A highly dispersed magnesium-based flame retardant and preparation method thereof

By preparing a highly dispersible magnesium-based flame retardant, the problem of poor dispersion in polymers is solved, and its flame retardant performance in polypropylene composite materials is significantly improved, achieving high dispersion and good flame retardant effects. .

CN118496564BActive Publication Date: 2024-11-19YANTAI AIFEL FLAME RETARDANT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410968581.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-19
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

Magnesium hydroxide as an additive flame retardant has poor dispersion in the polymer, resulting in poor compatibility with the polymer, and a large amount of additives is required to achieve the expected flame retardant effect, affecting the performance of the material.

Method used

By preparing solutions, preparing magnesium hydroxide, ultrasonic treatment, wet grinding and drying, a high dispersion magnesium-based flame retardant is prepared, and a silane coupling agent and surfactant are used to improve the dispersion of magnesium hydroxide and improve its polymerization. Compatibility in objects.

Benefits of technology

The preparation of high dispersible magnesium-based flame retardant was achieved, which significantly improved its flame retardant performance in polypropylene composite materials, with activation index reaching 97.5% to 98.5%, settlement mass fraction of 89% to 90%, and in polypropylene The flame retardant performance is significantly improved in composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention discloses a highly dispersed magnesium-based flame retardant and a preparation method thereof, and relates to the technical field of flame retardants. The preparation method of the highly dispersed magnesium-based flame retardant comprises the following steps: preparing a solution, preparing magnesium hydroxide, ultrasonic treatment, wet grinding, and drying. The highly dispersed magnesium-based flame retardant prepared by the preparation method of the highly dispersed magnesium-based flame retardant of the present invention has good hydrophobicity and lipophilicity, high dispersibility, and in the flame retardant application of the highly dispersed magnesium-based flame retardant to polymers, the addition ratio of the highly dispersed magnesium-based flame retardant is 25% to 45% of the total mass to obtain the expected flame retardant effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flame retardants, in particular to a highly dispersed magnesium-based flame retardant and a preparation method thereof. Background Art

[0002] Flame retardants are additives that can improve the fire resistance of flammable or combustible materials, making them difficult to ignite, self-extinguishing after ignition, or increasing the ignition time, thereby inhibiting or slowing down the spread of fire. Flame retardants are widely used in plastics, textiles, coatings, electronic equipment, automotive interiors, building materials and other fields, and the market consumption is very large.

[0003] As society pays more and more attention to environmental protection and human health, halogen-free, low-smoke, non-toxic flame retardants have become the focus of research and development. As a green and environmentally friendly inorganic flame retardant, magnesium hydroxide shows broad development prospects due to its excellent flame retardant efficiency and environmental friendliness. As an additive flame retardant, magnesium hydroxide decomposes when heated, absorbs the heat on the surface of the burning material and plays a flame retardant role; at the same time, it releases a large amount of water to dilute the oxygen and combustible gas on the surface of the burning material, reducing the combustion rate. In addition, the magnesium oxide produced by the decomposition of magnesium hydroxide forms a protective layer on the surface of the material, which can isolate oxygen and prevent further combustion of the material, while also reducing the smoke generated by combustion.

[0004] Although magnesium hydroxide has a significant flame retardant effect, when used alone, it usually requires a large amount of addition to achieve the desired flame retardant effect, which will cause serious degradation of the performance of polymer materials; and due to the hydrophilic and oleophobic surface properties of magnesium hydroxide, it has poor dispersibility when applied to polymers and is difficult to be evenly dispersed in the polymer, resulting in poor compatibility with the polymer. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a highly dispersed magnesium-based flame retardant and a preparation method thereof.

[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0007] A highly dispersed magnesium-based flame retardant and a preparation method thereof, comprising the following steps: preparing a solution, preparing magnesium hydroxide, ultrasonic treatment, wet grinding, and drying.

[0008] The method for preparing the solution is to dissolve magnesium chloride in water to form a magnesium chloride aqueous solution with a concentration of 2 mol / L; dissolve sodium hydroxide in water to form a sodium hydroxide aqueous solution with a concentration of 4 mol / L; and dissolve urea in water to form a urea aqueous solution with a concentration of 2 mol / L.

