A ternary positive electrode material and preparation method thereof, and a lithium battery

By doping metal element A into the ternary positive electrode material to form a protective layer and covering it with metal element B, the problem of high residual lithium in the prior art is solved, and the electrochemical performance and cyclic stability of the material are significantly improved.

CN118486834BActive Publication Date: 2024-11-08YINGDE KEHENG NEW ENERGY TECH CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202410944242.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-08
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The prior art is difficult to effectively reduce the residual lithium amount on the surface of the ternary positive electrode material, affecting the electrochemical performance of the material.

Method used

By doping metal element A in the ternary positive electrode material precursor for segmental primary sintering, an A-O bond protection layer is formed, and metal element B is coated in the secondary sintering, reducing residual lithium and improving the magnification of the material and capacity.

Benefits of technology

Effectively inhibit oxygen precipitation and transition metal dissolution, maintain the smoothness of Li+ migration channels, reduce the residual lithium amount, and improve the circulation and electrochemical properties of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the field of lithium ion batteries and discloses a ternary positive electrode material and a preparation method thereof, comprising the following steps: x Co y Mn z (OH) 2 ), a metal compound containing element A to obtain a mixture; the mixture obtained in step 1 is sintered once to obtain a primary sintered material; the primary sintered material obtained in step 2 is crushed to obtain a powder; finally, the powder obtained in step 3 is mixed with a metal compound containing element B and then sintered for a secondary time to obtain a ternary positive electrode material; by improving the doping and coating processes, the residual lithium content on the surface of the positive electrode material is reduced; in addition, the present application also discloses a ternary positive electrode material and a lithium battery prepared by the above method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium-ion batteries, and in particular to a ternary positive electrode material and a preparation method thereof, and a lithium battery. Background Art

[0002] At present, in the lithium-ion battery cathode material market, lithium battery manufacturers have higher and higher requirements for lithium battery energy density, and ternary cathode materials continue to move towards high nickel content; due to the lack of cobalt resources and high prices, ternary cathode materials are also moving towards low cobalt content to reduce material costs, and the medium-high nickel 613 single crystal ternary cathode material has high energy density, long cycle life, good safety performance, and low cobalt content, making it a very cost-effective lithium-ion battery cathode material. At present, in the 3C digital market, 613 single crystal ternary cathode materials are widely used, and battery manufacturers also have higher and higher performance requirements for them, requiring lower residual lithium and higher energy density. Lower residual lithium means that the material has better processing performance, and the material is less sensitive to the environment during preparation and use.

[0003] At present, single crystal materials or high-nickel materials on the market are all washed with water or wet coated to achieve the purpose of reducing residual lithium. Among them, Chinese patent application 202210154885.5 discloses a method for preparing a nickel-cobalt-manganese ternary positive electrode material. By introducing Zr and Mg doping into the ternary precursor and introducing Zr coating in the later stage of the reaction, a nickel-cobalt-manganese ternary positive electrode material with dual modification of zirconium-magnesium doping and zirconium coating is prepared.

[0004] This solution improves the cycle performance and storage performance of the ternary positive electrode material through wet coating of the nickel-cobalt-manganese ternary positive electrode material, using Zr metal, Mg metal doping and Zr coating.

[0005] Prior art 1: Chinese patent application 202211165088.3 discloses a low-cobalt ternary single crystal positive electrode material and a preparation method thereof. The low-cobalt ternary single crystal positive electrode material is Ni x Co y Mn 1-x-y(OH)2, 0.5≤x≤0.9, 0<y≤0.05 is a ternary precursor, and a dopant and a flux are added and mixed before sintering once. The first sintering is a staged sintering, including: first sintering the first stage, and then heating up the second stage; wherein the furnace pressure of the first stage sintering is 5-15Pa, and the furnace pressure of the second stage sintering is 25-40Pa; the first sintering material is mixed with a coating agent, and then a second sintering is performed in an air atmosphere to obtain a low-cobalt single crystal ternary positive electrode material. The dopant is at least one of Ta, La, Nb, Zr, Ti, Ge, Y, Al and Ba, and the coating agent is at least one of Al2O3 powder, TiO2 powder and WO3 powder.

[0006] This solution forms a metal coating on the surface of lithium manganese oxide through secondary sintering of low-cobalt ternary positive electrode materials, thereby reducing residual lithium on the surface of the material and improving the electrochemical performance of the material under high voltage.

