A magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal and its preparation method and application
By co-doping magnesium and thallium into zero-dimensional perovskite halide scintillation single crystals, the problem of low Tl-bound exciton emission efficiency in the Cs3Cu2I5:Tl series crystals is solved, and efficient light yield and energy resolution are achieved, which is suitable for many applications. field application.
Patent Information
- Application Number
- CN202410911528.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-09
AI Technical Summary
The emission efficiency of Tl-bound excitons in Cs3Cu2I5:Tl series crystals at room temperature is low, resulting in insufficient light yield and energy resolution.
The zero-dimensional perovskite halide scintillation single crystal is co-doped with magnesium and thallium. The general chemical formula is (Cs1-x-y-zTlxMgyAz)3(Cu1-mBm)2(I1-nXn), using the Bridgeman descent method or horizontal Prepared by directional solidification method, Mg ions are introduced to improve the emission efficiency of Tl ions at room temperature.
It significantly improves the emission efficiency of Tl-bound excitons at room temperature, improves light yield and energy resolution, and is suitable for nuclear medical imaging, homeland security and high-energy physics fields.
Smart Images

Figure CN118480865B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of radiation detection and X-ray imaging, and in particular relates to a magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal and a preparation method and application thereof. Background Art
[0002] Scintillator crystals can convert high-energy particles into luminescence in the ultraviolet-visible light band. As the core component of radiation detectors, they are widely used in many fields. In nuclear medicine imaging, high-performance scintillator crystals are the core components for achieving high-resolution imaging; in the field of land and social security, scintillator crystals are widely used in dangerous nuclide identification and public security inspection equipment; high-energy physics and deep space exploration applications also require a large number of scintillator crystals to detect high-energy rays and particles. With the continuous growth of application space and the rapid improvement of technical requirements, the further optimization of key parameters such as light yield, energy resolution, scintillation decay time and stability of scintillator crystals has attracted widespread attention.
[0003] Recently, metal halide scintillators with low-dimensional molecular structures have attracted widespread attention as efficient luminescent materials. These low-dimensional halides have strong quantum confinement effects and obtain strong electron-phonon coupling through the confinement effect, which reduces the probability of defect capture of carriers and the emission of self-trapped excitons generated by the soft lattice, making the crystals have high quantum efficiency and low self-absorption luminescence characteristics. In addition, these low-dimensional metal halides also tend to have lower melting points and higher air and thermal stability, which is of great significance for low-cost production and application. Among them, copper-based low-dimensional halides are a type of excellent scintillating crystals with efficient confined exciton luminescence. Taking zero-dimensional Cs3Cu2I5 as an example, it has the advantages of non-deliquescent, low self-absorption, low melting point, high light yield (38000 ph. / MeV) and high energy resolution (4.8%@662 keV), and it has been found that the Tl bound exciton effect produced after Tl ion doping can effectively improve the exciton radiative recombination efficiency, thereby significantly improving the light yield (87000 ph. / MeV) and energy resolution (3.4%@662 keV), which has great application prospects. However, the Tl ion bound exciton effect shows emission at 510nm and 560nm in Cs3Cu2I5 crystals at low temperature (78K), but only emission at 510nm appears at room temperature, which reduces the emission efficiency of Tl bound excitons at room temperature. Summary of the invention
[0004] Aiming at the problem of low emission efficiency of Tl bound excitons in Cs3Cu2I5:Tl series crystals at room temperature, the present invention provides a magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal and a preparation method and application thereof.
[0005] In a first aspect, the present invention provides a magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal, wherein the magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal has a chemical formula of (Cs 1-x-y-z Tl x Mg y A z )3(Cu 1-m B m )2(I 1-n X n )5; wherein: A = at least one of Na, K, and Rb; B = at least one of Ag, Li, and Au; X = at least one of Cl and Br; and 0<x<1, 0<y≤0.02, 0≤z<1, 0<x + y + z<1, 0≤m≤1, and 0≤n≤1.
