An organic small molecule inhibitor and its application method in thin film deposition

By using organic small molecule inhibitors with steric hindrance and multi-functional groups, the problems of deposition unevenness and performance degradation in 3D nanostructures are solved, achieving uniform deposition of films from top to bottom and high step coverage.

CN118496107BActive Publication Date: 2024-10-29HEFEI ADCHEM SEMI-TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410962766.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-29
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

In high-aspect-ratio 3D nanostructures, atomic layer deposition technology easily forms seams or voids during the top-down gap filling process, resulting in reduced device performance. Existing inhibitors also inhibit the deposition at the bottom of the trench, resulting in Uneven fill and poor step coverage.

Method used

Provide an organic small molecule inhibitor with steric hindrance and multi-functional groups that can effectively cover the active sites at the top of the substrate without inhibiting the bottom sites, reduce precursor adsorption, and promote uniform top-down deposition of the film . The chemical structure of the inhibitor includes specific central atoms and functional groups to ensure full inhibitory effect on the substrate.

Benefits of technology

It significantly improves the step coverage and uniformity of film deposition, reduces uneven filling at the bottom of the trench, and improves device performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118496107B_ABST
    Figure CN118496107B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of semiconductor technology, and specifically discloses an organic small molecule inhibitor. The organic small molecule inhibitor provided by the present invention has both certain steric hindrance and multi-functional group effect, so that the inhibitor can cover more active sites on the top of the substrate through the steric hindrance effect, and the bottom active sites are not inhibited; the present invention also provides an application method of the organic small molecule inhibitor in thin film deposition, through which it can be proved that the organic small molecule inhibitor can be conducive to the uniform deposition of the thin film from top to bottom, and significantly improve the step coverage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of semiconductor technology, and in particular relates to an organic small molecule inhibitor and an application method thereof in thin film deposition. Background Art

[0002] As human society enters the era of artificial intelligence, higher requirements are placed on the storage density and performance of devices. Atomic layer deposition technology (ALD) plays a vital role in the semiconductor field due to its excellent coating conformality and self-limiting properties. However, in 3D nanostructures with high aspect ratios, such as holes or trenches, ALD deposition often forms seams or voids during the top-down gap filling process, resulting in reduced device performance, electrical or thermal conductivity, and mechanical properties. Inhibitors are usually introduced during the deposition process to inhibit top deposition, while bottom deposition is not affected or is only weakly inhibited, thereby enhancing the uniformity of top-down filling of the deposited film, improving step coverage, and eliminating seams or voids. Existing inhibitors not only inhibit deposition at the top of the trench, but also have a certain inhibitory effect on deposition at the bottom of the trench, resulting in a certain degree of non-uniformity in the filling and poor step coverage improvement. For example, patent US20220119939A1 proposes organic small molecule inhibitors, taking triethylamine (TEA), tetrahydrofuran (THF), and ethylene glycol dimethyl ether (DME) as examples. The inhibitor molecules are gently physically adsorbed on high aspect ratio substrates, competing with precursor molecules for active sites on the substrate surface, inhibiting excessive adsorption of precursors on the top of the substrate, thereby improving step coverage. However, these inhibitors often also inhibit the growth of thin films at the bottom of the substrate, resulting in poor effects or poor process stability, so there is still a need to find more suitable inhibitors. Summary of the invention

[0003] The purpose of the present invention is to overcome the above problems existing in the prior art and to provide an organic small molecule inhibitor, which has both certain steric hindrance and contains multiple functional groups. Compared with previous inhibitor molecules, the inhibitor can cover more active sites on the top of the substrate through the steric hindrance effect, and leave the bottom active sites uninhibited; the inhibitor contains multiple functional groups, which increases the probability of binding with the active sites of the substrate, effectively reduces the adsorption of the precursor on the top of the substrate, is conducive to the uniform deposition of the thin film from top to bottom, and significantly improves the step coverage.

[0004] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0005] The embodiment of the first aspect of the present invention provides an organic small molecule inhibitor, the chemical structure of the organic small molecule inhibitor is shown in formula (I):

[0006] (I);

[0007] Wherein, M is N, P or B;

[0008] X1, X2, and X3 are all integers greater than or equal to 1;

[0009] R 1 , R 2 , R 3 Any one selected from H, C1-C10 aliphatic or cycloaliphatic substituents;

[0010] R 4 , R 5 , R 6 to exist or not to exist;

[0011] Y 1 , Y 2 , Y 3 It is any one of O, N, S, -OC=O, -C=O, where:

[0012] When Y 1 , Y 2 , Y 3 When it is O, S, -OC=O or -C=O, then R 4 , R 5 , R 6 does not exist;

[0013] When Y 1 , Y 2 , Y 3 When both are N, then R 4 , R 5 , R 6 Both exist;

[0014] When Y 1 N and Y 2 , Y 3 When it is O, S, -OC=O or -C=O, then R 4 Exists and R 5 , R 6 does not exist;

[0015] When Y 2 N and Y 1 , Y 3 When it is O, S, -OC=O or -C=O, then R 5 Exists and R 4 , R 6 does not exist;

[0016] When Y 3 N and Y 1 , Y 2When it is O, S, -OC=O or -C=O, then R 6 Exists and R 4 , R 5 does not exist;

[0017] When Y 1 , Y 2 N and Y 3 When it is O, S, -OC=O or -C=O, then R 4 , R 5 Exists and R 6 does not exist;

[0018] When Y 1 , Y 3 N and Y 2 When it is O, S, -OC=O or -C=O, then R 4 , R 6 Exists and R 5 does not exist;

[0019] When Y 2 , Y 3 N and Y 1 When it is O, S, -OC=O or -C=O, then R 5 , R 6 Exists and R 4 does not exist;

[0020] And, when R 4 , R 5 , R 6 When present, R 4 , R 5 , R 6 are independently any one of H, C1-C10 aliphatic or cycloaliphatic substituents.