[0007] Prior art 2: Chinese patent application 201910595304.X discloses a nickel cobalt manganese oxide ternary positive electrode material and a preparation method thereof. The nickel cobalt manganese oxide ternary positive electrode material is prepared by mixing a lithium source, a nickel cobalt manganese hydroxide and an M element compound, ball milling, sintering, and crushing to prepare a nickel cobalt manganese oxide ternary positive electrode material matrix; then the nickel cobalt manganese oxide ternary positive electrode material matrix, a Co source and an N element compound are mixed, ball milled, sintered, and crushed to obtain a nickel cobalt manganese oxide ternary positive electrode material; the M element is one or more of Zr, Al, Ti, Mg, Sr, Nb, Y, W, B, Mo, Ce, Bi, and In; the N element is selected from one or more of Zr, Al, Ti, B, Mo, Ce, and In.

[0008] This solution involves ball-milling and sintering the ternary positive electrode material, coating the metallic cobalt element on the surface of the ternary positive electrode material, and achieving the effect of surface doping. The coating layer is an electrochemically active substance of cobalt lithium oxide, which improves the structural stability while avoiding the capacity loss caused by conventional coating.

[0009] It is not difficult to see that the above three schemes respectively use the wet coating method to dope zirconium metal, coating zirconium metal and segmented secondary sintering, and secondary sintering to coat cobalt metal to reduce the amount of residual lithium on the surface of the ternary positive electrode material or improve the performance of the ternary positive electrode material battery.

[0010] The problem that this solution needs to solve: How to propose a new preparation method to reduce the amount of residual lithium on the surface of the ternary positive electrode material. Summary of the invention

[0011] The purpose of the present invention is to provide a ternary positive electrode material and a preparation method and application thereof. The precursor of the ternary positive electrode material is doped with metal element A and sintered in a staged manner, and then coated with metal element B in a secondary sintering process to obtain the ternary positive electrode material. Doping with metal element A can form a protective layered structure mainly composed of AO bonds in the ternary positive electrode material, which effectively inhibits oxygen precipitation and transition metal dissolution, and maintains a relatively smooth Li+ migration channel; the coating of metal element B can effectively reduce the residual lithium of the material, and the B element reacts with the free Li on the surface of the ternary positive electrode material, which can not only reduce the residual lithium, but also generate B compounds, effectively improving the electrochemical properties of the material such as rate and capacity.

[0012] To achieve the above object, the present application discloses a method for preparing a ternary positive electrode material, comprising the following steps:

[0013] Step 1: Mix the lithium salt, the ternary precursor, and the metal compound containing element A, sinter them once, and crush them to obtain a powder;

[0014] Step 2: The powder obtained in step 1 is mixed with a metal compound containing element B, and then secondary sintered, crushed, and sieved to obtain a ternary positive electrode material;

[0015] The ternary precursor is Ni x Co y Mn z (OH) 2, x+y+z=1 and x>0, y>0, z>0;

[0016] Element A is selected from one or more of Zr, B, W, Ti, and Y, and element A contains at least Zr;

[0017] The element B is selected from one or more of Co, Ti, W, and Al, and the element B contains at least Co;

[0018] The amount of the metal compound containing element A in step 1 is Ni x Co y Mn z The amount of the metal compound containing element B added in step 2 is 3000 to 5000 ppm of the mass of the powder.

[0019] Preferably, the Ni in step 1 x Co y Mn z In (OH)2, x+y+z=1 and 0.3<x<0.9, y>0, z>0.

[0020] Preferably, the Ni in step 1 x Co y Mn zIn (OH)2, x+y+z=1 and 0.5<x<0.8, y>0, z>0.

[0021] Preferably, the element A in step 1 is a combination of Zr, Y and Ti, and the molar ratio of Zr, Y and Ti is 6-8:1-3:5-7.

[0022] Preferably, the element B in step 2 is a combination of Co, Al and W, and the molar ratio of Co, Al and W is 14-16:4-6:1-3.

[0023] Preferably, the primary sintering step in step 1 is: firstly heating to 450-650°C at 3-5°C / min, and sintering at a constant temperature for 2-4h; then heating to 650-800°C at 2-4°C / min, and sintering at a constant temperature for 2-4h; finally heating to 930-980°C at 1-3°C / min, and sintering at a constant temperature for 10-14h.

[0024] Preferably, the secondary sintering step in step 2 is: heating to 550-750° C. at a rate of 3-5° C. / min, and sintering at a constant temperature for 6-10 hours.

[0025] Preferably, the powder particle size D50 in step 1 is 3.0-5.0 um.

[0026] In addition, it also includes a ternary positive electrode material obtained by a high-temperature sintering and coating ternary positive electrode material preparation method.

[0027] In addition, it also includes a lithium battery, which uses the above-mentioned ternary material as the active material of the positive electrode.