[0006] In the present invention, a more efficient emission of Tl bound excitons of low-dimensional metal halide scintillators is achieved by co-doping with magnesium and thallium, and it is expected to obtain a scintillating crystal that combines low self-absorption, low defect capture probability, high luminescence efficiency, etc. Compared with the existing low-dimensional structured halide scintillating crystals, which can obtain higher carrier utilization efficiency and scintillation efficiency, Mg / Tl ion co-doped low-dimensional halide scintillating crystals may provide a better scintillating crystal candidate for the fields of nuclear medical imaging, homeland and social security, high energy physics and deep space exploration.
[0007] Preferably, x=0.001-0.05; or / and y=0.001-0.015.
[0008] Preferably, x=0.01; or / and y=0.001-0.01.
[0009] Preferably, the light yield of the magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal under gamma rays is at least 80,000 Ph. / MeV; the light yield of the magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal under X-rays is 155,000 Ph. / MeV to 190,000 Ph. / MeV.
[0010] Preferably, the decay time of the magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal is 300-740ns.
[0011] Preferably, the energy resolution of the magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal is 3.4-4.5%.
[0012] In a second aspect, the present invention provides a method for preparing a magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal, comprising:
[0013] (1) weighing and mixing halide powders according to a general chemical formula to obtain raw material powders;
[0014] (2) The obtained raw material powder is sealed and placed in a crucible, and a magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal is obtained by using a Bridgman descent method or a horizontal directional solidification method.
[0015] Preferably, the halide powder includes: CsX, TlX, MgX2, CuX2, BX; the purity of the halide powder is ≥99.9%; and the atmosphere inside the crucible is a vacuum atmosphere.
[0016] Preferably, the parameters of the Bridgman descent method include: a melting temperature of 400-600°C until the raw material powder is completely melted; a bottom temperature of the crucible reaches 330-400°C; and a crucible descent rate of 0.3-1.0 mm / h.
[0017] Preferably, the parameters of the horizontal directional solidification method include a melting temperature of 400-600°C until the raw material powder is completely melted; a bottom temperature of the crucible reaches 330-400°C; and a horizontal movement rate of the crucible is 0.3-1.0 mm / h.
[0018] Preferably, the crucible is a crucible with a capillary bottom; the crucible includes a quartz crucible, a platinum crucible or a graphite crucible.
[0019] In a third aspect, the present invention provides an application of a magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal in X-ray imaging, gamma-ray and neutron detection.
[0020] Beneficial effects of the present invention:
[0021] In the present invention, the magnesium-thallium co-doped zero-dimensional perovskite halide scintillating crystal has low raw material cost, high chemical stability, low melting point, and is easy to prepare. In addition, the introduction of Mg ions constructs a new defect energy level, thereby promoting Tl ions to achieve double bound exciton emission at room temperature, improving the luminous efficiency of Tl bound exciton emission at room temperature, greatly improving the light yield of the crystal under steady-state X-ray irradiation, and accelerating the scintillation decay time under gamma ray irradiation. The magnesium-thallium co-doped zero-dimensional perovskite halide scintillating crystal has great application prospects in the fields of X-ray imaging and radiation detection. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The (Cs 0.99-y Tl 0.01 Mg y )Sample photo of 3Cu2I5 halide scintillating single crystal under natural light;
[0023] Figure 2 The (Cs 0.989 Tl 0.01 Mg0.001 )Photoluminescence spectrum of 3Cu2I5 halide scintillating single crystal;
[0024] Figure 3 The (Cs 0.99-y Tl 0.01 Mg y )3Cu2I5 halide scintillating single crystal and (Cs 0.99 Tl 0.01 )3Absorption spectrum of Cu2I5 halide scintillating single crystal;
[0025] Figure 4 The (Cs 0.99-y Tl 0.01 Mg y )3Cu2I5 halide scintillating single crystal and (Cs 0.99 Tl 0.0 1) X-ray irradiation luminescence spectrum of 3Cu2I5 halide scintillating single crystal;
[0026] Figure 5 The (Cs 0.989 Tl 0.01 Mg 0.001 )3Cu2I5 halide scintillating single crystal scintillation decay time curve;
[0027] Figure 6 The (Cs 0.99 Tl 0.01 )3Cu2I5 halide scintillating single crystal scintillation decay curve;
[0028] Figure 7 The photoluminescence spectrum of the Cs3Cu2I5 halide scintillating single crystal obtained in Comparative Example 2 is shown;
[0029] Figure 8 The control example (Na 0.91 6 Li 0.08 Tl 0.01 )I and (Na 0.904 6 Li 0.08 Tl 0.01 Mg 0.006 )I crystal X-ray irradiation luminescence spectrum. DETAILED DESCRIPTION
[0030] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.