[0021] Furthermore, the C1-C10 aliphatic or cycloaliphatic substituent is any one of an alkyl group, a cycloalkyl group, an alkenyl group, a cycloalkenyl group, an alkynyl group, and a cycloalkynyl group.

[0022] Furthermore, X1, X2, and X3 are all integers of 1-10, preferably integers of 1-5.

[0023] Preferably, X1, X2, and X3 are all integers of 1-3.

[0024] In one embodiment, the M is N, and the inhibitors include but are not limited to:

[0025]

[0026] Preferably, when M is N, Y 1 , Y 2 , Y3 It is O, S, -OC=O or -C=O.

[0027] In a preferred embodiment, when M is B, the inhibitors include but are not limited to:

[0028]

[0029] In a preferred embodiment, when M is P, the inhibitors include but are not limited to:

[0030]

[0031] Preferably, the R 1 and R 4 H, R 2 and R 5 H, R 3 and R 6 Not H at the same time.

[0032] Preferably, the R 1 , R 2 , R 3 , R 4 , R 5 , R 6 Not H at the same time.

[0033] Furthermore, the R 1 , R 2 , R 3 , R 4 , R 5 , R 6 Independently selected from C1-C10 alkyl substituents, preferably C1-C4 alkyl substituents.

[0034] The second aspect of the present invention provides a method for applying an organic small molecule inhibitor in thin film deposition, the method comprising the following steps: firstly attaching the inhibitor to a substrate, then introducing a precursor, and depositing it on the substrate.

[0035] Furthermore, the substrate is a high aspect ratio substrate, with an aspect ratio of ≥20, preferably ≥40.

[0036] In one embodiment, the aspect ratio of the substrate is 40.

[0037] Furthermore, the opening width of the high aspect ratio substrate is ≤50nm.

[0038] Furthermore, the opening width of the high aspect ratio substrate is ≤30 nm.

[0039] Furthermore, the specific process of attaching the inhibitor to the substrate is as follows: the inhibitor is heated into gas and then flows into the deposition reaction chamber through a pipeline, the heating temperature of the inhibitor is above 30° C., and the heating temperature of the pipeline is above 50° C.

[0040] Furthermore, the inhibitor is attached to the substrate, and then an inert gas is introduced into the reaction chamber to purge excess inhibitor.

[0041] Furthermore, the precursor includes but is not limited to at least one of silicon, titanium, vanadium, tungsten, aluminum, iron, and ruthenium precursors; the silicon system means silicon precursor, germanium precursor, and tin precursor; the titanium system means titanium precursor, zirconium precursor, and hafnium precursor; the vanadium system means vanadium precursor, niobium precursor, and tantalum precursor; the tungsten system means molybdenum precursor and tungsten precursor; the iron system means iron precursor, cobalt precursor, and nickel precursor; the aluminum system means boron precursor, aluminum precursor, gallium precursor, and indium precursor.

[0042] Furthermore, selectable silicon precursors include but are not limited to at least one of tetrakis(dimethylamino)silane, tetrakis(diethylamino)silane, diisopropylaminosilane, bis(tert-butylamino)silane, bis(diethylamino)silane, bis(diisopropylamino)silane, tris(diisopropylamino)silane, dichlorosilane, silane, disilane, and tetraethyl orthosilicate; germanium precursors include but are not limited to at least one of tetrakis(dimethylamino)germanium, N,N'-diisopropyltert-pentamidinegermanium, germanium, dichlorogermane, and trichlorogermane; tin precursors include but are not limited to at least one of tin tetrachloride, tetramethyltin, and tetrakis(dimethylamino)tin.

[0043] Further, the titanium precursors that can be selected include but are not limited to at least one of tris(dimethylamino) (cyclopentadienyl) titanium, tetra(dimethylamino) titanium, tris(dimethylamino) (methylcyclopentadienyl) titanium, titanium tetrachloride, tetra(ethoxy) titanium, tetra(isobutoxy) titanium, tris(methoxy) (cyclopentadienyl) titanium, and trimethoxy (pentamethylcyclopentadienyl) titanium; the zirconium precursors include but are not limited to tris(dimethylamino) (cyclopentadienyl) zirconium, tris(dimethylamino) (cyclopentadienyl) zirconium, At least one of (dimethylamino) (methylcyclopentadienyl) zirconium, tetrakis (dimethylamino) zirconium, tetrakis (diethylamino) zirconium, tetrakis (methylethylamino) zirconium, and tris (methylethylamino) (cyclopentadienyl) zirconium; the hafnium precursor includes but is not limited to at least one of tris (dimethylamino) (cyclopentadienyl) hafnium, tris (dimethylamino) (methylcyclopentadienyl) hafnium, tris (diethylamino) (ethylcyclopentadienyl) hafnium, tetrakis (dimethylamino) hafnium, and tetrakis (methylethylamino) hafnium.

