Submicron ammonium rhenate and preparation method thereof, and rhenium powder

Submicron ammonium rhenate is prepared through atomization and vacuum sublimation drying technology, and rhenium powder is prepared through reduction roasting, which solves the problem of difficulty in preparing ammonium rhenate and rhenium powder with a particle size of <1 μm in the existing technology, and achieves fine particle size The rhenium powder raw materials are guaranteed to meet the needs of the high-temperature alloy field.

CN118495595BActive Publication Date: 2024-10-29BEIJING MINING & METALLURGICAL TECH GRP CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410955749.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-29
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

The existing technology is difficult to prepare high-purity ammonium rhenate and rhenium powder with a particle size of <1 μm, and cannot meet the particle size requirements of rhenium alloys for rhenium powder.

Method used

By atomizing the ammonium rhenate solution, mixing frozen air to form ice crystals, and performing vacuum sublimation drying in a vacuum environment, submicron ammonium rhenate is prepared, and then rhenium powder is prepared through reduction roasting.

Benefits of technology

Submicron ammonium rhenate and rhenium powder with a particle size of <1 μm were successfully prepared to meet the particle size requirements for rhenium powder in the field of high-temperature alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118495595B_ABST
    Figure CN118495595B_ABST
Patent Text Reader

Abstract

The present application provides a submicron ammonium rhenate and a preparation method thereof, and rhenium powder, and relates to the field of rhenium powder preparation. The method comprises: atomizing an ammonium rhenate solution to obtain droplets, mixing the droplets with refrigerated air to obtain ice crystals, and vacuum sublimating and drying the ice crystals in a vacuum environment to obtain the submicron ammonium rhenate. The method first atomizes the ammonium rhenate solution to obtain small droplets, and then the fine mist is instantly cooled under low-temperature refrigerated air to form ice crystals, and vacuum sublimating and drying the ice crystals in a vacuum environment, so that the frozen water in the ice crystals sublimates from the solid particles, and the water molecules are detached from the surface of the particles and are extracted, thereby obtaining submicron ammonium rhenate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of rhenium powder preparation, and in particular to submicron ammonium rhenate and a preparation method thereof, and rhenium powder. Background Art

[0002] Rhenium is a rare metal element with high melting and boiling points, high density and resistance to thermal fatigue. It is known as a "strategic metal", "aerospace metal" and "super metal". About 65% of the global rhenium production is used in the aerospace field, mainly in high-temperature alloy parts of aircraft engine jet engines; 22% is used in petroleum catalysts to produce lead-free and high-octane gasoline; other applications include the preparation of rhenium filaments and tungsten-rhenium alloys, which are then used in mass spectrometers, ionization pressure gauges and modified nickel-based high-temperature alloys.

[0003] High-purity rhenium powder is the main raw material for preparing rhenium alloys. At present, the ammonium rhenate hydrogen reduction method is the only industrial method for large-scale production of high-purity rhenium powder. Therefore, as the main compound for preparing high-purity rhenium industrial products, the particle size of high-purity ammonium rhenate directly affects the particle size of high-purity rhenium powder in the hydrogen reduction production process. The particle size of the currently prepared high-purity ammonium rhenate is greater than 1μm, and the particle size of rhenium powder is greater than 1μm. There is no ammonium rhenate and rhenium powder preparation less than 1μm. Therefore, the crystal morphology of ammonium rhenate is optimized to prepare ammonium rhenate less than 1μm, and then prepare rhenium powder less than 1μm by reduction to meet the demand for rhenium powder particle size in rhenium alloys. Summary of the invention

[0004] The purpose of the present application is to provide a submicron ammonium rhenate and a preparation method thereof, and rhenium powder to solve the above-mentioned problems.

[0005] To achieve the above objectives, the present application provides a first aspect of a method for preparing submicron ammonium rhenate, comprising:

[0006] atomizing the ammonium rhenate solution to obtain droplets;

[0007] The mist droplets and the refrigerated air are mixed to obtain ice crystals;

[0008] Under a vacuum environment, the ice crystals are vacuum sublimated and dried to obtain the submicron ammonium rhenate.