[0031] In the present invention, the scintillator single crystal has physical and performance advantages such as low preparation cost, high stability, high light yield, and high energy resolution. At the same time, due to the introduction of Mg ions, Tl ions can achieve efficient bound exciton emission at room temperature, thereby improving the exciton utilization efficiency. Specifically, the magnesium-thallium co-doped zero-dimensional perovskite halide scintillator single crystal has the following general composition formula: (Cs 1-x-y-z Tl x Mg y A z )3(Cu 1-m B m )2(I 1-n X n )5, wherein: A = one or more combinations of Na, K, Rb; B = one or more combinations of Ag, Li, Au; X = one or more combinations of Cl and Br; and 0<x<1, 0<y≤0.02, 0≤z<1, 0<x + y + z<1, 0≤m≤1, 0≤n≤1.
[0032] Preferably, x=0.01, 0.02, 0.03, 0.04, 0.05, etc.
[0033] Preferably, y=0.0001, 0.00025, 0.0005, 0.00075, 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.007, 0.008, 0.009, 0.01, 0.012, 0.013, 0.014, 0.015, etc.
[0034] Preferably, z=0, 0.001, 0.005, 0.01, 0.05, 0.1, etc.
[0035] Preferably, m=0, 0.001, 0.05, 0.1, 0.2, etc.
[0036] Preferably, n=0, 0.1, 0.2, 0.5, etc.
[0037] It should be noted that the "range" disclosed herein is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of a particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 0 to 0.1 and 0 to 1 is listed for a particular parameter, it is understood that a range of 0 to 0.08 and 0 to 0.8 is also expected. In addition, if the minimum range values 0.001 and 0.002 are listed, and if the maximum range values 0.003, 0.004 and 0.005 are listed, the following ranges can all be expected: 0.001 to 0.003, 0.001 to 0.004, 0.001 to 0.005, 0.002 to 0.003, 0.002 to 0.004 and 0.002 to 0.005. In this application, unless otherwise specified, the numerical range "a-b" represents an abbreviation of any real number combination between a and b, where a and b are real numbers. For example, the numerical range "0-1" means that all real numbers between "0-1" are listed in this document, and "0-1" is just an abbreviation of these numerical combinations.
[0038] The following is an exemplary description of a method for preparing a magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal.
[0039] Using halide powder as raw material, the target component is formulated according to the general composition formula and loaded into a sealed container. The purity of the halide powder is ≥99.9%. Specifically, in an inert environment, the mixed raw materials are placed in a crucible with a capillary bottom, and then the crucible is evacuated to a vacuum and sealed by welding. The crucible includes a quartz crucible, a platinum crucible, and a graphite crucible. Preferably, the inert environment includes a glove box.
[0040] The sealed crucible is placed in a tube furnace or other heating furnace, and the compound satisfying the general composition formula is obtained by solid phase reaction method or molten salt cooling method, which mainly refers to the melting reaction process of the raw materials. This method raises the temperature above the melting point of the compound, such as 400-600°C, which can obtain higher product uniformity and reaction efficiency, so that the raw materials can fully react to synthesize the target component polycrystal.