[0044] Further, the selectable vanadium precursors include but are not limited to at least one of vanadium tetrachloride, tetrakis(dimethylamino)vanadium, tetrakis(diethylamino)vanadium, tetrakis(methylethylamino)vanadium, (tri-(2,4-pentanedione)vanadium, bis(cyclopentadienyl)vanadium (II), and tetracarbonylcyclopentadienyl vanadium; the niobium precursors include but are not limited to at least one of (tert-butylimino)tris(diethylamino)niobium, (tert-butylimino)bis(dimethylamino)(cyclopentadienyl)niobium; the tantalum precursors include but are not limited to at least one of penta(diethylamino)tantalum, penta(methylethylamino)tantalum, and (tert-butylimino)tris(diethylamino)tantalum.

[0045] Furthermore, the selectable molybdenum precursors include but are not limited to at least one of hexacarbonyl molybdenum, dichloromolybdenum dioxide, molybdenum pentachloride, molybdenum hexafluoride, and bis(tert-butylimino)bis(dimethylamino)molybdenum; the tungsten precursors include but are not limited to at least one of bis(tert-butylimino)bis(dimethylamino)tungsten, tungsten hexafluoride, bis(tert-butylimino)bis(diethylamino)tungsten, and bis(tert-butylimino)bis(methylethylamino)tungsten.

[0046] Furthermore, the selectable iron precursors include but are not limited to at least one of bis(cyclopentadienyl)iron and pentacarbonyl iron; the cobalt precursors include but are not limited to at least one of (3,3-dimethyl-1-butyne) dicobalt hexacarbonyl, dicobalt octacarbonyl, and bis(N,N'-di-iso-propylacetamidine)cobalt; the nickel precursors include but are not limited to at least one of nickel acetylacetonate, bis(cyclopentadienyl)nickel, and bis(dimethylamino-2-methyl-2-butoxy)nickel.

[0047] Furthermore, the selectable ruthenium precursor includes but is not limited to at least one of bis(cyclopentadienyl)ruthenium, bis(ethylcyclopentadienyl)ruthenium, and tris(2,2,6,6-tetramethyl-3,5-heptanedione)ruthenium.

[0048] Furthermore, the selectable boron precursors include but are not limited to at least one of borane, diborane, and trimethylboron; the aluminum precursors include but are not limited to at least one of trimethylaluminum, triethylaluminum, dimethylethylaminoaluminum, trimethylaminoaluminum, N-methylpyrrolidine, triisobutylaluminum, and dimethylaluminum hydride; the gallium precursors include but are not limited to at least one of gallium chloride, trimethylgallium, and tris(dimethylamino)gallium; and the indium precursors include but are not limited to at least one of trimethylindium and cyclopentadienylindium.

[0049] Further, the type of the deposited thin film includes any one or more of an oxide film, a nitride film, an oxynitride film, and a metal film, or a group thereof.

[0050] In one embodiment, the method for applying the organic small molecule inhibitor in thin film deposition comprises the following steps:

[0051] S1: placing a high aspect ratio substrate into an atomic layer deposition device, wherein the heating temperature in the reaction chamber of the atomic layer deposition device is 100-450° C., and the reaction chamber is evacuated to 0-30 Pa;

[0052] S2: The inhibitor is placed in a source bottle, which is connected to the reaction chamber via pipeline 1. The source bottle is heated to above 30° C., pipeline 1 is heated to above 50° C., an inert gas is used as a carrier gas, and the inhibitor is introduced into the reaction chamber in a pulsed form;

[0053] S3: Introduce inert gas into the reaction chamber to purge excess inhibitor in the reaction chamber. The purge time is 2-60s.

[0054] S4: Introduce precursor into the reaction chamber

[0055] The precursor is loaded into a precursor source bottle, the precursor source bottle is connected to the reaction chamber through pipeline 2, the precursor source bottle and pipeline 2 are heated, and an inert gas is used as a carrier gas to pass the precursor into the reaction chamber in a pulsed form;

[0056] S5: Introduce inert gas into the reaction chamber to purge excess precursor and reaction by-products, the purge time is 2-60s;

[0057] S6: introducing reaction gas into the reaction chamber to generate a corresponding film;

[0058] S7: Introducing an inert gas into the reaction chamber to purge excess reaction gas and reaction by-products, the purge time being 2-60 seconds;

[0059] S8: Repeat steps S2-S7 until the thin film is deposited to a preset thickness.

[0060] Furthermore, the heating temperature of the source bottle in S2 is 30-100°C, and the heating temperature of pipeline 1 is 50-150°C.

[0061] Furthermore, the heating temperature of the precursor source bottle in S4 is 30-150°C, preferably 30-120°C; the heating temperature of pipeline 2 is 50-180°C, preferably 50-160°C.

[0062] In a preferred embodiment, the precursor is any one or more of diisopropylaminosilane, bis(tert-butylamino)silane, tris(dimethylamino)cyclopentadienyl hafnium, tris(dimethylamino)cyclopentadienyl zirconium, tetra(methylethylamino)hafnium, tetra(methylethylamino)zirconium, trimethoxy(pentamethylcyclopentadienyl)titanium, (tert-butylimino)bis(dimethylamino)(cyclopentadienyl)niobium, and (tert-butylimino)tris(diethylamino)niobium, mixed in any proportion.

[0063] Furthermore, the reaction gas includes but is not limited to O3 , O 2 , H 2 O, H 2 O 2 , O 2 Plasma, formic acid, acetic acid, acetic anhydride, NH 3 NF 3 Plasma, NO, NO 2 , organic amine, or hydrogen.

[0064] Furthermore, the inert gas in steps S2, S3, S4, S5, and S7 is N 2 , Ar, He, Kr.

[0065] Furthermore, the preset thickness of the film is 2-20 nm.