[0009] The preparation method of magnesium hydroxide comprises the following steps: using a liquid pump to simultaneously add the prepared magnesium chloride aqueous solution, sodium hydroxide aqueous solution and urea aqueous solution into a reactor with a stirring speed of 90 to 100 rpm, controlling the temperature in the reactor at 80° C. to 90° C., and after the magnesium chloride aqueous solution, sodium hydroxide aqueous solution and urea aqueous solution are completely added into the reactor, stirring is continued for 60 minutes at a stirring speed of 90 to 100 rpm, and magnesium hydroxide slurry is obtained after the reaction is completed; transferring the magnesium hydroxide slurry into an aging device, standing for 3 to 6 hours, filtering and washing the filter cake with water to wash away water-soluble impurities in the filter cake, collecting the filter cake, and obtaining a magnesium hydroxide filter cake; and randomly selecting 5 portions of 1 to 5 g of magnesium hydroxide filter cake for water content determination, and calculating the weight of the magnesium hydroxide filter cake material.

[0010] The volume ratio of the magnesium chloride aqueous solution, the sodium hydroxide aqueous solution and the urea aqueous solution is 1:0.6 to 1:0.25 to 0.8.

[0011] The ultrasonic treatment method is to mix the magnesium hydroxide filter cake, water and a silane coupling agent by weight and then perform ultrasonic treatment for 60 minutes to obtain a magnesium hydroxide dispersion.

[0012] The ultrasonic treatment has an ultrasonic frequency of 30 kHz and an ultrasonic power of 1500 W.

[0013] The water accounts for 80% to 90% of the mass of the magnesium hydroxide filter cake.

[0014] The silane coupling agent accounts for 2% by weight of the magnesium hydroxide filter biscuit material.

[0015] The silane coupling agent is a silane coupling agent, specifically at least one of γ-aminopropyl triethoxysilane, γ-glycidyloxypropyl trimethoxysilane, γ-(methacryloyloxy)propyl trimethoxysilane, N-(β-aminoethoxy)-γ-aminopropyl trimethyl(ethyl)oxysilane, N-β-(aminoethoxy)-γ-aminopropyl methyldimethoxysilane, γ-(2,3-epoxypropyloxy)propyl trimethoxysilane, vinyl trimethoxysilane and vinyl triacetoxysilane.

[0016] The wet grinding method is to put the magnesium hydroxide dispersion, grinding aid, surfactant and grinding balls into a ball mill for wet grinding for 30 to 60 minutes. After the grinding is completed, sampling is performed to measure the particle size of the grinding product.

[0017] The material of the grinding spheres is zirconia spheres, with zirconia spheres with a diameter of 2 mm accounting for 40-50wt%, and zirconia spheres with a diameter of 3 mm accounting for 50-60wt%; the grinding temperature is controlled at 50°C to 70°C, and the grinding speed is 800-1200r / min. During wet grinding, the filling rate of the grinding spheres in the ball mill is 60% to 70%, and the remaining gaps in the ball mill are filled with a magnesium hydroxide mixture consisting of a magnesium hydroxide dispersion, a grinding aid, and a surfactant.

[0018] The surfactant is 4% to 6% by weight of the magnesium hydroxide filter biscuit material.

[0019] The grinding aid is 1% to 2% by weight of the magnesium hydroxide filter biscuit material.

[0020] The surfactant is selected from one or more of stearic acid, sodium stearate, zinc stearate, calcium stearate and magnesium stearate.

[0021] The grinding aid is polyethylene glycol with a molecular weight of 6000.

[0022] The drying method comprises: filtering the ground product to a moisture content of 20% to 30%, collecting the ground product material cake, and flash drying the material at 140° C. to 160° C. until the material moisture content is ≤0.5wt%, thereby obtaining a highly dispersed magnesium-based flame retardant.

[0023] The present invention provides a highly dispersed magnesium-based flame retardant having the following beneficial effects:

[0024] 1. The process flow of the method of the present invention is simple, the amount of surfactant used is small, the cost is low, and it is conducive to large-scale product production.

[0025] 2. The activation index of the highly dispersed magnesium-based flame retardant prepared by the present invention is 97.5% to 98.5%, indicating that 97.5% to 98.5% of the surfaces of the highly dispersed magnesium-based flame retardant are hydrophobic and lipophilic, and the sedimentation mass fraction of the highly dispersed magnesium-based flame retardant is 89% to 90%, which means that after 12 hours, 89% to 90% of the highly dispersed magnesium-based flame retardant is still suspended in the liquid paraffin without sedimentation, indicating that the highly dispersed magnesium-based flame retardant has high dispersibility.