[0041] The target scintillation single crystal is obtained by directional solidification method. The directional solidification method includes Bridgman descent method or horizontal directional solidification method. The preferred Bridgman method is a typical method for preparing high-quality single crystals with simple operation and high efficiency. The slow cooling method with controllable temperature field movement or temperature field distribution is also a preferred method.
[0042] After the raw material powder is completely melted and mixed evenly, the target magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal is obtained by using the Bridgman descent method. As an example of the Bridgman descent method, it includes: placing the welded crucible vertically in the middle position of the crystal growth furnace; heating the crystal growth furnace until the raw materials are completely melted and mixed evenly; adjusting the crucible position and furnace temperature so that the temperature at the bottom of the crucible reaches a predetermined value, and then lowering the crucible in the furnace body, and the crystal begins to nucleate and grow from the capillary bottom of the crucible until the melt is completely crystallized; then cool down until it drops to room temperature. Finally, take out the prepared magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal from the crucible in a dry environment. While heating the crystal growth furnace to 400-600°C, the temperature at the bottom of the crucible reaches 330-400°C.
[0043] Alternatively, after the raw material powder is completely melted and mixed evenly, the target magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal is obtained by horizontal directional solidification. As an example of a horizontal directional solidification method, it includes: placing the sealed crucible horizontally in the middle position of a horizontal directional growth furnace; heating the horizontal directional growth furnace until the raw materials are completely melted and mixed evenly; adjusting the crucible position and furnace temperature so that the temperature at the bottom of the crucible reaches a predetermined value, and then moving the crucible horizontally at a uniform speed in the furnace body, and the crystal begins to nucleate and grow from the capillary bottom of the crucible until the melt is completely crystallized; then cooling down until it drops to room temperature. Finally, the prepared magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal is taken out of the crucible in a dry environment. While heating the horizontal directional growth furnace to 400-600°C, the temperature at the bottom of the crucible reaches 330-400°C.
[0044] The single crystal material prepared by the present invention can be directly coupled to photoelectric devices for high-energy ionizing radiation detection after cutting, grinding and polishing. The most typical application is gamma spectrum detection. It is also suitable for use in medical imaging, homeland security, physical research and other fields through detection of X-rays, alpha particles, beta particles, neutrons, etc. according to specific needs.
[0045] In this application, if there is no special description, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution. In this application, if there is no special description, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.
[0046] In this application, unless otherwise specified, the terms "include" and "comprising" mentioned herein may be open-ended or closed-ended. For example, the terms "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0047] In the description herein, unless otherwise specified, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0048] Performance Testing:
[0049] The light yield of magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal under gamma rays was tested to be at least 80,000 Ph. / MeV by pulse height spectroscopy and traditional single photon counting method;
[0050] The light yield of magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal under X-ray was tested by pulse height spectrum and traditional single photon counting method, and was 155000 Ph. / MeV~190000 Ph. / MeV;
[0051] The decay time of magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystals was tested to be 300-740ns using Hamamatsu R6231 PMT and Tektronix DPO 5104 digitizer;
[0052] The energy resolution of magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystals was 3.4-4.5% using pulse height spectroscopy.
[0053] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples in a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0054] Example 1
[0055] The zero-dimensional perovskite halide scintillator proposed in this embodiment 1 has a chemical formula of (Cs 0.99-y Tl 0.01 Mg y )3Cu2I5, 0<y≤0.01 (y=0.0001, 0.0005, 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.008, 0.01), z=0, m=0, n=0. The zero-dimensional perovskite halide scintillating single crystal is prepared by the Bridgman descent method, and the preparation process includes:
[0056] (1) Chemical formula of halide scintillator prepared on demand (Cs 0.99-y Tl 0.01 Mg y )3Cu2I5 Weigh each raw material;
[0057] (2) In an inert gas environment, place each raw material in a quartz crucible with a capillary bottom; then evacuate the crucible to a vacuum and seal it with welding. In this embodiment 1, the inert gas environment is a glove box filled with argon;
[0058] (3) Place the welded quartz crucible vertically in the middle of the crystal growth furnace; heat the crystal growth furnace to about 600°C until the raw materials are completely melted and mixed evenly; adjust the crucible position and furnace temperature to reduce the temperature at the bottom of the crucible to about 340°C, and then lower the quartz crucible in the furnace at a rate of 0.7 mm / h. The crystals begin to nucleate and grow from the capillary bottom of the crucible until the melt is completely solidified; then cool it down at a rate of 8°C / h until it reaches room temperature; finally, remove the prepared halide scintillator from the quartz crucible in a dry environment and cut it.