[0009] Optionally, the method for preparing submicron ammonium rhenate satisfies at least one of the following conditions:

[0010] A. the concentration of the ammonium rhenate solution is ≤50 g / L;

[0011] B. the temperature of the ammonium rhenate solution before atomization is 20° C.-30° C.;

[0012] C. The temperature of the refrigerated air is minus 30°C to minus 80°C;

[0013] D. The vacuum degree of the vacuum environment is ≤100Pa;

[0014] E. The vacuum degree after the vacuum sublimation drying is completed is ≤5Pa;

[0015] F. The vacuum sublimation drying is carried out at a temperature of 40°C-50°C and for a time of 24h-48h.

[0016] Optionally, the atomization includes conveying the ammonium rhenate solution to an atomizer by a peristaltic pump, and the atomizer disperses the ammonium rhenate solution into the droplets.

[0017] Optionally, the flow rate of the peristaltic pump is ≤20 mL / min.

[0018] Optionally, the method for preparing submicron ammonium rhenate satisfies at least one of the following conditions:

[0019] A. The particle size of the submicron ammonium rhenate is ≤1 μm;

[0020] B. The submicron ammonium rhenate has a granular and / or needle-like morphology.

[0021] Optionally, the following conditions must be met to obtain the granular submicron ammonium rhenate:

[0022] A. The concentration of the ammonium rhenate solution is 10 g / L-20 g / L;

[0023] B. The flow rate of the peristaltic pump is 10mL / min-20mL / min;

[0024] C. The temperature of the refrigerated air is minus 30°C to minus 50°C.

[0025] Optionally, the method for preparing submicron ammonium rhenate satisfies at least one of the following conditions:

[0026] A. the aspect ratio of the needle-shaped submicron ammonium rhenate is greater than or equal to 5:1;

[0027] B. The following conditions must be met to obtain the needle-shaped submicron ammonium rhenate:

[0028] 1) The concentration of the ammonium rhenate solution is ≤10 g / L;

[0029] 2) The flow rate of the peristaltic pump is ≤5 mL / min;

[0030] 3) The temperature of the refrigerated air is minus 40°C to minus 80°C.

[0031] A second aspect of the present application provides submicron ammonium rhenate, which is prepared by the preparation method of submicron ammonium rhenate.

[0032] The third aspect of the present application provides a rhenium powder, which is prepared by reduction roasting of the submicron ammonium rhenate.

[0033] Optionally, the reduction roasting is carried out at a temperature of 300°C-750°C and for a time of 4h-12h.

[0034] Compared with the prior art, the beneficial effects of this application include:

[0035] The preparation method of submicron ammonium rhenate provided in the present application comprises the following steps: firstly atomizing the ammonium rhenate solution to obtain small droplets, then passing through low-temperature refrigerated air, the fine mist is instantly cooled to form ice crystals, and the ice crystals are vacuum sublimated and dried under a vacuum environment, so that the frozen water in the ice crystals sublimates from the solid particles, and the water molecules are detached from the surface of the particles and extracted, thereby obtaining submicron ammonium rhenate.

[0036] The submicron ammonium rhenate provided in the present application has fine particle size, with a particle size of less than 1 μm, and provides raw material particle size guarantee for the preparation of submicron rhenium powder.

[0037] The rhenium powder provided in the present application has a fine particle size, with a particle size of less than 1 μm, and can meet the demand for rhenium powder particle size in the field of high-temperature alloys. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0039] Figure 1 This is a scanning electron microscope image of the granular submicron ammonium rhenate prepared in Example 1;

[0040] Figure 2 This is a scanning electron microscope image of the rhenium powder prepared in Example 1;

[0041] Figure 3 This is a scanning electron microscope image of the needle-shaped submicron ammonium rhenate prepared in Example 2;

[0042] Figure 4 This is a scanning electron microscope image of the rhenium powder prepared in Example 2;

[0043] Figure 5 This is a scanning electron microscope image of the granular and needle-shaped mixed submicron ammonium rhenate prepared in Example 3;

[0044] Figure 6 This is a scanning electron microscope image of the rhenium powder prepared in Example 3;

[0045] Figure 7 This is a scanning electron microscope image of the ammonium rhenate prepared in Comparative Example 1. DETAILED DESCRIPTION

[0046] As used herein:

[0047] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0048] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0049] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range.

[0050] In these examples, parts and percentages are by mass unless otherwise indicated.

[0051] "Mass parts" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass parts of component A are a parts and the mass parts of component B are b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass parts of all components is not limited to 100 parts.

