A GAG composite film and its preparation process

By using a PETG and APET composite film structure in the GAG ​​sheet, combined with alkyl imidazole tetrafluoroborate and 2,3-cyclic glyceryl carbonate alkylenoate, the problem of APET hard sheets being easy to burn and becoming brittle due to aging is solved. problem, improves the transparency and mechanical properties of GAG films, and is suitable for applications in many fields.

CN118493986BActive Publication Date: 2024-10-11HENAN DAXINYUAN NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410961562.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-11
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

The APET hard sheet of GAG sheet is easy to burn and shrinks due to heat, causing uneven stress, affecting the mechanical strength, and is prone to aging and becoming brittle, affecting performance and lifespan. It also has poor water resistance, especially in high temperature and high humidity environments where the material becomes brittle. Impact resistance is reduced.

Method used

It adopts a composite film structure composed of an upper layer of PETG, a middle layer of APET and a lower layer of PETG. The middle layer of APET is composed of APET resin mixed with alkyl imidazole tetrafluoroborate and 2,3-cyclic glyceryl carbonate alkyl alkenoate. The extrusion process prepares GAG composite films to increase the crystallization rate and flame retardancy, and improves material uniformity and transparency by precisely controlling process conditions.

Benefits of technology

It improves the transparency, mechanical properties and flame retardancy of GAG film, extends its service life, reduces production costs, and maintains impact resistance in high temperature and high humidity environments. It is suitable for packaging, building materials, automotive interiors and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to a GAG composite film and a preparation process thereof. The GAG ​​composite film is composited by an upper PETG layer, an intermediate APET layer and a lower PETG layer; wherein the upper and lower PETG layers are formed by mixing and pressing PETG resin and glass fiber according to a suitable ratio, and the intermediate APET layer is formed by mixing and pressing APET resin with alkyl imidazole tetrafluoroborate and 2,3-cyclocarbonated glycerol alkyl olefinate. The alkyl imidazole borate contained in the intermediate APET layer can, on the one hand, increase the crystallization rate of APET and enhance its impact resistance, and on the other hand, can also synergize with the 2,3-cyclocarbonated glycerol alkyl olefinate contained in APET to promote the formation of a relatively stable force inside the APET layer and reduce the degree of thermal deformation of APET. The GAG ​​composite film finally obtained has high appearance transparency, no turbidity, no crystal point, no flow pattern, and has high heat sealing strength and impact resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of heat-sealed composite film materials, and in particular to a GAG composite film and a preparation process thereof. Background Art

[0002] APET is one of the important packaging materials, but due to its poor water resistance, especially under high temperature and high humidity conditions, such as during sea transportation, the material will hydrolyze, causing the material to become brittle and reduce its impact resistance, resulting in material cracking and other problems. In order to improve the impact resistance of APET sheets, polyolefin elastomers such as POE, SBS, EPDM, etc. are usually selected as tougheners, but such tougheners will affect the transparency of APET, and compatibilizers are usually required. Polyethylene terephthalate-1,4-cyclohexanedimethanol ester PETG is a PET copolymer modified product, which is a product of terephthalic acid, ethylene glycol and 1,4-cyclohexanedimethanol three monomers condensed by ester exchange method. It has excellent impact resistance and heat sealing properties, but the price of the material is relatively high, so its application is limited. Compounding APET resin with PETG resin through a multi-layer co-extrusion process is an economical and effective way to improve the toughness of APET and maintain the transparency of the material, which is one of the research hotspots in the blister packaging industry.

[0003] The composite sheet prepared by multi-layer co-extrusion process with APET as the middle layer and PETG as the upper and lower layers is called GAG composite material. GAG sheet is a composite sheet with many advantages, such as good transparency, excellent processability, good thermoforming, excellent food hygiene, and environmental protection. In the early days, GAG was mainly used in ID cards and credit cards in my country. Later, with the rise of environmental awareness, PVC was banned in home decoration materials in Europe and the United States, and GAG decorative panels were widely used. At present, domestic high-end brand cabinet manufacturers are also promoting the use of GAG to replace traditional materials such as PVC and melamine. It is mainly used in solid wall panels, door panels and cores, cabinets and wardrobe door panels, coffee tables and other panels. Downstream users print ink on its surface and then solidify it to obtain a wood-grain-like visual effect. The market growth potential of "replacing wood with plastic" is huge.