[0066] Compared with the prior art, the present invention has the following beneficial effects:

[0067] 1. The present invention provides an organic small molecule inhibitor, which has both certain steric hindrance and multi-functional group effect. Compared with the previous inhibitor molecules, the inhibitor can cover more active sites on the top of the substrate through the steric hindrance effect, and make the bottom active sites uninhibited; the inhibitor contains multiple functional groups, which increases the probability of combining with the active sites of the substrate, effectively reduces the adsorption of the precursor on the top of the substrate, is conducive to the uniform deposition of the film from top to bottom, and significantly improves the step coverage.

[0068] 2. In the structural formula of the organic small molecule inhibitor provided by the present invention, X1, X2, and X3 are all integers greater than or equal to 1 and may be unequal, thereby limiting the chain connected to the central atom to have at least one -CH 2 -, which is equivalent to stipulating the steric hindrance of the structure, and can better exert the inhibitory effect.

[0069] 3. The organic small molecule inhibitor provided by the present invention, the central atom M can be N, P or B, Y 1 , Y 2 , Y 3 is any one of O, N, S, -OC=O, -C=O, and the central atoms M and Y of this structure 1 , Y 2 , Y 3 They can all have an "affinity reaction" with the deposition substrate, thereby ensuring the adhesion of the inhibitor to the substrate.

[0070] 4. The "affinity effect" mentioned above and the appropriate steric hindrance effect expressed by the structure work together to enable the organic small molecule inhibitor provided by the present invention to fully play its role. During thin film deposition, the precursor deposition at the top of the groove is inhibited, and the precursor deposition at the bottom of the groove is minimized, thereby promoting uniform deposition of the thin film from top to bottom, thereby ensuring the groove filling of the substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0071] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0072] Figure 1 TEM and EDS images of the deposited thin film provided in Example 1 of the present invention; Figure 1 In the figure, (a) is a longitudinal image of the top deposited film of Example 1, with a scale of 100 nm; (b) is a longitudinal image of the bottom deposited film of Example 1, with a scale of 100 nm; (c) is an element distribution diagram of Hf in the film (EDS diagram), with a scale of 200 nm; (d) is a cross-sectional image of the top deposited film of Example 1, with a scale of 20 nm; (e) is a cross-sectional image of the bottom deposited film of Example 1, with a scale of 20 nm.

[0073] Figure 2 TEM and EDS images of the deposited thin film provided in Example 2 of the present invention; Figure 2 In the figure, (a) is a longitudinal image of the top deposited film of Example 2, with a scale of 100 nm; (b) is a longitudinal image of the bottom deposited film of Example 2, with a scale of 100 nm; (c) is an element distribution diagram of Hf in the film (EDS diagram), with a scale of 200 nm; (d) is a cross-sectional image of the top deposited film of Example 2, with a scale of 20 nm; (e) is a cross-sectional image of the bottom deposited film of Example 2, with a scale of 20 nm.

[0074] Figure 3 TEM and EDS images of the deposited thin film provided in Comparative Example 1 of the present invention; Figure 3 In the figure, (a) is a longitudinal image of the top deposited film of Comparative Example 1, with a scale of 100 nm; (b) is a longitudinal image of the bottom deposited film of Comparative Example 1, with a scale of 100 nm; (c) is an element distribution diagram of Hf in the film (EDS diagram), with a scale of 200 nm; (d) is a cross-sectional image of the top deposited film of Comparative Example 1, with a scale of 50 nm; (e) is a cross-sectional image of the bottom deposited film of Comparative Example 1, with a scale of 50 nm. DETAILED DESCRIPTION

[0075] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0076] An embodiment of the first aspect of the present invention provides an organic small molecule inhibitor, characterized in that the chemical structure of the organic small molecule inhibitor is as shown in formula (I):

[0077] (I);

[0078] Wherein, M is N, P or B;

[0079] X1, X2, and X3 are all integers greater than or equal to 1, and X1, X2, and X3 may be the same or different;

[0080] R 1 , R 2 , R 3 is selected from any one of H, C1-C10 aliphatic or cycloaliphatic substituents, and R 1 , R 2 , R 3 It can be the same or different;

[0081] R 4 , R 5 , R 6 to exist or not to exist;

[0082] Y 1 , Y 2 , Y 3 is any one of O, N, S, -OC=O, -C=O, and Y 1 , Y 2 , Y 3 They can be the same or different;

[0083] Among them, for R 4 , R 5 , R 6 Existence or non-existence, specifically analyzed as follows:

[0084] Case 1: When Y 1 , Y 2 , Y 3 When it is O, S, -OC=O or -C=O, then R 4 , R 5 , R 6 None exist;

[0085] Case 2: When Y 1 , Y 2 , Y 3 When both are N, then R 4 , R 5 , R 6 Both exist;

[0086] Case 3: When Y 1 N and Y 2 , Y 3 When it is O, S, -OC=O or -C=O, then R 4 Exists and R 5 , R 6 None exist;

[0087] Case 4: When Y 2 N and Y 1 , Y 3 When it is O, S, -OC=O or -C=O, then R 5 Exists and R 4 , R 6 None exist;

[0088] Case 5: When Y 3 N and Y 1 , Y 2 When it is O, S, -OC=O or -C=O, then R 6 Exists and R 4 , R 5 None exist;

[0089] Case 6: When Y 1 , Y 2 N and Y 3 When it is O, S, -OC=O or -C=O, then R 4 , R 5 Exists and R 6 does not exist;

[0090] Case 7: When Y 1 , Y 3 N and Y 2 When it is O, S, -OC=O or -C=O, then R 4 , R 6 Exists and R 5 does not exist;

[0091] Case 8: When Y 2 , Y 3 N and Y 1 When it is O, S, -OC=O or -C=O, then R 5 , R 6 Exists and R 4 does not exist;

[0092] And, when R 4 , R 5 , R 6 When present, R 4 , R 5 , R 6 are independently any one of H, C1-C10 aliphatic or cycloaliphatic substituents; wherein the C1-C10 aliphatic or cycloaliphatic substituent is any one of alkyl, cycloalkyl, alkenyl, cycloalkenyl, alkynyl, and cycloalkynyl.