[0026] 3. The highly dispersed magnesium-based flame retardant prepared by the method of the present invention is mixed with polypropylene to obtain a polypropylene composite flame retardant material. When the highly dispersed magnesium-based flame retardant accounts for 25.0wt%, the limiting oxygen index is 36.6%.

[0027] When the highly dispersed magnesium-based flame retardant accounts for 30.0wt%, the limiting oxygen index is 37.9%, compared with the limiting oxygen index of pure polyethylene of 19.4%. The flame retardant properties of the polypropylene composite flame retardant material made by adding highly dispersed magnesium-based flame retardant are significantly improved. DETAILED DESCRIPTION

[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] A preparation method of a highly dispersed magnesium-based flame retardant comprises the following steps:

[0031] Prepare the solution: Use magnesium chloride hexahydrate and water to prepare a magnesium chloride solution with a concentration of 2.0 mol / L for standby use; use sodium hydroxide flakes and water to prepare a sodium hydroxide solution with a concentration of 4.0 mol / L for standby use; use urea and water to prepare a urea solution with a concentration of 2.0 mol / L for standby use. The volume ratio of the prepared magnesium chloride aqueous solution, sodium hydroxide aqueous solution, and urea aqueous solution is 1:1:0.25.

[0032] Preparation of magnesium hydroxide: Using a liquid pump, the prepared magnesium chloride aqueous solution and sodium hydroxide aqueous solution are simultaneously added to a reactor with a stirring speed set to 90 rpm at a flow rate of 400 ml / min and a urea aqueous solution at a flow rate of 100 ml / min. The temperature in the reactor is controlled at 70°C. After the magnesium chloride aqueous solution, sodium hydroxide aqueous solution and urea aqueous solution are completely added to the reactor, stirring is continued for 60 min at a stirring speed of 90 rpm. After the reaction is completed, a magnesium hydroxide slurry is obtained. The obtained magnesium hydroxide slurry is transferred to an aging device, and after standing for 3 hours, the filter cake is filtered and washed with water to wash away water-soluble impurities in the filter cake. The filter cake is collected to obtain a magnesium hydroxide filter cake, and 5 portions of 2 g of the magnesium hydroxide filter cake are randomly selected for moisture content determination, and the weight of the magnesium hydroxide filter cake material is calculated.

[0033] Ultrasonic treatment: the magnesium hydroxide filter cake, water and silane coupling agent are mixed and then ultrasonically treated for 60 minutes to obtain a magnesium hydroxide dispersion, wherein water accounts for 90% of the mass of the magnesium hydroxide filter cake material, the silane coupling agent is γ-aminopropyltriethoxysilane, and γ-aminopropyltriethoxysilane accounts for 2% of the mass of the magnesium hydroxide filter cake material. The ultrasonic frequency of the ultrasonic treatment is 30kHz, and the ultrasonic power is 1500W.

[0034] Wet grinding: Put magnesium hydroxide dispersion, grinding aid, surfactant, and grinding sphere into a ball mill for wet grinding. The grinding time is 60 minutes. After grinding, the grinding product is obtained, and the particle size of the grinding product is measured by sampling. The surfactant is 4% of the weight of the magnesium oxide filter biscuit material, and the surfactant is composed of the following raw materials in weight percentage: 40wt% zinc stearate and 60wt% magnesium stearate; the grinding aid accounts for 1% to 2% of the weight of the magnesium hydroxide filter biscuit material, and the grinding aid is polyethylene glycol with a molecular weight of 6000. The material of the grinding sphere is zirconium oxide sphere, and the diameter of 2mm zirconium oxide sphere accounts for 40wt%, and the diameter of 3mm zirconium oxide sphere accounts for 60wt%; the grinding temperature is controlled at 50℃, and the grinding speed is 800r / min. In wet grinding, the filling rate of the grinding sphere in the ball mill is 70%, and the remaining gaps in the ball mill are filled with a magnesium hydroxide mixture composed of magnesium hydroxide dispersion, grinding aid, and surfactant.

[0035] Drying: filter press the ground product until the water content is 20% to 30%, collect the filter cake of the ground product, and flash dry it at 140°C to 160°C until the moisture content of the material is ≤0.5wt%, to obtain a highly dispersed magnesium-based flame retardant.