[0059] The scintillating crystal (y=0.005) prepared in Example 1 exhibited two obvious Tl bound exciton emissions at 510nm and 560nm respectively under X-ray irradiation at room temperature, achieving efficient emission of Tl bound excitons. It had a light yield of 180,000 ph. / MeV under X-ray irradiation, which was 20% higher than that of Cs3Cu2I5:Tl. The energy resolution was 3.8% under 662keV gamma ray irradiation, and it had a fast decay time of about 430 ns, which was 45% faster than that of Cs3Cu2I5:Tl. When the Mg co-doping content was 0.01, the light yield of the crystal under X-ray irradiation was reduced to 160,000 ph. / MeV.
[0060] Comparative Example 1
[0061] The chemical formula of the halide scintillating single crystal is Cs3Cu2I5:Tl, and it is prepared by the Bridgman descent method. The preparation process includes the following operations:
[0062] (1) Prepare the halide scintillator according to the chemical formula Cs3Cu2I5:Tl. Weigh the raw materials;
[0063] (2) In an inert gas environment, place the raw materials in a quartz crucible with a capillary bottom; then evacuate the crucible and seal it with a weld. In this embodiment, the inert gas environment is a glove box filled with argon;
[0064] (3) Place the welded quartz crucible vertically in the middle of the crystal growth furnace; heat the crystal growth furnace to about 600°C until the raw materials are completely melted and mixed evenly; adjust the crucible position and furnace temperature to reduce the temperature at the bottom of the crucible to about 340°C, and then lower the quartz crucible in the furnace at a rate of 0.7 mm / h. The crystals begin to nucleate and grow from the capillary bottom of the crucible until the melt is completely solidified; then cool it down at a rate of 8°C / h until it reaches room temperature; finally, remove the prepared halide scintillator from the quartz crucible in a dry environment and cut it.
[0065] The Cs3Cu2I5:Tl crystal obtained in this comparative example 1 only has Tl bound exciton emission at 510 nm under X-ray irradiation. When coupled to a photomultiplier tube for testing, the light yield of the Cs3Cu2I5:Tl crystal under gamma ray irradiation is 78000 ph. / MeV, the energy resolution is 3.8%, and the scintillation decay time is about 780 ns.
[0066] Comparative Example 2
[0067] The chemical formula of the scintillating single crystal is Cs3Cu2I5, which is prepared by the Bridgman descent method. The preparation process includes the following operations:
[0068] (1) Weigh the raw materials according to the chemical formula of the halide scintillator to be prepared;
[0069] (2) In an inert gas environment, place each raw material in a quartz crucible with a capillary bottom; then evacuate the crucible to a vacuum and seal it with welding. In this embodiment 1, the inert gas environment is a glove box filled with argon;
[0070] (3) Place the welded quartz crucible vertically in the middle of the crystal growth furnace; heat the crystal growth furnace to about 600°C until the raw materials are completely melted and mixed evenly; adjust the crucible position and furnace temperature to reduce the temperature at the bottom of the crucible to about 340°C, and then lower the quartz crucible in the furnace at a rate of 0.7 mm / h. The crystals begin to nucleate and grow from the capillary bottom of the crucible until the melt is completely solidified; then cool it down at a rate of 8°C / h until it reaches room temperature; finally, remove the prepared halide scintillator from the quartz crucible in a dry environment and cut it.