[0093] The embodiment of the second aspect of the present invention provides a method for applying an organic small molecule inhibitor in thin film deposition, the method comprising the following steps:

[0094] S1: placing a high aspect ratio substrate into an atomic layer deposition device, wherein the heating temperature in the reaction chamber of the atomic layer deposition device is 100-450° C., and the reaction chamber is evacuated to 0-30 Pa;

[0095] S2: The inhibitor is placed in a stainless steel source bottle 1, which is connected to the reaction chamber via a pipeline 1. The heating temperature of the stainless steel source bottle 1 is set to 30-100°C, and the heating temperature of the pipeline 1 is set to 50-150°C. An inert gas is used as a carrier gas, and the inhibitor is introduced into the reaction chamber in a pulsed form;

[0096] S3: Introduce inert gas into the reaction chamber to purge excess inhibitor in the reaction chamber. The purge time is 2-60s.

[0097] S4: Introduce precursor into the reaction chamber

[0098] The precursor is loaded into the second stainless steel source bottle, which is connected to the reaction chamber through the second pipeline. The heating temperature of the second stainless steel source bottle is 30-150°C, and the heating temperature of the second pipeline is 50-180°C. An inert gas is used as a carrier gas to pass the precursor into the reaction chamber in a pulsed form.

[0099] In step S4, the precursor is a silicon-based precursor and / or a metal-based precursor; specifically, the precursor is diisopropylaminosilane (DIPAS), bis(tert-butylamino)silane (BTBAS), tris(dimethylamino)cyclopentadienylhafnium ([CpHf(NMe 2 ) 3 ]), tris(dimethylamino)cyclopentadienyl zirconium ([CpZr(NMe 2 ) 3 ]), tetrakis(methylethylamino)hafnium (TEMAHf), tetrakis(methylethylamino)zirconium (TEMAZr), trimethoxy(pentamethylcyclopentadienyl)titanium ([Cp*Ti(OMe) 3], referred to as Star-Ti), (tert-butylimino)bis(dimethylamino)(cyclopentadienyl)niobium ([CpNb(tBuN)(NMe 2 ) 2 ]), (tert-butylimino)tri(diethylamino)niobium (TBTDEN) and any one or more thereof are mixed in any proportion;

[0100] S5: Introduce inert gas into the reaction chamber to purge excess precursor and reaction by-products, the purge time is 2-60s;

[0101] S6: introducing reaction gas into the reaction chamber to generate a corresponding film;

[0102] S7: Introducing an inert gas into the reaction chamber to purge excess reaction gas and reaction by-products, the purge time being 2-60 seconds;

[0103] In the above steps S2, S3, S4, S5, and S7, the inert gas is N 2 , Ar, He, Kr;

[0104] S8: Repeat steps S2-S7 until the thin film is deposited to a preset thickness, wherein the preset thickness is 2-20 nm.

[0105] The following are specific examples. Unless otherwise specified, all raw materials in the following examples can be obtained from commercial sources. Example 1

[0106] This embodiment provides an organic small molecule inhibitor, which is tris[2-(dimethylamino)ethyl]amine, and its chemical structure is as follows:

[0107] .

[0108] This embodiment also provides a method for applying an organic small molecule inhibitor in thin film deposition, the method specifically comprising the following steps:

[0109] S1: Place a substrate with an aspect ratio of 40 (opening width of 20 nm) into an atomic layer deposition device. The heating temperature in the reaction chamber of the atomic layer deposition device is 350°C, and the reaction chamber is evacuated to 15 Pa.

[0110] S2: The inhibitor, i.e., tri[2-(dimethylamino)ethyl]amine, is placed in a stainless steel source bottle 1, which is connected to the reaction chamber via a pipeline 1. The heating temperature of the stainless steel source bottle 1 is set to 45°C, with a pulse of 0.5s, and the heating temperature of the pipeline 1 is set to 100°C. An inert gas is used as a carrier gas, and the inhibitor is introduced into the reaction chamber in a pulsed form;

[0111] S3: Introduce inert gas into the reaction chamber to purge excess inhibitor in the reaction chamber. The purge time is 15 seconds.

[0112] S4: Introduce the precursor, tris(dimethylamino)cyclopentadienylhafnium (CpHf) (NMe 2 ) 3 Specifically, the precursor is loaded into the second stainless steel source bottle, the second stainless steel source bottle is connected to the reaction chamber through the second pipeline, the heating temperature of the second stainless steel source bottle is 80°C, the pulse is 2s, the heating temperature of the second pipeline is 150°C, an inert gas is used as a carrier gas, and the precursor is introduced into the reaction chamber in a pulsed form;

[0113] S5: Introduce inert gas into the reaction chamber to purge excess precursor and reaction by-products. The purge time is 20 seconds.