[0052] “And / or” is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0053] The first aspect of the present application provides a method for preparing submicron ammonium rhenate, comprising:

[0054] atomizing the ammonium rhenate solution to obtain droplets;

[0055] The mist droplets and the refrigerated air are mixed to obtain ice crystals;

[0056] Under a vacuum environment, the ice crystals are vacuum sublimated and dried to obtain the submicron ammonium rhenate.

[0057] In some embodiments, the method for preparing submicron ammonium rhenate satisfies at least one of the following conditions:

[0058] A. the concentration of the ammonium rhenate solution is ≤50 g / L;

[0059] Optionally, the concentration of the ammonium rhenate solution may be 1 g / L, 5 g / L, 10 g / L, 15 g / L, 20 g / L, 25 g / L, 30 g / L, 35 g / L, 40 g / L, 45 g / L, 50 g / L or any value ≤ 50 g / L;

[0060] Preferably, the concentration of the ammonium rhenate solution is ≤20 g / L;

[0061] It should be noted that when the concentration of ammonium rhenate is ≤20g / L, since the freezing spray atomizer is above the material bin and the temperature is relatively low, it can prevent the high concentration ammonium rhenate solution from crystallizing and clogging the atomizer during the process of flowing through the atomizer by the peristaltic pump.

[0062] B. the temperature of the ammonium rhenate solution before atomization is 20° C.-30° C.;

[0063] Optionally, the temperature of the ammonium rhenate solution before atomization can be 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C or any value between 20°C and 30°C;

[0064] It should be noted that the temperature of the ammonium rhenate solution before atomization can be room temperature without additional heating.

[0065] C. The temperature of the refrigerated air is minus 30°C to minus 80°C;

[0066] Optionally, the temperature of the refrigerated air may be minus 30°C, minus 35°C, minus 40°C, minus 45°C, minus 50°C, minus 55°C, minus 60°C, minus 65°C, minus 70°C, minus 75°C, minus 80°C or any value between minus 30°C and minus 80°C;

[0067] It should be noted that when the temperature of the frozen air is minus 30℃ - minus 80℃, ice crystals can form quickly.

[0068] D. The vacuum degree of the vacuum environment is ≤100Pa;

[0069] Optionally, the vacuum degree of the vacuum environment may be 10Pa, 20Pa, 30Pa, 40Pa, 50Pa, 60Pa, 70Pa, 80Pa, 90Pa, 100Pa or any value ≤100Pa;

[0070] Preferably, the vacuum degree of the vacuum environment is 10Pa-50Pa;

[0071] E. The vacuum degree after the vacuum sublimation drying is completed is ≤5Pa;

[0072] Optionally, the vacuum degree after vacuum sublimation drying is completed can be 0.1Pa, 1Pa, 2Pa, 3Pa, 4Pa, 5Pa or any value ≤5Pa;

[0073] It should be noted that when the vacuum degree is ≤5Pa, it means that the drying is complete, and the vacuum degree determines the degree of drying completion;

[0074] In some embodiments, the material chamber is evacuated after obtaining the ice crystals;

[0075] It should be noted that the role of vacuum is to reduce the air pressure in the drying chamber, making it easier for ice crystals to evaporate during the drying process; increasing the vacuum degree is conducive to the vaporization of water at a lower temperature, but when the vacuum degree is greater than 100Pa, it is not conducive to heat conduction and affects the heating effect on the material.

[0076] F. The vacuum sublimation drying is carried out at a temperature of 40°C-50°C and for a time of 24h-48h.

[0077] Optionally, the temperature of vacuum sublimation drying can be 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C, 50°C or any value between 40°C and 50°C, and the time can be 24h, 26h, 28h, 30h, 32h, 34h, 36h, 38h, 40h, 42h, 44h, 46h, 48h or any value between 24h and 48h.

[0078] It should be noted that when the vacuum sublimation drying temperature is 40℃-50℃ and the time is 24h-48h, the sublimation speed can be accelerated and energy can be provided for sublimation.

[0079] It can be understood that, in a vacuum environment, the material chamber is heated for sublimation. This is because the sublimation process is an endothermic process, and appropriate heating can provide the energy required for sublimation and promote the sublimation process.

[0080] In some embodiments, the atomization includes delivering the ammonium rhenate solution to an atomizer by a peristaltic pump, and the atomizer disperses the ammonium rhenate solution into the mist droplets.

[0081] In some embodiments, the flow rate of the peristaltic pump is ≤20 mL / min.