[0071] The test shows that the above-mentioned scintillating crystal only emits self-trapped excitons at around 440 nm under X-ray excitation. The light yield under gamma-ray irradiation is 38,000 ph. / MeV, the energy resolution is 4.5%, and the scintillation decay time is around 1,000 ns.
[0072] Example 2
[0073] (Cs0.99-y Tl 0.01 Mg y )3(Cu 1-m Ag m )2I5 halide scintillating single crystal (y=0, 0.0001, 0.0005, 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.008, 0.01, m=0.1 or 0.2) is prepared by the Bridgman descent method. The preparation process is shown in Example 1.
[0074] Example 3
[0075] (Cs 0.99-y Tl 0.01 Mg y )3Cu 2-2m Ag 2m I4Br halide scintillating single crystals (y=0, 0.0001, 0.0005, 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.008, 0.01, m=0.1 or 0.2, n=0.2) were prepared by the Bridgman descent method. The preparation process is shown in Example 1.
[0076] Example 4
[0077] The chemical formula is (Cs 0.99-y Tl 0.01 Mg y )3Cu2Br5 halide scintillating single crystals (y=0, 0.0001, 0.0005, 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.008, 0.01) were prepared by the Bridgman descent method. The preparation process is shown in Example 1.
[0078] Example 5
[0079] The chemical formula is (Cs 0.99-y Tl 0.01 Mg y )3(Cu 1-m Ag m )2I5 halide scintillating single crystals (y=0, 0.0001, 0.0005, 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.008, 0.01, m=0.1) are prepared by the Bridgman descent method. The preparation process includes:
[0080] (1) Chemical formula of halide scintillator prepared on demand (Cs 0.99-yT l 0.01 Mg y )3(Cu 1-mAg m )2I5 Weigh each raw material;
[0081] (2) In an inert gas environment, place each raw material in a quartz crucible with a capillary bottom; then evacuate the crucible and seal it with welding. In this embodiment, the inert gas environment is a glove box filled with argon or nitrogen;
[0082] (3) Place the welded quartz crucible vertically in the middle of the crystal growth furnace; heat the crystal growth furnace to about 550°C until the raw materials are completely melted and mixed evenly; adjust the crucible position and furnace temperature to reduce the temperature of the bottom of the crucible to about 350°C, and then lower the quartz crucible in the furnace at a rate of 0.5 mm / h. The crystal begins to nucleate and grow from the capillary bottom of the crucible until the melt is completely solidified; then cool it down at a rate of 7°C / h until it reaches room temperature; finally, take out the prepared crystal from the quartz crucible. Coupled to the photomultiplier tube test, (Cs 0.98 Tl 0.01 Mg 0.01 )3(Cu 0.9 Ag 0.1 The light yield of the )2I5 crystal is improved compared to that of the Cs3Cu2I5:Tl crystal, which is 90,000 ph. / MeV; the energy resolution is 3.2%; and the scintillation decay time is 561 ns, which is nearly 28% faster.
[0083] Example 6
[0084] The chemical formula is (Cs 0.99-y Tl 0.01 Mg y )3Cu2Br5 halide scintillating single crystals (y=0, 0.0001, 0.0005, 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.008, 0.01) were prepared by horizontal directional solidification method. The preparation process includes the following operations:
[0085] (1) Chemical formula of halide scintillator prepared on demand (Cs 0.99-y Tl 0.01 Mg y )3Cu2Br5 Weigh each raw material;
[0086] (2) In an inert gas environment, place each raw material in a quartz crucible with a capillary bottom; then evacuate the crucible and seal it with welding. In this embodiment, the inert gas environment is a glove box filled with argon or nitrogen;
[0087] (3) Place the welded quartz crucible horizontally in the middle of the horizontal directional growth furnace; heat the crystal growth furnace to about 600°C until the raw materials are completely melted and mixed evenly; adjust the crucible position and furnace temperature to reduce the crucible capillary temperature to about 360°C, and then move the quartz crucible horizontally at a uniform speed of 0.8 mm / h in the furnace body. The crystal begins to nucleate and grow from the crucible capillary until the melt is completely solidified; then cool it down at a rate of 10°C / h until it reaches room temperature; finally, take out the prepared crystal from the quartz crucible. Coupled to the photomultiplier tube test (Cs 0.98 Tl 0.01 Mg 0.01 )3Cu2Br5 crystal has a light yield of 120000 ph. / MeV.