[0004] However, the APET hard sheet in the core layer of the GAG ​​sheet is easy to burn. Although its combustion does not produce harmful gases, the thermal shrinkage will cause uneven stress inside the sheet, thus affecting the overall mechanical strength of the GAG ​​sheet. In addition, the GAG ​​sheet is also prone to aging and becoming brittle, affecting the final performance and life of the product. Summary of the invention

[0005] In order to solve the problems existing in the prior art and obtain a GAG sheet with higher transparency and better mechanical properties so that it can be more widely used in the fields of packaging, building materials and automobile interior, the present invention provides a GAG composite film and a preparation process thereof.

[0006] A GAG composite film is characterized in that it is composited by an upper PETG layer, an intermediate APET layer and a lower PETG layer; wherein the upper and lower PETG layers are made of PETG resin and glass fiber in a weight ratio of 35-40:2-3; the intermediate APET layer is made by mixing APET resin with alkyl imidazole tetrafluoroborate and 2,3-cyclocarbonate glycerol alkyl olefinate in a weight ratio of 85-92:5-8:1.2-1.5; the GAG ​​composite film has a thickness of 20-80 μm, the ratio of the sum of the thickness of the upper and lower PETG layers to the thickness of the intermediate APET layer is 60-85:15-40, and the thickness of the upper and lower PETG layers is the same or different.

[0007] In some embodiments of the present invention, the structure of the alkyl imidazole tetrafluoroborate is as shown in Formula I: ; In formula I, R1 is a C1-2 alkyl group, and R2 is a C2-8 alkyl group.

[0008] In some embodiments of the present invention, the method for preparing 2,3-cyclocarbonate glycerol alkyl olefinate comprises the following steps:

[0009] S1: adding distilled alkenyl acid glycidyl ester and polar solvent into a high-pressure reactor, and adding quaternary ammonium salt catalyst and metal halide co-catalyst, sealing the reactor, introducing carbon dioxide through a valve and exhausting the air in the reactor, and closing the valve when the pressure in the reactor reaches 1.2-1.5MPa;

[0010] S2: raising the temperature of the reaction kettle to 100-120°C, reacting at a constant temperature and high pressure for 4-5 hours, stopping the reaction and releasing the pressure to discharge the material when the pressure in the kettle no longer changes, washing with water to extract and separate to remove the catalyst, and removing the solvent by rotary evaporation, and finally performing column chromatography separation to obtain the 2,3-cyclocarbonate glyceryl alkyl olefinate.

[0011] Furthermore, the alkenyl acid glycidyl ester in S1 is at least one of glycidyl acetate, glycidyl propionate, glycidyl butyrate, and glycidyl methacrylate.

[0012] Furthermore, the quaternary ammonium salt catalyst in S1 is at least one of tetrapropylammonium bromide, tetrabutylammonium bromide, tetraethylammonium chloride, and tetrabutylammonium chloride; the metal halide is at least one of zinc chloride, zinc iodide, aluminum chloride, and aluminum iodide; and the total added mass of the quaternary ammonium salt catalyst and the metal halide accounts for 1-2% of the mass of the alkenyl acid glycidyl ester.

[0013] The present invention also provides a process for preparing the above-mentioned GAG film, comprising the following steps:

[0014] SS1: Preparation of upper and lower PETG layers: terephthalic acid and ethylene glycol are added into a pulping tank at a molar ratio of 1:1.1-1.2, and a catalyst of 200-300ppm is added. After the first stage esterification reaction in the first esterification kettle, the mixture is sent into the second esterification kettle together with dicarboxylic acid or diol for the second stage esterification reaction, and then pre-polycondensation and polycondensation reactions are carried out in a polycondensation kettle. After the polycondensation reaction is completed, the product and glass fiber are sent into a screw extruder according to a weight ratio, and after plasticization, melting, extrusion, vacuumization and filtration are performed;

[0015] SS2: Preparation of middle layer APET: terephthalic acid and ethylene glycol are added into a pulping tank at a molar ratio of 1:1.1-1.2, and a catalyst of 200-300 ppm is added. The first stage esterification reaction and the second stage esterification reaction are carried out in the first esterification kettle and the second esterification kettle respectively, and then pre-polycondensation and polycondensation are carried out in different polycondensation reaction kettles. Then, the obtained substance and the alkyl imidazole tetrafluoroborate and 2,3-cyclocarbonate glycerol alkyl acrylate are fed into a screw extruder according to a weight ratio, and after plasticization, melting and extrusion, vacuum treatment and filtration are carried out;

[0016] SS3: The PETG melt obtained in SS1 and the APET melt obtained in SS2 are extruded in three layers in a distributor in a casting die through three different pipes. The extrusion temperature is 260-280°C. The extruded melt is tightly attached to a quenching roller. The temperature of the quenching roller is 20-30°C and the rotation speed is 80-100m / min to obtain a cast sheet.