[0028] The beneficial effects of the present invention are:

[0029] The present invention provides a ternary positive electrode material and a preparation method and application thereof. The ternary positive electrode material is doped with metal element A by staged high-temperature one-time sintering. The strong bond energy of AO bond can act as a protective layer in the electrochemical cycle process, thereby effectively inhibiting oxygen precipitation and transition metal dissolution; the protective layered structure is not destroyed in the electrochemical cycle process, maintaining a relatively smooth Li + Migration channels are formed, which effectively curbs the capacity attenuation and cycle performance deterioration caused by the destruction of the layered structure; at the same time, the residual lithium of the material can be effectively reduced by coating with metal compounds containing element B. The reaction of element B with the free Li on the surface of the ternary positive electrode material can not only reduce the residual lithium, but also generate B compounds, effectively improving the electrochemical properties of the material such as rate and capacity. The synergistic combination of element A and element B can also more effectively reduce the amount of residual lithium on the surface of the ternary positive electrode material. DETAILED DESCRIPTION

[0030] In the description of the present invention, it should be noted that, if the specific conditions are not specified in the examples, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.

[0031] Example 1

[0032] Step 1: Lithium salt and Ni 0.6 Co 0.1 Mn 0.3 (OH)2 is prepared according to the molar ratio of metal elements (Li / (Ni+Co+Mn)) of 1.04:1, and mixed with ZrO2 with the mass of Ni 0.6 Co 0.1 Mn 0.3 4000ppm of (OH)2 mass, sintered once, crushed to obtain powder;

[0033] The primary sintering steps are: firstly heating to 550°C at 4°C / min and sintering at a constant temperature for 3 hours; then heating to 725°C at 3°C / min and sintering at a constant temperature for 3 hours; finally heating to 950°C at 2°C / min and sintering at a constant temperature for 12 hours.

[0034] Step 2: Mix the powder obtained in step 1 with cobalt hydroxide oxide, and the mass of cobalt hydroxide oxide is 5000ppm of the mass of the powder, then increase the temperature to 650°C at 4°C / min, sinter at a constant temperature for 8h, perform secondary sintering, crush, and sieve through a 300-mesh sieve to obtain a ternary positive electrode material.

[0035] Example 2

[0036] Step 1: Lithium salt and Ni 0.6 Co 0.1 Mn 0.3 (OH)2 is prepared according to the molar ratio of metal elements (Li / (Ni+Co+Mn)) of 1.04:1, and mixed with ZrO2 with the mass of Ni 0.6 Co 0.1 Mn 0.3 3000ppm by mass of (OH)2, sintered once, crushed to obtain powder;

[0037] The primary sintering step is to first increase the temperature to 450°C at 3°C / min and sinter at a constant temperature for 2 hours; then increase the temperature to 650°C at 2°C / min and sinter at a constant temperature for 2 hours; and finally increase the temperature to 930°C at 1°C / min and sinter at a constant temperature for 10 hours.

[0038] Step 2: Mix the powder obtained in step 1 with cobalt hydroxide oxide, and the mass of cobalt hydroxide oxide is 7000ppm of the mass of the powder, then increase the temperature to 550°C at 3°C / min, sinter at a constant temperature for 6 hours, crush, and sieve through a 400-mesh sieve to obtain a ternary positive electrode material.

[0039] Example 3

[0040] Step 1: Lithium salt and Ni 0.6 Co 0.1 Mn 0.3 (OH)2 is prepared according to the molar ratio of metal elements (Li / (Ni+Co+Mn)) of 1.04, mixed with ZrO2 and the mass of ZrO2 is Ni 0.6 Co 0.1 Mn 0.3 5000ppm by mass of (OH)2, sintered once, crushed to obtain powder;

[0041] The primary sintering steps are: firstly heating to 650°C at 5°C / min and sintering at a constant temperature for 4 hours; then heating to 800°C at 4°C / min and sintering at a constant temperature for 4 hours; finally heating to 980°C at 3°C / min and sintering at a constant temperature for 14 hours.

[0042] Step 2: Mix the powder obtained in step 1 with cobalt hydroxide oxide, and the mass of cobalt hydroxide oxide is 4000ppm of the mass of the powder, then increase the temperature to 750°C at 5°C / min, sinter at a constant temperature for 10 hours, perform secondary sintering, crush, and sieve through a 350-mesh sieve to obtain a ternary positive electrode material.

[0043] Example 4

[0044] The method is basically the same as Example 1, except that in step 1, a mixture of ZrO2, Y2O3 and TiO2 is used instead of ZrO2, and the molar ratio of Zr element, Y element and Ti element is 7:2:6, and the total mass of ZrO2, Y2O3 and TiO2 is Ni 0.6 Co 0.1 Mn 0.3 4000ppm by mass of (OH)2.