[0036] Example 2

[0037] A preparation method of a highly dispersed magnesium-based flame retardant comprises the following steps:

[0038] Prepare the solution: Use magnesium chloride hexahydrate and water to prepare a magnesium chloride solution with a concentration of 2.0 mol / L for standby use; use sodium hydroxide flakes and water to prepare a sodium hydroxide solution with a concentration of 4 mol / L for standby use; use urea and water to prepare a urea solution with a concentration of 2.0 mol / L for standby use. The volume ratio of the prepared magnesium chloride aqueous solution, sodium hydroxide aqueous solution, and urea aqueous solution is 1:0.8:0.4.

[0039] Preparation of magnesium hydroxide: Using a liquid pump, the prepared magnesium chloride aqueous solution at a flow rate of 400 ml / min, the sodium hydroxide aqueous solution at a flow rate of 320 ml / min, and the urea aqueous solution at a flow rate of 160 ml / min are simultaneously added into a reactor with a stirring speed set to 100 rpm, and the temperature in the reactor is controlled at 70°C. After the magnesium chloride aqueous solution, the sodium hydroxide aqueous solution, and the urea aqueous solution are completely added to the reactor, stirring is continued for 60 min at a stirring speed of 100 rpm. After the reaction is completed, a magnesium hydroxide slurry is obtained, and the obtained magnesium hydroxide slurry is transferred to an aging device. After standing for 4 hours, the filter and the filter cake are washed with water to wash away water-soluble impurities in the filter cake, and the filter cake is collected to obtain a magnesium hydroxide filter cake, and 5 portions of 2 g of the magnesium hydroxide filter cake are randomly selected for moisture content determination, and the weight of the magnesium hydroxide filter cake material is calculated.

[0040] Ultrasonic treatment: the magnesium hydroxide filter cake, water and silane coupling agent are mixed and then ultrasonically treated for 60 minutes to obtain a magnesium hydroxide dispersion, wherein water accounts for 80% of the mass of the magnesium hydroxide filter cake material, the silane coupling agent is γ-glycidyloxypropyltrimethoxysilane, and γ-glycidyloxypropyltrimethoxysilane accounts for 2% of the mass of the magnesium hydroxide filter cake material. The ultrasonic frequency of the ultrasonic treatment is 30kHz, and the ultrasonic power is 1500W.

[0041] Wet grinding: Put magnesium hydroxide dispersion, grinding aid, surfactant, and grinding sphere into a ball mill for wet grinding. The grinding time is 60 minutes. After grinding, the grinding product is obtained, and the particle size of the grinding product is measured by sampling. The surfactant is 4% of the weight of the magnesium oxide filter biscuit material, and the surfactant is composed of the following raw materials in weight percentage: 50wt% zinc stearate and 50wt% stearic acid; the grinding aid accounts for 1% of the weight of the magnesium hydroxide filter biscuit material, and the grinding aid is polyethylene glycol with a molecular weight of 6000. The material of the grinding sphere is zirconium oxide sphere, and the diameter of 2mm zirconium oxide sphere accounts for 50wt%, and the diameter of 3mm zirconium oxide sphere accounts for 50wt%; the grinding temperature is controlled at 60℃, and the grinding speed is 1000r / min. In wet grinding, the filling rate of the grinding sphere in the ball mill is 70%, and the remaining gaps in the ball mill are filled with a magnesium hydroxide mixture composed of magnesium hydroxide dispersion, grinding aid, and surfactant.

[0042] Drying: filter press the ground product until the water content is 20% to 30%, collect the filter cake of the ground product, and flash dry it at 140°C to 160°C until the moisture content of the material is ≤0.5wt%, to obtain a highly dispersed magnesium-based flame retardant.

[0043] Example 3

[0044] A preparation method of a highly dispersed magnesium-based flame retardant comprises the following steps:

[0045] Prepare the solution: Use magnesium chloride hexahydrate and water to prepare a magnesium chloride solution with a concentration of 2.0 mol / L for standby use; use sodium hydroxide flakes and water to prepare a sodium hydroxide solution with a concentration of 4 mol / L for standby use; use urea and water to prepare a urea solution with a concentration of 2.0 mol / L for standby use. The volume ratio of the prepared magnesium chloride aqueous solution, sodium hydroxide aqueous solution, and urea aqueous solution is 1:0.6:0.8.