[0017] SS4: The cast sheet obtained in SS3 passes through guide rollers and enters the longitudinal and transverse stretching areas to obtain the GAG ​​film.

[0018] Furthermore, the dicarboxylic acid or diol in SS1 contains a cycloalkane structure, and the added amount thereof accounts for 20-30% of the total mass of terephthalic acid and ethylene glycol.

[0019] Furthermore, in SS1 and SS2, the temperature of the first-stage esterification reaction is 250-255°C, and the pressure is 0.2-0.3MPa; the temperature of the second-stage esterification reaction is 260-265°C, and the pressure is 0.2-0.3Mpa, and the esterification rate is 96-98%; the temperature of the pre-polycondensation reaction is 265-270°C, and the reaction pressure is 20-25kPa; the temperature of the polycondensation reaction is 270-275°C, and the reaction pressure is 3.0-3.5kPa, and the intrinsic viscosity of the obtained substance is 0.17-0.20dl / g.

[0020] Furthermore, in SS1 and SS2, the moisture content of the product obtained after filtration is ≤50ppm; the basic mass ratio of the upper layer PETG, the middle layer APET and the lower layer PETG is 1:0.25-1:2.5.

[0021] Furthermore, the upper and lower GAG layers may also contain additives such as an anti-blocking agent and a lubricant, wherein the anti-blocking agent is one of alumina, mica powder, kaolin or silica; and the lubricant is one of stearamide, oleamide or erucamide.

[0022] Furthermore, in SS4, the heat treatment zone length of the longitudinal stretching is 8-10m, the temperature of the preheating zone is 70-95°C, and the time is 8-15s; the transverse stretching is divided into five zones, namely, a preheating zone, a stretching zone, a buffer zone, a heat setting zone, and a cooling zone. The preheating temperature is 90-110°C, the stretching temperature is 90-115°C, the heat setting temperature is 125-145°C, the cooling temperature is 45-65°C, and the stretching multiple is 2.0-3.8 times.

[0023] Beneficial effects:

[0024] 1. The present invention increases the crystallization rate of APET and enhances its impact resistance by adding alkyl imidazole tetrafluoroborate and 2,3-cyclocarbonate glycerol alkyl olefinate to the middle layer APET. At the same time, the force formed by the two inside APET and the cyclic stability of nitrogen-containing heterocycles and cyclocarbonic acid can be used to reduce the degree of deformation of APET under heat and stress; the flame retardancy of the obtained GAG film is also greatly improved;

[0025] 2. By precisely controlling the operating conditions of each area in the preparation process, the uniformity of the material is effectively guaranteed, thereby improving the transparency and mechanical properties of the GAG ​​film; moreover, the GAG ​​film has higher transparency than the GAG ​​sheet, does not turn white or crack when bent, and has a wide range of application potential;

[0026] 3. The preparation method of the GAG ​​composite film provided by the present invention is simple to operate and easy to control the thickness, which can effectively reduce the production and product costs. DETAILED DESCRIPTION

[0027] The present invention is further described in detail below in conjunction with the embodiments. It should be noted that the following embodiments and comparative examples are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various improvements within the concept of the present invention may be carried out without departing from the gist or scope of the present invention.

[0028] The following is an exemplary description of the preparation process of the 2,3-cyclocarbonate glycerol alkyl olefin ester used in the examples:

[0029] 2,3-Cyclocarbonate Glyceryl Acrylate:

[0030] S1: 100 g of distilled glycidyl acrylate and 200 ml of xylene were added into a high-pressure reactor, and 1 g of tetrapropylammonium bromide and zinc chloride co-catalyst were added, the reactor was sealed, carbon dioxide was introduced through a valve and the air in the reactor was evacuated, and the valve was closed when the pressure in the reactor reached 1.2 MPa;

[0031] S2: Raise the temperature of the reactor to 100°C, react at a constant temperature and high pressure for 4 hours, stop the reaction and release the pressure to discharge the material when the pressure in the reactor no longer changes, remove the catalyst by water washing, extract and separate, remove the solvent by rotary evaporation, and finally separate by column chromatography to obtain the 2,3-cyclocarbonate glyceryl acrylate.