[0045] Example 5

[0046] It is basically the same as Example 1, except that in step 2, a mixture of cobalt oxyhydroxide, Al2O3 and WO3 is used instead of cobalt oxyhydroxide, and the molar ratio of Co element, Al element and W element is 15:5:2, and the total mass of cobalt oxyhydroxide, Al2O3 and WO3 is 5000ppm of the powder mass.

[0047] Example 6

[0048] The method is basically the same as Example 1, except that in step 1, a mixture of ZrO2, Y2O3 and TiO2 is used instead of ZrO2, and the molar ratio of Zr element, Y element and Ti element is 7:2:6, and the total mass of ZrO2, Y2O3 and TiO2 is Ni 0.6 Co 0.1 Mn 0.3 In step 2, a mixture of cobalt oxyhydroxide, Al2O3 and WO3 is used instead of cobalt oxyhydroxide, and the molar ratio of Co element, Al element and W element is 15:5:2, and the total mass of cobalt oxyhydroxide, Al2O3 and WO3 is 5000ppm of the powder mass.

[0049] Example 7

[0050] The method is basically the same as Example 1, except that in step 1, a mixture of ZrO2, Y2O3 and TiO2 is used instead of ZrO2, and the molar ratio of Zr element, Y element and Ti element is 6:1:5, and the total mass of ZrO2, Y2O3 and TiO2 is Ni 0.6 Co 0.1 Mn 0.3 4000ppm by mass of (OH)2.

[0051] Example 8

[0052] The method is basically the same as Example 1, except that in step 1, a mixture of ZrO2, Y2O3 and TiO2 is used instead of ZrO2, and the molar ratio of Zr element, Y element and Ti element is 8:3:7, and the total mass of ZrO2, Y2O3 and TiO2 is Ni 0.6 Co 0.1 Mn 0.3 4000ppm by mass of (OH)2.

[0053] Example 9

[0054] It is basically the same as Example 1, except that in step 2, a mixture of cobalt oxyhydroxide, Al2O3 and WO3 is used instead of cobalt oxyhydroxide, and the molar ratio of Co element, Al element and W element is 14:4:1, and the total mass of cobalt oxyhydroxide, Al2O3 and WO3 is 5000ppm of the powder mass.

[0055] Example 10

[0056] It is basically the same as Example 1, except that in step 2, a mixture of cobalt oxyhydroxide, Al2O3 and WO3 is used instead of cobalt oxyhydroxide, and the molar ratio of Co element, Al element and W element is 16:6:3, and the total mass of cobalt oxyhydroxide, Al2O3 and WO3 is 5000ppm of the powder mass.

[0057] Embodiment 11

[0058] It is basically the same as Example 1, except that the ternary precursor in step 1 is Ni 0.34 Co 0.33 Mn 0.33 (OH)2.

[0059] Example 12

[0060] It is basically the same as Example 1, except that the ternary precursor in step 1 is Ni 0.9 Co 0.05 Mn 0.05 (OH)2.

[0061] Comparative Example 1

[0062] Step 1: Lithium salt and Ni 0.6 Co 0.1 Mn 0.3 (OH)2 is prepared according to the molar ratio of metal elements (Li / (Ni+Co+Mn)) of 1.04:1, mixed, sintered once, and crushed to obtain powder;

[0063] The primary sintering steps are: firstly heating to 550°C at 4°C / min and sintering at a constant temperature for 3 hours; then heating to 725°C at 3°C / min and sintering at a constant temperature for 3 hours; finally heating to 950°C at 2°C / min and sintering at a constant temperature for 12 hours.

[0064] Step 2: The powder obtained in step 1 is heated to 650°C at a rate of 4°C / min, sintered at a constant temperature for 8 hours, crushed, and sieved through a 300-400 mesh sieve to obtain a ternary positive electrode material.

[0065] Comparative Example 2

[0066] It is basically the same as Comparative Example 1, except that in step 1, lithium salt and Ni 0.6 Co 0.1 Mn 0.3 (OH)2 is prepared according to the molar ratio of metal elements (Li / (Ni+Co+Mn)) of 1.04:1, and mixed with ZrO2 with the mass of Ni 0.6 Co 0.1 Mn 0.3 4000ppm of (OH)2 mass, sintered once, crushed to obtain powder;

[0067] The primary sintering steps are: firstly heating to 550°C at 4°C / min and sintering at a constant temperature for 3 hours; then heating to 725°C at 3°C / min and sintering at a constant temperature for 3 hours; finally heating to 950°C at 2°C / min and sintering at a constant temperature for 12 hours.