[0114] S6: Introduce reaction gas into the reaction chamber. The reaction gas is O 3 , forming a hafnium oxide film;

[0115] S7: Introduce inert gas into the reaction chamber to purge excess oxygen source and reaction by-products, the purge time is 15 s;

[0116] In the above steps S2, S3, S4, S5 and S7, the inert gas is Ar;

[0117] S8: Repeat steps S2-S7 to 100 cyc (ie, steps S2-S7 are cycled 100 times in sequence) until the film is deposited to a preset thickness of about 6 nm. Example 2

[0118] This embodiment provides an organic small molecule inhibitor, which is 1-methoxy-N,N'-bis(methoxymethyl)methylamine, and its chemical structure is as follows:

[0119] .

[0120] This embodiment also provides a method for applying an organic small molecule inhibitor in thin film deposition, the method specifically comprising the following steps:

[0121] S1: Place a substrate with an aspect ratio of 40 (opening width of 20 nm) into an atomic layer deposition device. The heating temperature in the reaction chamber of the atomic layer deposition device is 350°C, and the reaction chamber is evacuated to 15 Pa.

[0122] S2: The inhibitor, i.e., 1-methoxy-N,N'-bis(methoxymethyl)methylamine, is placed in a stainless steel source bottle 1, which is connected to the reaction chamber via a pipeline 1. The heating temperature of the stainless steel source bottle 1 is set to 35°C, with a pulse of 0.2s, and the heating temperature of the pipeline 1 is set to 100°C. An inert gas is used as a carrier gas, and the inhibitor is introduced into the reaction chamber in a pulsed form;

[0123] S3: Introduce inert gas into the reaction chamber to purge excess inhibitor in the reaction chamber. The purge time is 15 seconds.

[0124] S4: Introduce the precursor, tris(dimethylamino)cyclopentadienylhafnium (CpHf) (NMe 2 ) 3 Specifically, the precursor is loaded into the second stainless steel source bottle, the second stainless steel source bottle is connected to the reaction chamber through the second pipeline, the heating temperature of the second stainless steel source bottle is 80°C, the pulse is 2s, the heating temperature of the second pipeline is 150°C, an inert gas is used as a carrier gas, and the precursor is introduced into the reaction chamber in a pulsed form;

[0125] S5: Introduce inert gas into the reaction chamber to purge excess precursor and reaction by-products. The purge time is 20 seconds.

[0126] S6: Introduce reaction gas into the reaction chamber. The reaction gas is O 3 , forming a hafnium oxide film;

[0127] S7: Introduce inert gas into the reaction chamber to purge excess oxygen source and reaction by-products, the purge time is 15 s;

[0128] In the above steps S2, S3, S4, S5 and S7, the inert gas is Ar;

[0129] S8: Repeat steps S2-S7 to 100 cyc (ie, steps S2-S7 are cycled 100 times in sequence) until the film is deposited to a preset thickness of about 6 nm. Example 3

[0130] This embodiment provides an organic small molecule inhibitor, which is bis(diethylaminomethyl)methoxymethylamine, and its chemical structure is as follows:

[0131] .

[0132] This embodiment also provides a method for applying an organic small molecule inhibitor in thin film deposition, the method specifically comprising the following steps:

[0133] S1: Place a substrate with an aspect ratio of 40 (opening width of 20 nm) into an atomic layer deposition device. The heating temperature in the reaction chamber of the atomic layer deposition device is 300°C, and the reaction chamber is evacuated to 15 Pa.

[0134] S2: The inhibitor is placed in a stainless steel source bottle 1, which is connected to the reaction chamber via a pipeline 1. The heating temperature of the stainless steel source bottle 1 is set to 45° C., the pulse is 0.5 s, the heating temperature of the pipeline 1 is set to 130° C., an inert gas is used as a carrier gas, and the inhibitor is introduced into the reaction chamber in a pulsed form;

[0135] S3: Introduce inert gas into the reaction chamber to purge excess inhibitor in the reaction chamber. The purge time is 15 seconds.

[0136] S4: Introduce the precursor, namely tris(dimethylamino)cyclopentadienyl zirconium CpZr(NMe 2 ) 3 Specifically, the precursor is loaded into the second stainless steel source bottle, the second stainless steel source bottle is connected to the reaction chamber through the second pipeline, the heating temperature of the second stainless steel source bottle is 90°C, the pulse is 1s, the heating temperature of the second pipeline is 150°C, an inert gas is used as a carrier gas, and the precursor is passed into the reaction chamber in a pulsed form;

[0137] S5: Introduce inert gas into the reaction chamber to purge excess precursor and reaction by-products. The purge time is 20 seconds.

[0138] S6: Introduce reaction gas into the reaction chamber. The reaction gas is O 3 , forming a zirconium oxide film;

[0139] S7: Introduce inert gas into the reaction chamber to purge excess oxygen source and reaction by-products, the purge time is 15 s;

[0140] In the above steps S2, S3, S4, S5 and S7, the inert gas is Ar;

[0141] S8: Repeat steps S2-S7 to 100 cyc (ie, steps S2-S7 are cycled 100 times in sequence) until the film is deposited to a preset thickness of about 6 nm. Example 4

[0142] This embodiment provides an organic small molecule inhibitor, which is bis(ethoxyethyl)(diethylamino)ethylamine, and its chemical structure is as follows:

[0143] .

[0144] This embodiment also provides a method for applying an organic small molecule inhibitor in thin film deposition, the method specifically comprising the following steps:

[0145] S1: Place a substrate with an aspect ratio of 40 (opening width of 20 nm) into an atomic layer deposition device. The heating temperature in the reaction chamber of the atomic layer deposition device is 300°C, and the reaction chamber is evacuated to 15 Pa.