[0032] 2,3-Cyclocarbonate Glyceryl Methacrylate:

[0033] S1: 100 g of distilled glycidyl methacrylate and 200 ml of xylene were added into a high-pressure reactor, and 1.5 g of tetrabutylammonium bromide and zinc iodide co-catalyst were added, the reactor was sealed, carbon dioxide was introduced through a valve and the air in the reactor was evacuated, and the valve was closed when the pressure in the reactor reached 1.3 MPa;

[0034] S2: Raise the temperature of the reactor to 110°C, react at a constant temperature and high pressure for 4 hours, stop the reaction and release the pressure to discharge the material when the pressure in the reactor no longer changes, wash and extract to remove the catalyst, and remove the solvent by rotary evaporation, and finally separate by column chromatography to obtain the 2,3-cyclocarbonate glyceryl methacrylate.

[0035] 2,3-Cyclocarbonate Glyceryl Ethyl Acrylate:

[0036] S1: Add 100g of distilled 2-ethyl-glycidyl acrylate (CAS: 40525-02-8) and 200ml of xylene into a high-pressure reactor, and add 2g of tetrabutylammonium bromide and zinc iodide as co-catalysts, seal the reactor, introduce carbon dioxide through the valve and exhaust the air in the reactor, and close the valve when the pressure in the reactor reaches 1.5MPa;

[0037] S2: Raise the temperature of the reactor to 120°C, and react for 5 hours at a constant temperature and high pressure. When the pressure in the reactor no longer changes, stop the reaction and release the pressure to discharge the material. Wash with water, extract and separate to remove the catalyst, and remove the solvent by rotary evaporation. Finally, separate by column chromatography to obtain the 2,3-cyclocarbonate glyceryl ethyl acrylate.

[0038] 2,3-Cyclocarbonate Glyceryl Propyl Acrylate:

[0039] The preparation process is the same as that of 2,3-cyclocarbonate glyceryl ethyl acrylate, except that 2-ethyl-glycidyl acrylate is replaced by 2-propyl-glycidyl acrylate.

[0040] Example 1

[0041] SS1: Preparation of upper and lower PETG layers: 166 g (1 mol) of terephthalic acid and 68.2 g (1.1 mol) of ethylene glycol were added to a pulping tank, and 200 ppm of dioctyltin distearate was added. After the first stage esterification reaction (250°C, 0.2 MPa, 1.0 h) in the first esterification kettle, it was put into the second esterification kettle together with 46.84 g of 1,4-cyclohexanedimethanol for the second stage esterification reaction (260°C, 0.25 MPa, 0.5 h), and then pre-polycondensation (265°C, 20 kPa, 0.5 h) and polycondensation reaction (270°C, 3.0 kPa, 0.5 h) were carried out in the polycondensation kettle. After the polycondensation reaction was completed, the product PETG resin (intrinsic viscosity 0.17 dl / g) and glass fiber were sent to the screw extruder at a weight ratio of 35:2. After plasticization, melting and extrusion, vacuumization and filtration were performed;

[0042] SS2: Preparation of middle layer APET: 166 g (1 mol) of terephthalic acid and 74.4 g (1.2 mol) of ethylene glycol were added to a pulping tank, 200 ppm of dioctyltin distearate was added, and the first stage esterification reaction (250°C, 0.2 MPa, 1.0 h) and the second stage esterification reaction (260°C, 0.25 MPa, 0.5 h) were carried out in the first esterification kettle and the second esterification kettle respectively, and then pre-polycondensation (265°C, 20 kPa, 0.5 h) and polycondensation (270°C, 3.0 kPa, 0.5 h) were carried out in different polycondensation reactors, and then the obtained material APET resin and the 1-ethyl-3-methylimidazole tetrafluoroborate and 2,3-cyclocarbonate glycerol acrylate were fed into a screw extruder in a weight ratio of 85:5:1.2, and after plasticization, melting and extrusion, vacuum treatment and filtration were carried out;

[0043] SS3: The PETG melt obtained from SS1 and the APET melt obtained from SS2 are passed through three different pipes to achieve three-layer composite extrusion in the distributor in the casting die head. The extrusion mass ratio of the upper layer PETG, the middle layer APET and the lower layer PETG is 1:0.25:2.5. The extrusion temperature is 260°C. The extruded melt is tightly attached to the quenching roller. The temperature of the quenching roller is 20°C and the rotation speed is 80m / min to obtain a cast sheet.