[0082] Optionally, the flow rate of the peristaltic pump can be 1 mL / min, 2 mL / min, 5 mL / min, 10 mL / min, 15 mL / min, 20 mL / min, or any value ≤ 20 mL / min.

[0083] It should be noted that when the flow rate of the peristaltic pump is ≤20mL / min, the ammonium rhenate solution is transported to the atomizer by the peristaltic pump, and the atomizer disperses the ammonium rhenate solution into droplets. The droplets and the refrigerated air are fully mixed to directly form fine ice crystals and fall to the bottom of the material bin. When the flow rate is greater than 20mL / min, and there are too many droplets in the refrigerated air, some droplets cannot directly form fine droplets, and fall to the bottom of the material bin in liquid state to form large ice cubes, causing the sublimated ammonium rhenate particles to agglomerate and increase in particle size.

[0084] In some embodiments, the method for preparing submicron ammonium rhenate satisfies at least one of the following conditions:

[0085] A. The particle size of the submicron ammonium rhenate is ≤1 μm;

[0086] Optionally, the particle size of the submicron ammonium rhenate may be 0.001 μm, 0.005 μm, 0.01 μm, 0.05 μm, 0.1 μm, 0.5 μm, 1 μm or any value ≤ 1 μm;

[0087] B. The submicron ammonium rhenate has a granular and / or needle-like morphology.

[0088] It should be noted that when the submicron ammonium rhenate has a needle-like morphology, its particle size is the width of the needle-like submicron ammonium rhenate.

[0089] In some embodiments, the following conditions must be met to obtain the submicron ammonium rhenate in the granular form:

[0090] A. The concentration of the ammonium rhenate solution is 10 g / L-20 g / L;

[0091] Optionally, the concentration of the ammonium rhenate solution for obtaining the granular submicron ammonium rhenate may be 10 g / L, 11 g / L, 12 g / L, 13 g / L, 14 g / L, 15 g / L, 16 g / L, 17 g / L, 18 g / L, 19 g / L, 20 g / L or any value between 10 g / L and 20 g / L;

[0092] B. The flow rate of the peristaltic pump is 10mL / min-20mL / min;

[0093] Optionally, the flow rate of the peristaltic pump for obtaining granular submicron ammonium rhenate can be 10 mL / min, 11 mL / min, 12 mL / min, 13 mL / min, 14 mL / min, 15 mL / min, 16 mL / min, 17 mL / min, 18 mL / min, 19 mL / min, 20 mL / min or any value between 10 mL / min and 20 mL / min;

[0094] C. The temperature of the refrigerated air is minus 30°C to minus 50°C.

[0095] Optionally, the temperature of the refrigerated air for obtaining the granular submicron ammonium rhenate may be minus 30°C, minus 35°C, minus 40°C, minus 45°C, minus 50°C, or any value between minus 30°C and minus 50°C.

[0096] It should be noted that the submicron ammonium rhenate granules are the result of the combined effect of the flow rate of the peristaltic pump, the concentration of the ammonium rhenate solution, and the temperature of the refrigerated air.

[0097] In some embodiments, the method for preparing submicron ammonium rhenate satisfies at least one of the following conditions:

[0098] A. the aspect ratio of the needle-shaped submicron ammonium rhenate is greater than or equal to 5:1;

[0099] Optionally, the aspect ratio of the needle-shaped submicron ammonium rhenate may be 5:1, 10:1, 15:1, 20:1, 50:1, or any value greater than or equal to 5:1;

[0100] B. The following conditions must be met to obtain the needle-shaped submicron ammonium rhenate:

[0101] 1) The concentration of the ammonium rhenate solution is ≤10 g / L;

[0102] Optionally, the concentration of the ammonium rhenate solution for obtaining the needle-shaped submicron ammonium rhenate may be 10 g / L, 9 g / L, 5 g / L, 1 g / L, 0.1 g / L or any value ≤ 10 g / L;

[0103] 2) The flow rate of the peristaltic pump is ≤5 mL / min;

[0104] Optionally, the flow rate of the peristaltic pump for obtaining the needle-shaped submicron ammonium rhenate may be 5 mL / min, 4 mL / min, 3 mL / min, 2 mL / min, 1 mL / min, 0.1 mL / min, 0.01 mL / min or any value ≤ 5 mL / min;

[0105] 3) The temperature of the refrigerated air is minus 40°C to minus 80°C.