[0068] Comparative Example 3

[0069] It is basically the same as Comparative Example 1, except that in step 2, the powder is mixed with cobalt hydroxide oxide, and the mass of cobalt hydroxide oxide is 5000ppm of the mass of the powder, and then the temperature is increased to 650°C at 4°C / min, sintered at a constant temperature for 8h, crushed, and sieved through a 300-400 mesh sieve to obtain a ternary positive electrode material.

[0070] Comparative Example 4

[0071] It is basically the same as Comparative Example 2, except that the mass of ZrO2 added in step 1 is Ni 0.6 Co 0.1 Mn 0.3 2500ppm by mass of (OH)2.

[0072] Comparative Example 5

[0073] It is basically the same as Comparative Example 2, except that the mass of ZrO2 added in step 1 is Ni 0.6 Co 0.1 Mn 0.3 5500ppm by mass of (OH)2.

[0074] Comparative Example 6

[0075] The method is substantially the same as Comparative Example 3, except that the mass of the cobalt oxyhydroxide added in Step 2 is 3500 ppm of the powder mass.

[0076] Comparative Example 7

[0077] The method is substantially the same as Comparative Example 3, except that the mass of the cobalt oxyhydroxide added in Step 2 is 7500 ppm of the powder mass.

[0078] Comparative Example 8

[0079] It is basically the same as Comparative Example 1, except that the ternary precursor in step 1 is Ni 0.34 Co 0.33 Mn 0.33 (OH)2.

[0080] Comparative Example 9

[0081] It is basically the same as Comparative Example 1, except that the ternary precursor in step 1 is Ni 0.9 Co 0.05 Mn 0.05 (OH)2.

[0082] Power-off performance test

[0083] The sintered positive electrode material, polyvinylidene fluoride (PVDF), and conductive agent (C) were weighed in a mass ratio of 92:3:5. PVDF was first dissolved in N-methylpyrrolidone (NMP), and then the positive electrode material and conductive agent were added and stirred thoroughly to form a viscous slurry. The slurry was applied to the surface of the aluminum foil, and after drying, it was cut into positive electrode sheets of appropriate size. The above-mentioned positive electrode sheets, diaphragms, negative electrode lithium metal sheets, electrolytes, etc. were assembled into CR-2032 button batteries in a glove box filled with argon protection. The assembled batteries were tested for electrochemical performance at a voltage range of 3.0 to 4.4 V at temperatures of 25°C and 45°C, respectively. The results are shown in Table 1.

[0084] Table 1 Performance test results

[0085] experiment Discharge capacity (0.1C, 25℃) mAh / g Discharge capacity (1C, 25℃) mAh / g 25℃, 1C cycle capacity retention after 100 cycles (%) 45℃, 1C cycle capacity retention after 100 cycles (%) Example 1 192.3 172.8 92.7 92.9 Example 2 191.6 171.6 92.1 92.7 Example 3 191.7 171.9 92.0 92.6 Example 4 193.3 173.2 93.2 93.4 Example 5 193.1 173.6 93.0 93.5 Example 6 195.1 174.2 93.8 93.9 Example 7 193.0 172.9 92.9 93.1 Example 8 192.9 172.7 92.8 93.2 Example 9 192.6 173.1 92.9 92.9 Example 10 192.7 173.2 92.7 93.0 Embodiment 11 191.6 171.6 92.2 92.5 Example 12 191.8 171.3 92.1 92.4 Comparative Example 1 190.5 170.8 90.1 90.3 Comparative Example 2 190.8 171.0 90.8 90.9 Comparative Example 3 190.9 171.1 90.7 91.0 Comparative Example 4 190.6 170.6 90.3 90.6 Comparative Example 5 190.2 170.4 90.5 90.7 Comparative Example 6 190.5 170.9 90.7 90.8 Comparative Example 7 190.9 171.3 90.8 90.9 Comparative Example 8 191.2 170.9 90.8 92.7 Comparative Example 9 191.6 171.0 90.9 91.3

[0086] Titration test for residual lithium

[0087] Weigh 10 g of sample (accurate to 0.01 g) into a beaker and add 100 mL of distilled water.

[0088] Place the clean magnetic rotor in a beaker, seal it with a sealing film, and place it on a magnetic stirrer and stir at a rate of 500 r / min for 15 min.

[0089] After standing, the sample solution was filtered using a vacuum filtration device.

[0090] Use a pipette of corresponding specifications to accurately transfer 1mL to 10mL of the filtrate to be tested into a 100mL beaker, add 50mL of distilled water, and place it on the potentiometric titrator.

[0091] Turn on the automatic potentiometric titrator, adjust the magnetic stirring rate of the automatic potentiometric titrator to prevent bubbles from being generated in the test solution, and titrate with pH value as the ordinate and the volume of hydrochloric acid titration solution consumed as the abscissa. Record the volumes V1 and V2 of the hydrochloric acid titration solution consumed corresponding to the electrode potential jump points EP1 and EP2.