[0044] The cast sheet obtained by SS4:SS3 enters the longitudinal and transverse stretching areas through guide rollers, and is first stretched longitudinally and then stretched transversely; the longitudinal stretching conditions are: preheating temperature of 70±5°C, stretching ratio of 1.0, and cooling and setting temperature of 45±5°C; the transverse stretching conditions are: preheating temperature of 95±5°C, stretching ratio of 2, stretching temperature of 95±5°C, setting temperature of 130±5°C, and cooling temperature of 50±5°C, and a new GAG heat-sealed composite film can be obtained with a film thickness of 20μm, and the thickness ratio of the upper PETG layer, the middle layer APET and the lower layer PETG is 30:20:30.

[0045] Example 2

[0046] SS1: Preparation of upper and lower PETG layers: 166 g (1 mol) of terephthalic acid and 68.2 g (1.1 mol) of ethylene glycol were added to a pulping tank, and 200 ppm of dioctyltin distearate was added. After the first stage esterification reaction (255°C, 0.25 MPa, 1.5 h) in the first esterification kettle, the mixture was put into the second esterification kettle together with 58.55 g of 1,4-cyclohexanedimethanol for the second stage esterification reaction (265°C, 0.2 MPa, 0.5 h), and then pre-polycondensation (270°C, 25 kPa, 0.5 h) and polycondensation reaction (275°C, 3.5 kPa, 0.5 h) were carried out in the polycondensation kettle. After the polycondensation reaction was completed, the product PETG resin (intrinsic viscosity 0.18 dl / g) and glass fiber were fed into a screw extruder at a weight ratio of 38:2. After plasticization, melting and extrusion, the mixture was vacuumed and filtered.

[0047] SS2: Preparation of middle layer APET: 166 g (1 mol) of terephthalic acid and 74.4 g (1.2 mol) of ethylene glycol were added to a pulping tank, 300 ppm of dioctyltin distearate was added, and the first stage esterification reaction (250°C, 0.2 MPa, 1.0 h) and the second stage esterification reaction (260°C, 0.25 MPa, 0.5 h) were carried out in the first esterification kettle and the second esterification kettle respectively, and then pre-polycondensation (265°C, 20 kPa, 0.5 h) and polycondensation (270°C, 3.0 kPa, 0.5 h) were carried out in different polycondensation reactors, and then the obtained material APET resin and the 1-butyl-3-methylimidazole tetrafluoroborate and 2,3-cyclocarbonate glyceryl methacrylate were fed into a screw extruder in a weight ratio of 88:6:1.3, and after plasticization, melting and extrusion, vacuum treatment and filtration were carried out;

[0048] SS3: The PETG melt obtained from SS1 and the APET melt obtained from SS2 are passed through three different pipes to achieve three-layer composite extrusion in the distributor in the casting die head. The extrusion mass ratio of the upper layer PETG, the middle layer APET and the lower layer PETG is 1:0.5:2.5. The extrusion temperature is 270°C. The extruded melt is tightly attached to the quenching roller. The temperature of the quenching roller is 25°C and the rotation speed is 90m / min to obtain a cast sheet.

[0049] The cast sheet obtained by SS4:SS3 enters the longitudinal and transverse stretching areas through guide rollers, and is first stretched longitudinally and then stretched transversely; the longitudinal stretching conditions are: preheating temperature of 76±5°C, stretching ratio of 1.5, and cooling and setting temperature of 45±5°C; the transverse stretching conditions are: preheating temperature of 110±5°C, stretching ratio of 2.5, stretching temperature of 105±5°C, setting temperature of 140±5°C, and cooling temperature of 60±5°C, and a new GAG heat-sealed composite film can be obtained with a film thickness of 50μm, and the thickness ratio of the upper PETG layer, the middle layer APET and the lower layer PETG is 35:25:45.