[0106] Optionally, the temperature of the refrigerated air for obtaining the needle-shaped submicron ammonium rhenate can be minus 40°C, minus 45°C, minus 50°C, minus 55°C, minus 60°C, minus 65°C, minus 70°C, minus 75°C, minus 80°C or any value between minus 40°C and minus 80°C.

[0107] It should be noted that when the flow rate of the peristaltic pump is ≤5mL / min, the temperature of the refrigerated air is -40℃--80℃, and the concentration of the ammonium rhenate solution is ≤10g / L, needle-shaped ammonium rhenate crystals can be formed. This is due to the slow flow rate of the peristaltic pump, the low concentration of the ammonium rhenate solution, and the long freezing process of the spray during the falling process, resulting in the final needle-shaped ammonium rhenate crystal morphology.

[0108] A second aspect of the present application provides submicron ammonium rhenate, which is prepared by the preparation method of submicron ammonium rhenate.

[0109] The third aspect of the present application provides a rhenium powder, which is prepared by reduction roasting of the submicron ammonium rhenate.

[0110] In some embodiments, the reduction roasting is performed at a temperature of 300° C. to 750° C. for a time of 4 h to 12 h.

[0111] Optionally, the temperature of the reduction roasting can be 300℃, 350℃, 400℃, 450℃, 500℃, 550℃, 600℃, 650℃, 700℃, 750℃ or a range value between 300℃-750℃, and the time can be 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h or a range value between 4h-12h.

[0112] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0113] Example 1

[0114] This embodiment provides a submicron ammonium rhenate and a preparation method thereof, comprising:

[0115] Dissolving ammonium rhenate in deionized water to prepare a 20 g / L ammonium rhenate solution, the initial temperature of the ammonium rhenate solution being 30° C., and precooling a material bin of a vacuum freeze spray drying system in a vacuum freeze spray dryer, the precooling temperature being minus 30° C.;

[0116] The ammonium rhenate solution is transported to the atomizer by a peristaltic pump and dispersed into fine droplets. The flow rate of the peristaltic pump is 20mL / min. The fine mist is instantly cooled by the frozen air in the material bin of the vacuum freeze spray drying system to form ice crystals.

[0117] After all the ammonium rhenate solution has formed ice crystals, the material bin is evacuated to a vacuum degree of 95 Pa, and the system enters the freeze-drying stage. The moisture in the ice crystals is quickly vacuum sublimated and dried. The vacuum sublimation drying temperature is 50°C and the time is 36 hours. After the vacuum sublimation drying is completed, the vacuum degree is 5 Pa, and 0.5 μm granular submicron ammonium rhenate is prepared.

[0118] The scanning electron microscope image of the granular submicron ammonium rhenate is as follows Figure 1 shown.

[0119] The present application also provides a rhenium powder, which is prepared by reduction roasting of the above-mentioned submicron ammonium rhenate, and the reduction roasting temperature is 450° C. and the time is 4 hours.

[0120] The scanning electron microscope image of the rhenium powder is as follows Figure 2 shown.

[0121] Example 2

[0122] This embodiment provides a submicron ammonium rhenate and a preparation method thereof, comprising:

[0123] Dissolving ammonium rhenate in deionized water to prepare a 5 g / L ammonium rhenate solution, the initial temperature of the ammonium rhenate solution being 20° C., and precooling a material bin of a vacuum freeze spray drying system in a vacuum freeze spray dryer, the precooling temperature being minus 70° C.;

[0124] The ammonium rhenate solution is transported to the atomizer by a peristaltic pump and dispersed into fine droplets. The flow rate of the peristaltic pump is 3mL / min. The fine mist is instantly cooled by the frozen air in the material bin of the vacuum freeze spray drying system to form ice crystals.

[0125] After all the ammonium rhenate solution has formed ice crystals, the material bin is evacuated to a vacuum degree of 90 Pa, and the system enters the freeze-drying stage. The moisture in the ice crystals is quickly vacuum sublimated and dried. The vacuum sublimation drying temperature is 40°C and the time is 48 hours. After the vacuum sublimation drying is completed, the vacuum degree is 4 Pa, and 0.8 μm needle-shaped submicron ammonium rhenate is prepared.

[0126] The scanning electron microscope image of the needle-shaped submicron ammonium rhenate is as follows Figure 3 shown.

[0127] The present application also provides a rhenium powder, which is prepared by reduction roasting of the above-mentioned submicron ammonium rhenate, and the reduction roasting temperature is 550° C. and the time is 6 hours.

