10 Pa.

[0056] (8) Temperature measurement: After the temperature of the molten steel is raised to a certain level, the temperature is measured to determine whether the temperature of the molten steel has reached the first preset target, which is 1587 °C.

[0057] (9) First micro-carbon alloying: Add carbon particles with a weight percentage of 0.02% of the total raw material weight for smelting high carbon steel into the molten steel to complete the first deoxidation.

[0058] (9) Refining: During refining, the furnace pressure is 10 Pa, the refining temperature is 1587 °C, the refining time is 25 min, and the second deoxidation is completed.

[0059] (10) Power failure filming: The power is cut off until the film forms on the surface of the molten steel.

[0060] (11) Second micro-carbon alloying: Add carbon particles with a weight percentage of 0.03% of the total raw material weight for smelting high carbon steel into the molten steel to complete the third deoxidation.

[0061] (12) Low-temperature degassing: Low-temperature vacuum carbon-oxygen reaction deoxidation for 25 minutes to complete the fourth deoxidation.

[0062] (13) Temperature measurement and pouring: Before pouring, measure the temperature of the molten steel to ensure that the temperature of the pure iron liquid is 1543 ℃ and pour it into a 60 mm diameter steel ingot.

[0063] The second batch of heat completes the manganese alloying and deoxidizes through carbon-oxygen reaction. The specific steps are:

[0064] (1) Charging: The steel ingots cast in the first batch and carbon particles accounting for 0.06% by weight of the total raw materials for smelting high carbon steel are all charged into the crucible.

[0065] (2) Vacuuming: Extract the air in the furnace so that the pressure inside the furnace reaches 10 Pa.

[0066] (3) Power on: Power is supplied according to the process curve.

[0067] (4) Melting of initial charge: Melt the initial charge under vacuum conditions, adjust the power supply, and control the melting speed to 3 kg / min to ensure that the carbon-oxygen reaction proceeds fully and complete the first deoxidation.

[0068] (5) Temperature measurement: After the temperature of the molten steel rises to a certain level, the temperature is measured and the temperature of the molten steel is controlled to rise to the second preset target. At this time, the temperature of the molten steel is 1560 °C.

[0069] (6) Carbon alloying: Add carbon particles accounting for 1.03% by weight of the total raw materials for smelting high carbon steel to complete the second deoxidation.

[0070] (7) Refining: During refining, the furnace pressure is 10 Pa, the refining temperature is 1560 °C, the refining time is 20 min, and the third deoxidation is completed.

[0071] (8) Power-off filming: The power is turned off until filming forms on the surface of the molten steel.

[0072] (9) Argon filling: Argon gas is filled into the furnace to make the pressure inside the furnace reach 20,000 Pa.

[0073] (10) Manganese alloying: All the metallic manganese in the raw materials is added to carry out manganese alloying reaction.

[0074] (11) Temperature measurement and pouring: The molten steel is poured after its composition meets the requirements. The temperature of the molten steel is measured before pouring to ensure that the temperature of the pure iron liquid is 1560 °C and then poured into a 60 mm diameter steel ingot.

[0075] The chemical composition and inclusions of the steel ingots produced in the second batch were measured. The chemical composition results are shown in Table 2 below. High carbon steel can be controlled: the mass percentage of aluminum is less than 0.0005%, the mass percentage of oxygen is less than 0.001%, and the remaining components also meet the requirements of high carbon steel.

[0076] Table 2 Chemical composition of high carbon steel (mass percentage)

[0077]

[0078] The steel ingot samples were extracted and sampled, and then statistical analysis of inclusions was performed under a scanning electron microscope. The analysis area was 30 mm 2 The number, size and type of inclusions were statistically analyzed using the inclusion analysis software provided by the scanning electron microscope. The results showed that there were no alumina inclusions larger than 3 μm inside the ingot. The average size of the alumina inclusions inside the ingot was 0.9 μm, the average size did not exceed 1.3 μm, and the density was about 0.3 / mm 2 , that is, the number of alumina inclusions does not exceed 0.4 / mm 2 ; Effectively solve the problem of high wire breakage rate caused by excessive number and large size of alumina inclusions in the drawing process of high carbon steel wire rod for diamond wire busbar in the prior art.

[0079] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. A person with ordinary knowledge in the technical field to which the present invention belongs may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be determined by the definition of the claims.