[0050] Example 3

[0051] SS1: Preparation of upper and lower PETG layers: 166 g (1 mol) of terephthalic acid and 68.2 g (1.1 mol) of ethylene glycol were added to a pulping tank, and 200 ppm of dioctyltin distearate was added. After the first stage esterification reaction (255°C, 0.25 MPa, 1.5 h) in the first esterification kettle, the mixture was put into the second esterification kettle together with 58.55 g of 1,4-cyclohexanedimethanol for the second stage esterification reaction (265°C, 0.2 MPa, 0.5 h), and then pre-polycondensation (270°C, 25 kPa, 0.5 h) and polycondensation reaction (275°C, 3.5 kPa, 0.5 h) were carried out in the polycondensation kettle. After the polycondensation reaction was completed, the product PETG resin (intrinsic viscosity 0.18 dl / g) and glass fiber were sent to the screw extruder at a weight ratio of 40:3. After plasticization, melting and extrusion, the mixture was vacuumed and filtered.

[0052] SS2: Preparation of middle layer APET: 166 g (1 mol) of terephthalic acid and 74.4 g (1.2 mol) of ethylene glycol were added to a pulping tank, 300 ppm of dioctyltin distearate was added, and the first stage esterification reaction (255°C, 0.3 MPa, 1.0 h) and the second stage esterification reaction (265°C, 0.2 MPa, 0.5 h) were carried out in the first esterification kettle and the second esterification kettle respectively, and then pre-polycondensation (270°C, 25 kPa, 0.5 h) and polycondensation (275°C, 3.5 kPa, 0.5 h) were carried out in different polycondensation reactors, and then the obtained material APET resin (intrinsic viscosity 0.19 dl / g) and the 1,3-di-tert-butyl imidazole tetrafluoroborate and 2,3-cyclocarbonate glycerol ethyl acrylate were fed into a screw extruder in a weight ratio of 92:8:1.5, and after plasticization, melting and extrusion, vacuum treatment and filtration were carried out;

[0053] SS3: The PETG melt obtained in SS1 and the APET melt obtained in SS2 are passed through three different pipes to achieve three-layer composite extrusion in the distributor in the casting die head. The extrusion mass ratio of the upper layer PETG, the middle layer APET and the lower layer PETG is 1:1:2.5. The extrusion temperature is 270°C. The extruded melt is tightly attached to the quenching roller. The temperature of the quenching roller is 30°C and the rotation speed is 100m / min to obtain a cast sheet.

[0054] The cast sheet obtained by SS4:SS3 enters the longitudinal and transverse stretching areas through guide rollers, and is first stretched longitudinally and then stretched transversely; the longitudinal stretching conditions are: preheating temperature of 76±5°C, stretching ratio of 2, and cooling and setting temperature of 45±5°C; the transverse stretching conditions are: preheating temperature of 110±5°C, stretching ratio of 3.8, stretching temperature of 105±5°C, setting temperature of 140±5°C, and cooling temperature of 60±5°C, and a GAG heat-sealed composite film with a film thickness of 80μm is obtained, and the thickness ratio of the upper PETG layer, the middle layer APET and the lower layer PETG is 45:40:40.

[0055] Example 4

[0056] The preparation process is the same as that of Example 3, except that the 1,3-di-tert-butylimidazole tetrafluoroborate is replaced by 1-hexyl-3-methylimidazole tetrafluoroborate.

[0057] Example 5

[0058] The preparation process is the same as that of Example 3, except that the 1,3-di-tert-butylimidazole tetrafluoroborate is replaced by 1-heptyl-3-methylimidazole tetrafluoroborate.

[0059] Example 6

[0060] The preparation process is the same as that of Example 3, except that the 2,3-cyclocarbonate glyceryl ethyl acrylate is replaced by 2,3-cyclocarbonate glyceryl propyl acrylate.

[0061] Comparative Example 1

[0062] The preparation process is the same as that of Example 3, except that 1,3-di-tert-butylimidazole tetrafluoroborate is not added to the intermediate layer APET.

[0063] Comparative Example 2

[0064] The preparation process is the same as that of Example 3, except that no 2,3-cyclocarbonate glyceryl ethyl acrylate is added to the intermediate layer APET.

[0065] Comparative Example 3

[0066] The preparation process is the same as that of Example 3, except that the mass ratio of APET resin, 1,3-di-tert-butylimidazole tetrafluoroborate, and 2,3-cyclocarbonate glycerol ethyl acrylate in the intermediate layer APET is 92:8:1.8.