[0088] Example 7
[0089] The chemical formula is (Cs 0.99-y Tl 0.01 Mg y )3Cu 1.8 Ag 0.2 I4Br halide scintillating single crystals (y=0, 0.0001, 0.0005, 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.008, 0.01, m=0, 0.1 or 0.2, n=1) are prepared by the Bridgman descent method. The preparation process includes the following operations:
[0090] (1) Chemical formula of halide scintillator prepared on demand (Cs 0.99-y Tl 0.01 Mg y )3Cu 1.8 Ag 0.2 I4Br Weigh each raw material;
[0091] (2) In an inert gas environment, place each raw material in a quartz crucible with a capillary bottom; then evacuate the crucible and seal it with welding. In this embodiment, the inert gas environment is a glove box filled with argon or nitrogen;
[0092] (3) Place the welded quartz crucible vertically in the middle of the crystal growth furnace; heat the crystal growth furnace to about 600°C until the raw materials are completely melted and mixed evenly; adjust the crucible position and furnace temperature to reduce the temperature of the bottom of the crucible to about 370°C, and then lower the quartz crucible in the furnace at a rate of 1.5 mm / h. The crystals begin to nucleate and grow from the capillary bottom of the crucible until the melt is completely solidified; then cool it down at a rate of 12°C / h until it reaches room temperature; finally, take out the prepared (Cs 0.99-y Tl 0.01 Mgy )3Cu 1.8 Ag 0.2 I4Br crystals.
[0093] Table 1 shows the composition and properties of the halide scintillating single crystal prepared by the present invention:
[0094] .
[0095] Comparison example:
[0096] (Na 0.904 6 Li 0.08 Tl 0.01 Mg 0.006 )I The preparation method of the halide scintillator single crystal comprises: preparing the halide scintillator composition chemical formula (Na 0.904 6 Li 0.08 Tl 0.01 Mg 0.006 )I Weigh all the raw materials and mix them thoroughly, then put them into a conical quartz crucible and seal it; place the welded quartz crucible vertically in the middle of the descending method crystal growth furnace; heat the crystal growth furnace to 800°C and keep it warm for a certain period of time until the raw materials are completely melted and mixed evenly; adjust the crucible position and furnace temperature to reduce the bottom temperature of the crucible to about the melting point of the scintillation crystal, and then lower the quartz crucible in the furnace body at a descending speed of 3mm / h, and the crystal begins to nucleate and grow from the bottom of the crucible until the melt is completely solidified and crystallized. Reduce the furnace temperature at a rate of 8°C / h, and take out the prepared single crystal when the thermocouple shows that it has dropped to room temperature.
[0097] (Na 0.91 6 Li 0.08 Tl 0.01 )I The preparation method of the halide scintillator single crystal comprises: preparing the halide scintillator composition chemical formula (Na 0.904 6 Li 0.08 Tl 0.01 Mg 0.006 )I Weigh all the raw materials and mix them thoroughly, then put them into a conical quartz crucible and seal it; place the welded quartz crucible vertically in the middle of the descending method crystal growth furnace; heat the crystal growth furnace to 800°C and keep it warm for a certain period of time until the raw materials are completely melted and mixed evenly; adjust the crucible position and furnace temperature to reduce the bottom temperature of the crucible to about the melting point of the scintillation crystal, and then lower the quartz crucible in the furnace body at a descending speed of 3mm / h, and the crystal begins to nucleate and grow from the bottom of the crucible until the melt is completely solidified and crystallized. Reduce the furnace temperature at a rate of 8°C / h, and take out the prepared single crystal when the thermocouple shows that it has dropped to room temperature.