[0128] The scanning electron microscope image of the rhenium powder is as follows Figure 4 shown.

[0129] Example 3

[0130] This embodiment provides a submicron ammonium rhenate and a preparation method thereof, comprising:

[0131] Dissolving ammonium rhenate in deionized water to prepare a 10 g / L ammonium rhenate solution, the initial temperature of the ammonium rhenate solution being 25° C., and precooling a material bin of a vacuum freeze spray drying system in a vacuum freeze spray dryer at a precooling temperature of minus 40° C.;

[0132] The ammonium rhenate solution is transported to the atomizer by a peristaltic pump and dispersed into fine droplets. The flow rate of the peristaltic pump is 8 mL / min. The fine mist is instantly cooled by the frozen air in the material bin of the vacuum freeze spray drying system to form ice crystals.

[0133] After all the ammonium rhenate solution has formed ice crystals, the material bin is evacuated to a vacuum degree of 98 Pa, and the system enters the freeze-drying stage. The moisture in the ice crystals is quickly vacuum sublimated and dried. The vacuum sublimation drying temperature is 42°C and the time is 48 hours. The vacuum degree after the vacuum sublimation drying is completed is 4.5 Pa, and 0.9 μm granular and needle-shaped mixed submicron ammonium rhenate is prepared.

[0134] The scanning electron microscope image of the granular and needle-shaped mixed submicron ammonium rhenate is as follows: Figure 5 shown.

[0135] The present application also provides a rhenium powder, which is prepared by reduction roasting of the above-mentioned submicron ammonium rhenate, and the reduction roasting temperature is 350° C. and the time is 8 hours.

[0136] The scanning electron microscope image of the rhenium powder is as follows Figure 6 shown.

[0137] Comparative Example 1

[0138] This comparative example provides ammonium rhenate and a preparation method thereof, and rhenium powder. The difference from Example 1 is that in this comparative example, 20 g / L of ammonium rhenate solution is directly placed in a -10°C freezer and frozen to 0°C, and after solid-liquid separation, the ammonium rhenate crystals are obtained by drying.

[0139] The particle size of the ammonium rhenate crystals was 200 μm.

[0140] The scanning electron microscope image of the ammonium rhenate crystal is as follows Figure 7 shown.

[0141] Comparative Example 2

[0142] This comparative example provides an ammonium rhenate and a preparation method thereof, and rhenium powder. The difference from Example 1 is that the concentration of the ammonium rhenate solution in this comparative example is 80 g / L, and other conditions are consistent with Example 1.

[0143] The particle size of the ammonium rhenate crystals was 4.5 μm.

[0144] Comparative Example 3

[0145] This comparative example provides ammonium rhenate and a preparation method thereof, and rhenium powder. The difference from Example 1 is that the temperature of the refrigerated air in this comparative example is minus 20° C., and other conditions are consistent with Example 1.

[0146] The particle size of the ammonium rhenate crystals was 2 μm.

[0147] Comparative Example 4

[0148] This comparative example provides ammonium rhenate and a preparation method thereof, and rhenium powder. The difference from Example 1 is that the vacuum degree of the vacuum environment of this comparative example is 200 Pa, and other conditions are consistent with Example 1.

[0149] The particle size of the ammonium rhenate crystals was 1.8 μm.

[0150] Comparative Example 5

[0151] This comparative example provides ammonium rhenate and a preparation method thereof, and rhenium powder. The difference from Example 1 is that the flow rate of the peristaltic pump in this comparative example is 25 mL / min, and other conditions are consistent with Example 1.

[0152] The particle size of the ammonium rhenate crystals was 1.3 μm.

[0153] It can be seen from the above embodiments and comparative examples that in comparative example 1, the ammonium rhenate solution is directly frozen, and the particle size of the ammonium rhenate crystals obtained is large;

[0154] When the concentration of the ammonium rhenate solution in Comparative Example 2 is higher than the concentration range specified in the present application, the high-concentration ammonium rhenate solution crystallizes when flowing through the atomizer by the peristaltic pump, and agglomerated crystals are formed during the atomization process. The dispersion of the liquid during the atomization process decreases, which, on the one hand, causes the particle size of the ammonium rhenate obtained by sublimation to become coarser, and on the other hand, it is easy to clog the atomization port of the atomizer, causing the atomization process to be interrupted.