[0146] S2: The inhibitor is placed in a stainless steel source bottle 1, which is connected to the reaction chamber via a pipeline 1. The heating temperature of the stainless steel source bottle 1 is set to 50° C., the pulse is 0.6 s, the heating temperature of the pipeline 1 is set to 130° C., an inert gas is used as a carrier gas, and the inhibitor is introduced into the reaction chamber in a pulsed form;

[0147] S3: Introduce inert gas into the reaction chamber to purge excess inhibitor in the reaction chamber. The purge time is 15 seconds.

[0148] S4: Introduce the precursor, namely tris(dimethylamino)cyclopentadienyl zirconium CpZr(NMe 2 ) 3 Specifically, the precursor is loaded into the second stainless steel source bottle, the second stainless steel source bottle is connected to the reaction chamber through the second pipeline, the heating temperature of the second stainless steel source bottle is 90°C, the pulse is 1s, the heating temperature of the second pipeline is 150°C, an inert gas is used as a carrier gas, and the precursor is passed into the reaction chamber in a pulsed form;

[0149] S5: Introduce inert gas into the reaction chamber to purge excess precursor and reaction by-products. The purge time is 20 seconds.

[0150] S6: Introduce reaction gas into the reaction chamber. The reaction gas is O 3 , forming a zirconium oxide film;

[0151] S7: Introduce an inert gas into the reaction chamber to purge excess oxygen source and reaction by-products, and the purge time is 15 seconds;

[0152] In the above steps S2, S3, S4, S5 and S7, the inert gas is Ar;

[0153] S8: Repeat steps S2-S7 to 100 cyc (ie, steps S2-S7 are cycled 100 times in sequence) until the film is deposited to a preset thickness of about 6 nm.

[0154] Comparative Example 1

[0155] No inhibitor was used in this comparative example.

[0156] The method for applying an inhibitor in thin film deposition provided in this comparative example is carried out by referring to the method for applying an organic small molecule inhibitor in thin film deposition provided in Example 1. Compared with Example 1, no inhibitor is added in this comparative example, and the rest of the operation process and operation method are the same as Example 1.

[0157] Comparative Example 2

[0158] No inhibitor was used in this comparative example.

[0159] The method for applying an inhibitor in thin film deposition provided in this comparative example is carried out by referring to the method for applying an organic small molecule inhibitor in thin film deposition provided in Example 3. Compared with Example 3, no inhibitor is added in this comparative example, and the rest of the operation process and operation method are the same as Example 3.

[0160] Comparative Example 3

[0161] The inhibitor used in this comparative example is triethylamine.

[0162] The application method of an inhibitor in thin film deposition provided in this comparative example is carried out by referring to the application method of an organic small molecule inhibitor in thin film deposition provided in Example 1. Compared with Example 1, the inhibitor in this comparative example is replaced by triethylamine by tri[2-(dimethylamino)ethyl]amine, and the rest of the operation process and operation method are the same as Example 1.

[0163] Comparative Example 4

[0164] The inhibitor used in this comparative example is methoxyamine.

[0165] The application method of an inhibitor in thin film deposition provided in this comparative example is carried out by referring to the application method of an organic small molecule inhibitor in thin film deposition provided in Example 1. Compared with Example 1, the inhibitor in this comparative example is replaced by methoxyamine by tri[2-(dimethylamino)ethyl]amine, and the rest of the operation process and operation method are the same as Example 1.

[0166] Comparative Example 5

[0167] The inhibitor used in this comparative example is N-ethyl-N-(methoxymethyl)ethylamine.

[0168] The method for applying an inhibitor in thin film deposition provided in this comparative example is carried out by referring to the method for applying an organic small molecule inhibitor in thin film deposition provided in Example 1. Compared with Example 1, the inhibitor in this comparative example is replaced by tri[2-(dimethylamino)ethyl]amine with N-ethyl-N-(methoxymethyl)ethylamine, and the rest of the operation process and operation method are the same as Example 1.

[0169] Comparative Example 6

[0170] The inhibitor used in this comparative example is bis(2-methoxyethyl)amine.

[0171] The application method of an inhibitor in thin film deposition provided in this comparative example is carried out by referring to the application method of an organic small molecule inhibitor in thin film deposition provided in Example 1. Compared with Example 1, the inhibitor in this comparative example is replaced by tri[2-(dimethylamino)ethyl]amine with bis(2-methoxyethyl)amine, and the rest of the operation process and operation method are the same as Example 1.

[0172] Comparative Example 7

[0173] The inhibitor used in this comparative example is N,N-di(methoxymethyl)ethylamine.

[0174] The method for applying an inhibitor in thin film deposition provided in this comparative example is carried out by referring to the method for applying an organic small molecule inhibitor in thin film deposition provided in Example 3. Compared with Example 3, the inhibitor in this comparative example is replaced by tri[2-(dimethylamino)ethyl]amine with N,N-di(methoxymethyl)ethylamine, and the rest of the operation process and operation method are the same as Example 3.

[0175] Comparative Example 8

[0176] The inhibitor used in this comparative example is di[2-(dimethylamino)ethyl]ethylamine.

[0177] The method for applying an inhibitor in thin film deposition provided in this comparative example is carried out by referring to the method for applying an organic small molecule inhibitor in thin film deposition provided in Example 3. Compared with Example 3, the inhibitor in this comparative example is replaced by tri[2-(dimethylamino)ethyl]amine with di[2-(dimethylamino)ethyl]ethylamine, and the rest of the operation process and operation method are the same as Example 3.