[0092] Calculate the results: The content of Li2CO3 and lithium hydroxide in the sample is calculated according to formula 1 and formula 2, and the content of free lithium in the sample is calculated according to formula 3, formula 4 and formula 5:

[0093] Formula 1: ;

[0094] Formula 2: ;

[0095] Formula 3: ;

[0096] Formula 4: ;

[0097] Formula 5: .

[0098] Where:

[0099] WX——Mass fraction of Li2CO3 in the sample, expressed as percentage;

[0100] WY——The mass fraction of lithium hydroxide in the sample, expressed as percentage;

[0101] w X ——The mass fraction of lithium in Li2CO3 in the sample, expressed as percentage;

[0102] w Y ——The mass fraction of lithium in lithium hydroxide in the sample, expressed as percentage;

[0103] w Z ——Total content of free lithium in the sample, expressed as percentage;

[0104] Va——The volume of distilled water used when stirring and leaching the sample, in milliliters mL;

[0105] Vb——The volume of distilled water used for stirring and leaching the sample after filtration, in milliliters mL;

[0106] V1——The volume of hydrochloric acid titration solution consumed when titrating to the potential jump point EP1, in milliliters mL;

[0107] V2——The volume of hydrochloric acid titration solution consumed when titrating to the potential jump point EP2, in milliliters mL;

[0108] m ——the mass of the sample weighed, in grams;

[0109] C —— molar concentration of hydrochloric acid titration solution, in moles per liter mol / L;

[0110] 73.88 – the molar mass of Li2CO3 in grams per mole (g / mol);

[0111] 23.94 – The molar mass of lithium hydroxide in grams per mole (g / mol).

[0112] 0.188——The mass ratio of lithium in Li2CO3;

[0113] 0.290 – The mass ratio of lithium in lithium hydroxide.

[0114] Finally, the residual lithium results of the samples were calculated as shown in Table 2:

[0115] Table 2 Residual lithium content

[0116] experiment Residual lithium content (ppm) experiment Residual lithium content (ppm) Example 1 2106.4 Comparative Example 1 2461.3 Example 2 2236.1 Comparative Example 2 2345.3 Example 3 2236.8 Comparative Example 3 2350.1 Example 4 2026.1 Comparative Example 4 2296.2 Example 5 1986.3 Comparative Example 5 2304.6 Example 6 1789.6 Comparative Example 6 2286.7 Example 7 2106.3 Comparative Example 7 2136.3 Example 8 2162.3 Comparative Example 8 2466.1 Example 9 2036.1 Comparative Example 9 2487.3 Example 10 2087.3 Embodiment 11 2306.1 Example 12 2246.3

[0117] Result analysis:

[0118] 1. It can be seen from Examples 1-3 and Comparative Example 1 that the addition amount of the metal compound of element A and the addition amount of the metal compound of element B have a certain influence on the performance of the ternary positive electrode material such as rate and capacity, as shown in Table 3:

[0119] Table 3

[0120] experiment Discharge capacity (0.1C, 25℃) mAh / g Discharge capacity (1C, 25℃) mAh / g 25℃, 1C cycle capacity retention after 100 cycles (%) 45℃, 1C cycle capacity retention after 100 cycles (%) Residual lithium content (ppm) Example 1 192.3 172.8 92.7 92.9 2106.4 Example 2 191.6 171.6 92.1 92.7 2236.1 Example 3 191.7 171.9 92.0 92.6 2236.8 Comparative Example 1 190.5 170.8 90.1 90.3 2461.3

[0121] It can be seen from Example 1 and Comparative Example 1 that when the added amount of the metal compound of element A is 4000ppm of the mass of the ternary precursor and the added amount of the metal compound of element B is 5000ppm of the mass of the powder, the 0.1C discharge capacity and 1C discharge capacity of the ternary positive electrode material are increased by 0.8mAh / g and 1mAh / g respectively, and the cycle performance at 25°C and 45°C is also increased by 1.2% and 1.6% respectively, while the residual lithium content is reduced even more to 354.9ppm.