[0046] Preparation of magnesium hydroxide: Using a liquid pump, the prepared magnesium chloride aqueous solution at a flow rate of 400 ml / min, the sodium hydroxide aqueous solution at a flow rate of 240 ml / min, and the urea aqueous solution at a flow rate of 320 ml / min are simultaneously added to a reactor with a stirring speed set to 100 rpm, and the temperature in the reactor is controlled at 80° C. After the magnesium chloride aqueous solution, the sodium hydroxide aqueous solution, and the urea aqueous solution are completely added to the reactor, stirring is continued for 60 min at a stirring speed of 100 rpm. After the reaction is completed, a magnesium hydroxide slurry is obtained, and the obtained magnesium hydroxide slurry is transferred to an aging device. After standing for 5 hours, the filter and the filter cake are washed with water to wash away water-soluble impurities in the filter cake, and the filter cake is collected to obtain a magnesium hydroxide filter cake, and 5 portions of 2 g of the magnesium hydroxide filter cake are randomly selected for moisture content determination, and the weight of the magnesium hydroxide filter cake material is calculated.

[0047] Ultrasonic treatment: the magnesium hydroxide filter cake, water and silane coupling agent are mixed and ultrasonically treated for 60 minutes to obtain a magnesium hydroxide dispersion, wherein water accounts for 80% of the mass of the magnesium hydroxide filter cake material, the silane coupling agent is γ-(methacryloyloxy)propyltrimethoxysilane, and γ-(methacryloyloxy)propyltrimethoxysilane accounts for 2% of the mass of the magnesium hydroxide filter cake material. The ultrasonic frequency of the ultrasonic treatment is 30kHz, and the ultrasonic power is 1500W.

[0048] Wet grinding: Put magnesium hydroxide dispersion, grinding aid, surfactant, and grinding sphere into a ball mill for wet grinding. The grinding time is 60 minutes. After grinding, the grinding product is obtained, and the particle size of the grinding product is measured by sampling. The surfactant is 5% of the weight of the magnesium oxide filter biscuit material, and the surfactant is composed of the following raw materials in weight percentage: 50wt% magnesium stearate and 50wt% stearic acid; the grinding aid accounts for 1% of the weight of the magnesium hydroxide filter biscuit material, and the grinding aid is polyethylene glycol with a molecular weight of 6000. The material of the grinding sphere is zirconium oxide sphere, and the diameter of 2mm zirconium oxide sphere accounts for 40wt%, and the diameter of 3mm zirconium oxide sphere accounts for 60wt%; the grinding temperature is controlled at 60℃, and the grinding speed is 1200r / min. In wet grinding, the filling rate of the grinding sphere in the ball mill is 70%, and the remaining gaps in the ball mill are filled with a magnesium hydroxide mixture composed of magnesium hydroxide dispersion, grinding aid, and surfactant.

[0049] Drying: filter press the ground product until the water content is 20% to 30%, collect the filter cake of the ground product, and flash dry it at 140°C to 160°C until the moisture content of the material is ≤0.5wt%, to obtain a highly dispersed magnesium-based flame retardant.

[0050] Example 4

[0051] A preparation method of a highly dispersed magnesium-based flame retardant comprises the following steps:

[0052] Prepare the solution: Use magnesium chloride hexahydrate and water to prepare a magnesium chloride solution with a concentration of 2.0 mol / L for standby use; use sodium hydroxide flakes and water to prepare a sodium hydroxide solution with a concentration of 4 mol / L for standby use; use urea and water to prepare a urea solution with a concentration of 2.0 mol / L for standby use. The volume ratio of the prepared magnesium chloride aqueous solution, sodium hydroxide aqueous solution, and urea aqueous solution is 1:0.8:0.4.

[0053] Preparation of magnesium hydroxide: Using a liquid pump, the prepared magnesium chloride aqueous solution at a flow rate of 400 ml / min, the sodium hydroxide aqueous solution at a flow rate of 320 ml / min, and the urea aqueous solution at a flow rate of 160 ml / min are simultaneously added to a reactor with a stirring speed set to 100 rpm, and the temperature in the reactor is controlled at 80° C. After the magnesium chloride aqueous solution, the sodium hydroxide aqueous solution, and the urea aqueous solution are completely added to the reactor, stirring is continued for 60 min at a stirring speed of 100 rpm. After the reaction is completed, a magnesium hydroxide slurry is obtained, and the obtained magnesium hydroxide slurry is transferred to an aging device. After standing for 5 hours, the filter and the filter cake are washed with water to wash away water-soluble impurities in the filter cake, and the filter cake is collected to obtain a magnesium hydroxide filter cake, and 5 portions of 2 g of the magnesium hydroxide filter cake are randomly selected for moisture content determination, and the weight of the magnesium hydroxide filter cake material is calculated.