[0155] When the temperature of the refrigerated air in Comparative Example 3 is minus 20°C, which is higher than the temperature range specified in the present application, as the atomization process transports droplets to the material bin, the refrigerated air combines with the droplets to form ice crystals. This process is an exothermic process, which will cause the temperature of the material bin to rise. When the refrigerated air is minus 20°C, the exothermic process will cause the temperature of the material bin to approach zero degrees, and the ice crystals will partially melt into liquid. Later, as the temperature drops, large ice cubes will be formed, causing the sublimation ammonium rhenate particle size to become larger.

[0156] When the vacuum degree of the vacuum environment of Comparative Example 4 is 200 Pa, the higher the vacuum degree value, the lower the vacuum degree. The vacuum degree of Comparative Example 4 is lower than the vacuum degree range specified in the present application, and the air pressure in the material bin is still relatively high. The ice crystals are not easy to evaporate during the drying process, and the vaporization time of water at a lower temperature is prolonged, which is not conducive to heat conduction, resulting in the agglomeration of the ammonium rhenate particles obtained by sublimation and the increase of the particle size.

[0157] When the flow rate of the peristaltic pump of Comparative Example 5 is 25 mL / min, it is higher than the flow rate range specified in the present application. At the same time, there are too many droplets in the refrigerated air, and some droplets cannot directly form fine droplets. After falling to the bottom of the material bin in a liquid state, large ice cubes are formed, causing the sublimated ammonium rhenate particles to agglomerate and increase in particle size.

[0158] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

[0159] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.

Claims

1. A method for preparing submicron ammonium rhenate, characterized in that: include: atomizing the ammonium rhenate solution to obtain droplets; The mist droplets and the refrigerated air are mixed to obtain ice crystals; Under a vacuum environment, the ice crystals are vacuum sublimated and dried to obtain the submicron ammonium rhenate; The concentration of the ammonium rhenate solution is ≤50 g / L; The temperature of the refrigerated air is minus 30°C to minus 80°C; The vacuum degree of the vacuum environment is ≤100Pa; The vacuum degree after the vacuum sublimation drying is completed is ≤5Pa; The atomization includes delivering the ammonium rhenate solution to an atomizer by a peristaltic pump, and the atomizer disperses the ammonium rhenate solution into the droplets; The flow rate of the peristaltic pump is ≤20 mL / min.

2. The method for preparing submicron ammonium rhenate according to claim 1, characterized in that: At least one of the following conditions is met: A. the temperature of the ammonium rhenate solution before atomization is 20° C.-30° C.; B. The vacuum sublimation drying is carried out at a temperature of 40°C-50°C and for a time of 24h-48h.

3. The method for preparing submicron ammonium rhenate according to claim 1, characterized in that: At least one of the following conditions is met: A. The particle size of the submicron ammonium rhenate is ≤1 μm; B. The submicron ammonium rhenate has a granular and / or needle-like morphology.

4. The method for preparing submicron ammonium rhenate according to claim 3, characterized in that: The following conditions must be met to obtain the submicron ammonium rhenate in the granular form: A. The concentration of the ammonium rhenate solution is 10 g / L-20 g / L; B. The flow rate of the peristaltic pump is 10mL / min-20mL / min; C. The temperature of the refrigerated air is minus 30°C to minus 50°C.

5. The method for preparing submicron ammonium rhenate according to claim 3, characterized in that: At least one of the following conditions is met: A. the aspect ratio of the needle-shaped submicron ammonium rhenate is greater than or equal to 5:1; B. The following conditions must be met to obtain the needle-shaped submicron ammonium rhenate: 1) The concentration of the ammonium rhenate solution is ≤10 g / L; 2) The flow rate of the peristaltic pump is ≤5 mL / min; 3) The temperature of the refrigerated air is minus 40°C to minus 80°C.

Citation Information

Patent Citations

  • Method and apparatus for atomizing, freezing and drying for powder production by using low-temperature low-dew point gas

    CN101403561A

  • Method for preparing ultra-pure ammonium rhenate crystals with controllable particle sizes

    CN110527854A

  • Method for purifying ammonium rhenate

    CN114314672A

  • Pyrogenic process for recovering rhenium-containing material

    CN118291786A

  • Method of the Preparation of Fibrillar and Lamellar Porous Microstructures and Nanostructures by Means of Controlled Vacuum Freeze-Drying of Liquid Nanoparticles Dispersions

    US20140230264A1