[0122] 2. It can be seen from Example 1 and Examples 4-6 that in Example 1, element A is Zr element and element B is Co element;

[0123] In Example 4, element A is Zr element, Y element and Ti element, and element B is Co element;

[0124] In Example 5, element A is Zr element, and element B is Co element, Al element and W element;

[0125] In Example 6, element A is Zr element, Y element and Ti element, and element B is Co element, Al element and W element. The experimental data are shown in Table 4:

[0126] Table 4

[0127] experiment Discharge capacity (0.1C, 25℃) mAh / g Discharge capacity (1C, 25℃) mAh / g 25℃, 1C cycle capacity retention after 100 cycles (%) 45℃, 1C cycle capacity retention after 100 cycles (%) Residual lithium content (ppm) Example 1 192.3 172.8 92.7 92.9 2106.4 Example 4 193.3 173.2 93.2 93.4 2026.1 Example 5 193.1 173.6 93.0 93.5 1986.3 Example 6 194.3 174.2 93.8 93.9 1789.6

[0128] It can be seen from Example 6 that when element A is a combination of Zr, Y and Ti, and element B is a combination of Co, Al and W, compared with Example 1 in which element A is Zr and element B is Co, the 0.1C discharge capacity and 1C discharge capacity of the prepared ternary positive electrode material are respectively increased by 2 mAh / g and 1.4 mAh / g, and the cycle performance at 25°C and 45°C are also increased by 1.5% and 1%, respectively, while the residual lithium content is reduced by 316.8 ppm.

[0129] 3. It can be seen from Example 4 and Examples 7-8 that the element A in Example 4 is a combination of Zr element, Y element and Ti element, and the molar ratio of Zr element, Y element and Ti element is 7:2:6;

[0130] In Example 7, element A is a combination of Zr element, Y element and Ti element, and the molar ratio of Zr element, Y element and Ti element is 6:1:5;

[0131] In Example 8, element A is a combination of Zr element, Y element and Ti element, and the molar ratio of Zr element, Y element and Ti element is 8:3:7. The experimental data is shown in Table 5:

[0132] Table 5

[0133] experiment Discharge capacity (0.1C, 25℃) mAh / g Discharge capacity (1C, 25℃) mAh / g 25℃, 1C cycle capacity retention after 100 cycles (%) 45℃, 1C cycle capacity retention after 100 cycles (%) Residual lithium content (ppm) Example 4 193.3 173.2 93.7 93.4 2026.1 Example 7 193.0 172.9 92.9 93.1 2106.3 Example 8 192.9 172.7 92.8 93.2 2162.3

[0134] It can be seen from Example 4 that when element A is a combination of Zr, Y and Ti and the molar ratio of Zr, Y and Ti is 7:2:6, the obtained ternary positive electrode material has better performance such as rate and capacity.

[0135] 4. It can be seen from Example 5 and Examples 9-10 that the element B in Example 5 is a combination of Co element, Al element and W element, and the molar ratio of Co element, Al element and W element is 15:5:2;

[0136] In Example 9, element B is a combination of Co element, Al element and W element, and the molar ratio of Co element, Al element and W element is 14:4:1;

[0137] In Example 10, element B is a combination of Co element, Al element and W element, and the molar ratio of Co element, Al element and W element is 16:6:3. The experimental data is shown in Table 6:

[0138] Table 6

[0139] experiment Discharge capacity (0.1C, 25℃) mAh / g Discharge capacity (1C, 25℃) mAh / g 25℃, 1C cycle capacity retention after 100 cycles (%) 45℃, 1C cycle capacity retention after 100 cycles (%) Residual lithium content (ppm) Example 5 193.1 173.6 93.0 93.5 1986.3 Example 9 192.6 173.1 92.9 92.9 2036.1 Example 10 192.7 173.2 92.7 93.0 2087.3

[0140] It can be seen from Example 5 that when element B is a combination of Co, Al and W and the molar ratio of Co, Al and W is 15:5:2, the obtained ternary positive electrode material has better performance such as rate and capacity.

[0141] 5. It can be seen from Example 1, Examples 11-12 and the corresponding Comparative Examples 1 and Comparative Examples 8-9 that the present invention respectively 0.3 Department, Ni 0.6 Department, Ni 0.9 Three experiments were conducted, and the results are shown in Table 7:

[0142] Table 7

[0143] experiment Discharge capacity (0.1C, 25℃) mAh / g Discharge capacity (1C, 25℃) mAh / g 25℃, 1C cycle capacity retention after 100 cycles (%) 45℃, 1C cycle capacity retention after 100 cycles (%) Residual lithium content (ppm) Example 1 192.3 172.8 92.7 92.9 2106.4 Comparative Example 1 190.5 170.8 90.1 90.3 2461.3 Embodiment 11 191.6 171.6 92.2 92.5 2306.1 Comparative Example 8 191.2 170.9 90.8 92.7 2466.1 Example 12 191.8 171.3 92.1 92.4 2246.3 Comparative Example 9 191.6 171.0 90.9 91.3 2487.3

[0144] Among them, the ternary precursor in Example 1 and Comparative Example 1 is Ni 0.6 It is a ternary precursor;

[0145] In Example 11 and Comparative Example 8, the ternary precursor is Ni 0.3 It is a ternary precursor;

[0146] In Example 12 and Comparative Example 9, the ternary precursor is Ni 0.9 It is a ternary precursor;

[0147] Combined with the above table, it can be seen that when the ternary precursor is Ni 0.6 When it is a ternary precursor, the effect of improving the prepared ternary cathode material is better than Ni 0.3 Department, Ni 0.9 The ternary positive electrode material prepared is good.