[0067] Comparative Example 4

[0068] The preparation process is the same as that of Example 3, except that the mass ratio of APET resin, 1,3-di-tert-butylimidazole tetrafluoroborate, and 2,3-cyclocarbonate glyceryl ethyl acrylate in the intermediate layer APET is 92:9:1.5.

[0069] Performance Testing

[0070] 1. Tensile strength and elongation at break: According to the provisions of "GB / T13022-1991 Test method for tensile properties of plastic films", the specimen is a strip with a length of 150 mm and a width of (15 ± 0.1) mm, the distance between the fixtures is 100 mm, and the test speed is (250 ± 25) mm / min;

[0071] 2. Light transmittance and haze: Test in accordance with GB / T 2410-2008 Test method for light transmittance and haze of transparent plastics;

[0072] 3. Crystal point detection: Cut 40cm×5 thick sheets from the entire width of the film, count the number of crystal points under the oblique illumination of the flashlight, and then calculate how many crystal points there are in 1m. The crystal points found are determined by the outer diameter of the crystal core: if the outer diameter of the crystal core is less than or equal to 1mm and greater than 0.5mm, the number of crystal points exceeds 2 / m or the outer diameter of the crystal core is greater than 1mm, it is unqualified and indicated by "×"; if the outer diameter of the crystal core is less than or equal to 1mm and greater than 0.5mm, the number of crystal points is less than or equal to 2, it is qualified and indicated by "O";

[0073] 4. Heat seal strength: Test according to “QB / T 2358-1998 Test method for heat seal strength of plastic film packaging bags”.

[0074] The test results are detailed in Table 1-1 and Table 1-2:

[0075]

[0076] From the above data, it can be seen that in Comparative Examples 1-2, alkyl imidazole tetrafluoroborate or 2,3-cyclocarbonate alkylene ester is lacking, the mechanical strength of the obtained film is poor, and the transmittance and haze are reduced, and the crystal points are increased. It can be seen that the presence or absence of these two substances affects the crystallinity of PETG and APET resins. In addition, the data of Comparative Examples 3-4 show that in the APET used as the middle layer, the mass ratio of the APET resin, 1,3-di-tert-butyl imidazole tetrafluoroborate, and 2,3-cyclocarbonate glyceryl ethyl acrylate will also affect the performance of the film, which may be because excessive addition will cause excessive internal forces in the film layer or uneven distribution.

[0077] In summary, the GAG ​​composite film prepared according to the preparation method provided by the present invention has better mechanical properties, excellent transparency and heat-sealing strength, and has considerable application prospects in the field of plastic sealing.

Claims

1. A GAG composite film, It is characterized in that The composite film is composed of an upper layer of PETG, a middle layer of APET and a lower layer of PETG; wherein the upper and lower layers of PETG are made of PETG resin and glass fiber in a weight ratio of 35-40:2-3; the middle layer of APET is made of APET resin, alkyl imidazole tetrafluoroborate, and 2,3-cyclocarbonate glycerol alkyl olefinate in a weight ratio of 85-92:5-8:1.2-1.5; the thickness of the GAG ​​composite film is 20-80 μm, the ratio of the sum of the thickness of the upper and lower layers of PETG to the thickness of the middle layer of APET is 60-85:15-40, and the thickness of the upper and lower layers of PETG are the same or different; The structure of the alkyl imidazole tetrafluoroborate is shown in Formula I: In Formula I, R 1 is a C1-4 alkyl group, R 2 is a C2-6 alkyl group; The preparation method of 2,3-cyclocarbonate glycerol alkyl olefinate comprises the following steps: S1: adding distilled alkenyl acid glycidyl ester and polar solvent into a high-pressure reactor, and adding quaternary ammonium salt catalyst and metal halide catalyst, sealing the reactor, introducing carbon dioxide through a valve and exhausting the air in the reactor, and closing the valve when the pressure in the reactor reaches 1.2-1.5MPa; S2: raising the temperature of the reaction kettle to 100-120° C., reacting at a constant temperature and high pressure for 4-5 hours, stopping the reaction and releasing the pressure to discharge the material when the pressure in the kettle no longer changes, washing with water to extract and separate to remove the catalyst, and removing the solvent by rotary evaporation, and finally performing column chromatography separation to obtain the 2,3-cyclocarbonate glyceryl alkyl olefinate; The alkenyl acid glycidyl ester in S1 is at least one of glycidyl acrylate, glycidyl methacrylate, and glycidyl ethacrylate; The quaternary ammonium salt catalyst in S1 is at least one of tetrapropylammonium bromide, tetrabutylammonium bromide, tetraethylammonium chloride, and tetrabutylammonium chloride; the metal halide is at least one of zinc chloride, zinc iodide, aluminum chloride, and aluminum iodide; and the total added mass of the quaternary ammonium salt catalyst and the metal halide accounts for 1-2% of the mass of the vinyl acid glycidyl ester.