Claims

1. A high carbon steel ultra-clean smelting process, characterized in that: A vacuum induction furnace is used for double-heat smelting, the first smelting heat is dealuminated by oxygen-aluminum reaction, and the second smelting heat is used for manganese alloying and deoxidation by carbon-oxygen reaction, so as to obtain high carbon steel with aluminum mass percentage less than 0.0005% and oxygen mass percentage less than 0.001%; The process of dealumination by oxygen-aluminum reaction in the first smelting heat comprises the following steps: Put the raw materials of industrial pure iron, polysilicon and metallic chromium into the crucible of the vacuum induction furnace, and extract the air in the furnace to reduce the pressure in the furnace to 10-20Pa; Power is supplied to the vacuum induction furnace according to the process curve, and when the power supply reaches 70-80% of the rated power, oxygen is filled into the furnace to make the pressure inside the furnace reach 20000-25000Pa, and the raw materials are melted in the oxygen atmosphere to carry out oxygen-aluminum reaction; After the raw materials are fully melted, they are kept warm for 20 to 30 minutes, and the power supply is controlled to be 50 to 60% of the rated power to discharge the aluminum oxide produced by the oxygen-aluminum reaction; After the heat preservation is completed, the oxygen in the furnace is extracted to reduce the pressure in the furnace to 10-20 Pa, and after the temperature of the molten steel is controlled to reach the first preset target, carbon particles accounting for 0.01-0.02% of the total weight of the raw materials for smelting high-carbon steel are added to the molten steel to perform the first micro-carbon alloying and complete the first deoxidation; Control the pressure in the furnace to 10-20Pa for refining, the refining temperature to 1580-1590℃, and the refining time to 20-25 minutes to complete the second deoxidation; The power is turned off until the surface of the molten steel forms a film, and after the film forms, carbon particles accounting for 0.02-0.03% of the total weight of the raw materials for smelting high-carbon steel are added to the molten steel to perform a second micro-carbon alloying and complete the third deoxidation; After the carbon particles are fully melted, the temperature of the molten steel is controlled at 1535-1545°C, and low-temperature vacuum carbon-oxygen reaction deoxidation is carried out for 20-25 minutes to complete the fourth deoxidation; After the low-temperature vacuum carbon-oxygen reaction is completed, the temperature of the molten steel rises to the pouring temperature of 1560-1570°C and is poured into steel ingots.

2. The ultra-clean smelting process for high carbon steel according to claim 1, characterized in that: The process of performing manganese alloying and deoxidation by carbon-oxygen reaction in the second heat smelting comprises the following steps: The first smelting product and carbon particles accounting for 0.05-0.07% of the total raw material weight of smelting high carbon steel are loaded into the crucible of the vacuum induction furnace, and the air in the furnace is evacuated to reduce the pressure in the furnace to 10-20 Pa; According to the process curve, the vacuum induction furnace is powered, and the initial charge is melted under relative vacuum conditions to carry out carbon-oxygen reaction and complete the first deoxidation; When the temperature of the molten steel rises to a second preset target, carbon particles are added at a weight percentage of 1.03-1.05% of the total raw material weight of the smelting high-carbon steel to perform carbon alloying and complete the second deoxidation; Control the pressure in the furnace to 10-20Pa for refining, the refining temperature to 1550-1560℃, and the refining time to 15-20min to complete the third deoxidation; Cut off the power supply until the steel liquid surface forms a film, and fill the furnace with argon gas to raise the pressure inside the furnace to 18000-20000Pa; Adding raw material metal manganese into the furnace filled with argon to carry out manganese alloying reaction; After the composition of the molten steel is determined to meet the target composition requirements, high carbon steel is cast when the temperature of the molten steel is reduced to a pouring temperature of 1540-1560°C.

3. The ultra-clean smelting process for high carbon steel according to claim 1 or 2, characterized in that: The crucible of the vacuum induction furnace includes the following chemical components in mass percentage: CaO ≥97%, MgO ≤1%, SiO2 ≤0.2%, Al2O3 ≤0.05%, and CeO2 0.8-1.75%.

4. The ultra-clean smelting process for high carbon steel according to claim 2, characterized in that: The target composition requirements of the high carbon steel include the following components in mass percentage: C 1.0-1.1%, Si 0.4-0.5%, Mn 0.6-0.7%, Cr 0.3-0.4%, Al<0.0005%, O<0.001%, N≤0.001%, S≤0.005%, P≤0.005%, and the balance is Fe and unavoidable impurity elements.

5. The ultra-clean smelting process for high carbon steel according to claim 1, characterized in that: During the first smelting process, the raw materials are melted at a melting speed of 2 to 3 kg / min in an oxygen atmosphere by adjusting the power supply.

6. The ultra-clean smelting process for high carbon steel according to claim 2, characterized in that: During the second furnace smelting process, the melting rate of the initial charge is controlled to be 3-4 kg / min by adjusting the power supply.

7. The ultra-clean smelting process for high carbon steel according to claim 2, characterized in that: The raw materials of the high carbon steel, industrial pure iron, polysilicon, electrolytic manganese and metallic chromium, have a main element mass percentage greater than 99.9% and an aluminum element mass percentage less than 0.001%.

8. The ultra-clean smelting process for high carbon steel according to claim 1, characterized in that: The average size of the aluminum oxide inclusions in the high carbon steel does not exceed 1.3 μm, and the number of aluminum oxide inclusions does not exceed 0.4 / mm 2 .