[0148] 6. It can be seen from Example 1 and Comparative Examples 1-3 that in Example 1, both the metal compound containing element A and the metal compound containing element B are added;

[0149] In Comparative Example 1, no metal compound containing element A and element B is added;

[0150] In Comparative Example 2, only the metal compound containing element A is added;

[0151] In Comparative Example 3, only the metal compound containing element B was added, and the data of the obtained ternary positive electrode material are shown in Table 8.

[0152] Table 8

[0153] experiment Discharge capacity (0.1C, 25℃) mAh / g Discharge capacity (1C, 25℃) mAh / g 25℃, 1C cycle capacity retention after 100 cycles (%) 45℃, 1C cycle capacity retention after 100 cycles (%) Residual lithium content (ppm) Example 1 192.3 172.8 92.7 92.9 2106.4 Comparative Example 1 191.5 171.8 91.1 91.3 2461.3 Comparative Example 2 191.8 172.0 91.8 91.9 2345.3 Comparative Example 3 191.9 172.1 91.7 92.0 2350.1

[0154] It can be seen from the data that adding metal compounds containing element A or metal compounds containing element B can improve the performance of the ternary positive electrode material such as rate and capacity, but the improvement effect is better when the metal compounds containing element A and the metal compounds containing element B are used in combination.

[0155] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement methods and shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a ternary positive electrode material, It is characterized in that The following steps are included: Step 1: Mix the lithium salt, the ternary precursor, and the metal compound containing element A, sinter them once, and crush them to obtain a powder; Step 2: The powder obtained in step 1 is mixed with a metal compound containing element B, and then secondary sintered, crushed, and sieved to obtain a ternary positive electrode material; The ternary precursor is Ni 0.6 Co 0.1 Mn 0.3 (OH) 2 ; Element A is a combination of Zr, Y, and Ti, and the molar ratio of Zr, Y, and Ti is 7:2:6; Element B is a combination of Co, Al, and W, and the molar ratio of Co, Al, and W is 15:5:2; The amount of the metal compound containing element A in step 1 is Ni 0.6 Co 0.1 Mn 0.3 (OH) 2 The amount of the metal compound containing element B added in step 2 is 5000ppm of the powder mass; The first sintering step in step 1 is to first heat the temperature to 550° C. and sinter at a constant temperature for 3 hours; then heat the temperature to 725° C. and sinter at a constant temperature for 3 hours; and finally heat the temperature to 950° C. and sinter at a constant temperature for 12 hours; In step 2, the secondary sintering temperature is 650° C., and the constant temperature sintering is performed for 8 hours.

2. The method for preparing the ternary cathode material according to claim 1, It is characterized in that The first sintering step in step 1 is: firstly, heating to 550°C at 4°C / min and sintering at a constant temperature for 3 hours; then heating to 725°C at 3°C / min and sintering at a constant temperature for 3 hours; finally, heating to 950°C at 2°C / min and sintering at a constant temperature for 12 hours.

3. The method for preparing the ternary cathode material according to claim 1, It is characterized in that The secondary sintering step in step 2 is: heating to 650° C. at 4° C. / min and sintering at a constant temperature for 8 hours.

4. The method for preparing the ternary cathode material according to claim 1, It is characterized in that The powder particle size D50 obtained in step 1 is 3.0-5.0 um.

5. A ternary cathode material, It is characterized in that The method is prepared by the preparation method of the ternary positive electrode material described in any one of claims 1 to 4.

6. A lithium battery, It is characterized in that Contains the ternary positive electrode material as claimed in claim 5.

Citation Information

Patent Citations

  • Nickel-cobalt-lithium manganate ternary cathode material and preparation method thereof

    CN110474026A

  • Nickel-cobalt-manganese ternary precursor, positive electrode material and preparation method

    CN114229922A

  • Low-cobalt ternary single-crystal positive electrode material, preparation method thereof and lithium ion battery

    CN115477333A

  • Preparation method of large single crystal lithium ion battery nickel cobalt lithium manganate cathode material

    CN110534733A

  • High-nickel low-cobalt type high-voltage-resistant ternary positive electrode material and preparation method thereof

    CN111384392A