2. The preparation process of the GAG ​​composite film according to claim 1, It is characterized in that The following steps are involved: SS1: Preparation of upper and lower PETG layers: terephthalic acid and ethylene glycol are added into a pulping tank at a molar ratio of 1:1.1-1.2, and a catalyst of 200-300 ppm is added. After the first stage esterification reaction in the first esterification kettle, the mixture is sent into the second esterification kettle together with 1,4-cyclohexanedimethanol for the second stage esterification reaction, and then pre-polycondensation and polycondensation reactions are carried out in the polycondensation kettle. After the polycondensation reaction is completed, the product and glass fiber are sent into a screw extruder according to the weight ratio, and after plasticization, melting, extrusion, vacuumization and filtration are carried out; SS2: Preparation of middle layer APET: terephthalic acid and ethylene glycol are added into a pulping tank at a molar ratio of 1:1.1-1.2, and a catalyst of 200-300 ppm is added. The first stage esterification reaction and the second stage esterification reaction are carried out in the first esterification kettle and the second esterification kettle respectively, and then pre-polycondensation and polycondensation are carried out in different polycondensation reaction kettles. Then, the obtained substance and the alkyl imidazole tetrafluoroborate and 2,3-cyclocarbonate glycerol alkyl acrylate are fed into a screw extruder according to a weight ratio, and after plasticization, melting and extrusion, vacuum treatment and filtration are carried out; SS3: The PETG melt obtained in SS1 and the APET melt obtained in SS2 are extruded in three layers in a distributor in a casting die through three different pipes. The extrusion temperature is 260-280°C. The extruded melt is tightly attached to a quenching roller. The temperature of the quenching roller is 20-30°C and the rotation speed is 80-100m / min to obtain a cast sheet. SS4: The cast sheet obtained from SS3 passes through guide rollers and enters the longitudinal and transverse stretching areas to obtain the GAG ​​composite film.

3. The preparation process of the GAG ​​composite film according to claim 2, It is characterized in that The amount of 1,4-cyclohexanedimethanol added to SS1 accounts for 20-30% of the total mass of terephthalic acid and ethylene glycol.

4. The preparation process of the GAG ​​composite film according to claim 2, It is characterized in that In SS1 and SS2, the temperature of the first stage esterification reaction is 250-255°C, and the pressure is 0.2-0.3MPa; the temperature of the second stage esterification reaction is 260-265°C, and the pressure is 0.2-0.3Mpa, and the esterification rate is 96-98%; the temperature of the pre-polycondensation reaction is 265-270°C, and the reaction pressure is 20-25kPa; the temperature of the polycondensation reaction is 270-275°C, and the reaction pressure is 3.0-3.5kPa, and the intrinsic viscosity of the obtained substance is 0.17-0.20dl / g.

5. The preparation process of the GAG ​​composite film according to claim 2, It is characterized in that In SS1 and SS2, the moisture content of the product obtained after filtration is ≤50ppm; the extrusion mass ratio of the upper layer PETG, the middle layer APET and the lower layer PETG is 1:0.25-1:2.

5.

6. The preparation process of the GAG ​​composite film according to claim 2, It is characterized in that In SS4, the heat treatment zone length of the longitudinal stretching is 8-10m, the temperature of the preheating zone is 70-95°C, the time is 8-15s, and the stretching ratio is 1-2 times; the transverse stretching is divided into five zones, namely, preheating zone, stretching zone, buffer zone, heat setting zone, and cooling zone. The preheating temperature is 90-110°C, the stretching temperature is 90-115°C, the heat setting temperature is 125-145°C, the cooling temperature is 45-65°C, and the stretching ratio is 2.0-3.8 times.