[0178] Comparative Example 9

[0179] The inhibitor used in this comparative example is [2-(dimethylamino)ethyl]diethylamine.

[0180] The method for applying an inhibitor in thin film deposition provided in this comparative example is carried out by referring to the method for applying an organic small molecule inhibitor in thin film deposition provided in Example 3. Compared with Example 3, the inhibitor in this comparative example is replaced by tri[2-(dimethylamino)ethyl]amine with [2-(dimethylamino)ethyl]diethylamine, and the rest of the operation process and operation method are the same as Example 3.

[0181] Experimental example

[0182] The film thicknesses in Examples 1-4 and Comparative Examples 1-9 were measured, and the step coverage and growth rate per cycle (GPC) were calculated. The obtained experimental data are shown in Table 1 below.

[0183] See also Figure 1-3 This experimental example also provides TEM images and EDS images of the thin films of Example 1, Example 2 and Comparative Example 1, respectively. Figure 1 , Figure 2 as well as Figure 3As shown, it can be seen from the TEM cross-section image that in Examples 1-2, due to the use of organic small molecule inhibitors, tri[2-(dimethylamino)ethyl]amine and 1-methoxy-N,N'-bis(methoxymethyl)methylamine, respectively, the uniformity of the deposition of the film from top to bottom is better, while in Comparative Example 1, since no inhibitor is added, the film deposition is non-uniform.

[0184] Table 1

[0185]

[0186] It can be seen from the data in Table 1 that, compared with Comparative Examples 1-9, in Examples 1-4, applying multi-antennary organic small molecule inhibitors to thin film deposition can significantly improve step coverage.

[0187] The present invention provides an organic small molecule inhibitor, which has both certain steric hindrance and multi-functional group effect. Compared with the previous inhibitor molecules, the inhibitor can cover more active sites on the top of the substrate through the steric hindrance effect, and make the bottom active sites uninhibited; the inhibitor contains multiple functional groups, which increases the probability of combining with the active sites of the substrate, effectively reduces the adsorption of the precursor on the top of the substrate, is conducive to the uniform deposition of the film from top to bottom, and significantly improves the step coverage.

[0188] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0189] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. An organic small molecule inhibitor, characterized in that: The chemical structure of the organic small molecule inhibitor is shown in formula (III) or (IV): (Ⅲ); (IV)。 2. A method for using the organic small molecule inhibitor according to claim 1 in thin film deposition, characterized in that: The method comprises the following steps: firstly attaching an inhibitor to a substrate, then introducing a precursor and depositing it on the substrate; Wherein, the substrate is a high aspect ratio substrate; The specific process of attaching the inhibitor to the substrate is as follows: the inhibitor is heated into gas and then flows into the deposition reaction chamber through a pipeline, and the heating temperature of the inhibitor is above 30°C.

3. The method for applying an organic small molecule inhibitor in thin film deposition according to claim 2, characterized in that: The method comprises the following steps: S1: placing a high aspect ratio substrate into an atomic layer deposition device, wherein the heating temperature in the reaction chamber of the atomic layer deposition device is 100-450° C., and the reaction chamber is evacuated to 0-30 Pa; S2: The inhibitor is placed in a source bottle, which is connected to the reaction chamber via pipeline 1. The source bottle is heated to above 30° C., pipeline 1 is heated to above 50° C., an inert gas is used as a carrier gas, and the inhibitor is introduced into the reaction chamber in a pulsed form; S3: Introduce inert gas into the reaction chamber to purge excess inhibitor in the reaction chamber. The purge time is 2-60s. S4: Introduce precursor into the reaction chamber The precursor is loaded into a precursor source bottle, the precursor source bottle is connected to the reaction chamber through pipeline 2, the precursor source bottle and pipeline 2 are heated, and an inert gas is used as a carrier gas to pass the precursor into the reaction chamber in a pulsed form; S5: Introduce inert gas into the reaction chamber to purge excess precursor and reaction by-products, the purge time is 2-60s; S6: introducing reaction gas into the reaction chamber to generate a corresponding film; S7: Introducing an inert gas into the reaction chamber to purge excess reaction gas and reaction by-products, the purge time being 2-60 seconds; S8: Repeat steps S2-S7 until the thin film is deposited to a preset thickness.

4. The method for applying an organic small molecule inhibitor in thin film deposition according to claim 2, characterized in that: The precursor includes at least one of silicon, titanium, vanadium, tungsten, aluminum, iron, and ruthenium precursors; the silicon series refers to silicon precursors, germanium precursors, and tin precursors; the titanium series refers to titanium precursors, zirconium precursors, and hafnium precursors; the vanadium series refers to vanadium precursors, niobium precursors, and tantalum precursors; the tungsten series refers to molybdenum precursors and tungsten precursors; the iron series refers to iron precursors, cobalt precursors, and nickel precursors; the aluminum series refers to boron precursors, aluminum precursors, gallium precursors, and indium precursors.

Citation Information

Patent Citations

  • Method of improving step coverage using an inhibitor molecule for high aspect ratio structures

    US20220119939A1

  • Lithium precursor for deposition of lithium-containing layers, islands or clusters

    CN114641593A

  • Method for deposition of high aspect ratio structures using inhibitor molecules

    CN116508134A

  • Small organic molecule inhibitor and application method thereof in thin film deposition

    CN118291951A

  • Nonconformal oxide film deposition using carbon-containing inhibitor

    WO2023205570A1