[0098] Table 2:
[0099] .
[0100] In the early stage of the research, the inventor introduced Mg into the lithium-thallium co-doped sodium iodide scintillator crystal. At this time, Mg ions and Tl ions also coexisted. However, the role of the introduction of Mg ions was only to improve the energy resolution, and its decay time was not greatly affected. The light yield was even reduced. The inventor also explored the luminescence spectrum (see Figure 8 ), found that the introduction of Mg into Li-Tl co-doped NaI scintillating crystals did not improve the emission efficiency of Tl bound excitons at room temperature.
[0101] Finally, it is necessary to explain here that the above embodiments are only used to further illustrate the technical solution of the present invention in detail and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above content of the present invention all fall within the scope of protection of the present invention.
Claims
1. A magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal, It is characterized in that The chemical formula of the magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal is (Cs 1-x-y Tl x Mg y ) 3 (Cu 1-m B m ) 2 (I 1-n X n ) 5 ; Wherein: B = Ag; X = at least one of Cl and Br; and 0<x<1, 0<y≤0.01, 0<x + y<1, 0≤m≤1, 0≤n≤1.
2. The magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal according to claim 1, It is characterized in that x=0.001~0.05; or / and y=0.001~0.
01.
3. The magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal according to claim 2, It is characterized in that x=0.01; or / and y=0.001~0.
01.
4. The magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal according to any one of claims 1 to 3, It is characterized in that The light yield of the magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal under gamma rays is at least 80,000 Ph. / MeV; The light yield of the magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal under X-ray is 155,000 Ph. / MeV to 190,000 Ph. / MeV; The decay time of the magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal is 300-740ns; The energy resolution of the magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal is 3.4-4.5%.
5. A method for preparing the magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal according to claim 1, It is characterized in that include: (1) weighing and mixing halide powders according to a general chemical formula to obtain raw material powders; (2) The obtained raw material powder is sealed and placed in a crucible, and a magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal is obtained by using a Bridgman descent method or a horizontal directional solidification method.
6. The preparation method according to claim 5, It is characterized in that The halide powder includes: CsX, TlX, MgX 2 ,CuX 2 , BX; the purity of the halide powder is ≥99.9%; the atmosphere inside the crucible is a vacuum atmosphere.
7. The preparation method according to claim 5 or 6, It is characterized in that The parameters of the Bridgman descent method include: a melting temperature of 400-600° C. until the raw material powder is completely melted; a bottom temperature of the crucible reaches 330-400° C.; and a crucible descent rate of 0.3-1.0 mm / h.
8. The preparation method according to claim 5 or 6, It is characterized in that The parameters of the horizontal directional solidification method include a melting temperature of 400-600° C. until the raw material powder is completely melted; a bottom temperature of the crucible reaches 330-400° C.; and a horizontal movement rate of the crucible is 0.3-1.0 mm / h.
9. The preparation method according to claim 5 or 6, It is characterized in that The crucible is a crucible with a capillary bottom; the crucible includes a quartz crucible, a platinum crucible or a graphite crucible.
10. Use of the magnesium-thallium co-doped zero-dimensional perovskite halide scintillating single crystal as claimed in claim 1 in X-ray imaging and gamma-ray detection.
Citation Information
Patent Citations
Li<+>-doped zero-dimensional perovskite structure metal halide scintillation crystal, preparation method and application thereof
CN113529168A
Novel perovskite-like structure scintillator for neutron detection as well as preparation method and application of novel perovskite-like structure scintillator
CN114411252A
Rare-earth-based zero-dimensional perovskite halide scintillation single crystal and preparation method and application thereof
CN117552106A
Spraying preparation process of scintillator film
CN117654849A