[0054] Ultrasonic treatment: the magnesium hydroxide filter cake, water and silane coupling agent are mixed and then ultrasonically treated for 60 minutes to obtain a magnesium hydroxide dispersion, wherein water accounts for 80% of the mass of the magnesium hydroxide filter cake material, the silane coupling agent is vinyl triacetoxysilane, and vinyl triacetoxysilane accounts for 2% of the mass of the magnesium hydroxide filter cake material. The ultrasonic frequency of the ultrasonic treatment is 30kHz, and the ultrasonic power is 1500W.

[0055] Wet grinding: Put magnesium hydroxide dispersion, grinding aid, surfactant, and grinding spheres into a ball mill for wet grinding. The grinding time is 60 minutes. After grinding, the grinding product is obtained, and the particle size of the grinding product is measured by sampling. The surfactant is 6% of the weight of the magnesium oxide filter biscuit material, and the surfactant is composed of the following raw materials in weight percentage: magnesium stearate 60wt%, stearic acid 40wt%; the grinding aid accounts for 1% of the weight of the magnesium hydroxide filter biscuit material, and the grinding aid is polyethylene glycol with a molecular weight of 6000. The material of the grinding sphere is zirconium oxide sphere, and the diameter of 2mm zirconium oxide sphere accounts for 50wt%, and the diameter of 3mm zirconium oxide sphere accounts for 50wt%; the grinding temperature is controlled at 60℃, and the grinding speed is 1200r / min. In wet grinding, the filling rate of the grinding sphere in the ball mill is 70%, and the remaining gaps in the ball mill are filled with a magnesium hydroxide mixture composed of magnesium hydroxide dispersion, grinding aid, and surfactant.

[0056] Drying: filter press the ground product until the water content is 20% to 30%, collect the filter cake of the ground product, and flash dry it at 140°C to 160°C until the moisture content of the material is ≤0.5wt%, to obtain a highly dispersed magnesium-based flame retardant.

[0057] Performance test of highly dispersed magnesium-based flame retardant:

[0058] Activity index test: weigh a highly dispersed magnesium-based flame retardant, recorded as W1, add it into deionized water with a volume five times that of W1, stir it at a uniform speed, let it stand for 10 hours, filter the floating powder, drain it, dry it and weigh it as W2, activity index = W2 / W1.

[0059] Sedimentation test: 1.00 g of highly dispersed magnesium-based flame retardant was placed in a 25 mL stoppered measuring cylinder, liquid paraffin was added to the scale, and then ultrasonically vibrated for 20 minutes, shaken and allowed to stand, and the volume of the suspension of modified magnesium hydroxide flame retardant in liquid paraffin was read at 12 hours and recorded as V. Sedimentation mass fraction (%) of highly dispersed magnesium-based flame retardant = V / 25×100%.

[0060] The performance parameters of the highly dispersed magnesium-based flame retardants prepared in specific examples 1 to 4 are shown in Table 1:

[0061] Table 1 Performance parameters of highly dispersed magnesium-based flame retardants prepared in various embodiments

[0062]

[0063] Application Example 1

[0064] The highly dispersed magnesium-based flame retardant and polypropylene (PP) prepared in the above Example 4 were melt-blended at 180° C. for 15 minutes, and then pressed and cooled to obtain a polypropylene composite flame retardant material; the highly dispersed magnesium-based flame retardant accounted for 25.0 wt % in the blend.

[0065] Application Example 2

[0066] The highly dispersed magnesium-based flame retardant and polypropylene (PP) prepared in the above Example 4 were melt-blended at 180° C. for 15 minutes, and then pressed and cooled to obtain a polypropylene composite flame retardant material; the highly dispersed magnesium-based flame retardant accounted for 30.0 wt % in the blend.

[0067] Application Example 3

[0068] The highly dispersed magnesium-based flame retardant and polypropylene (PP) prepared in the above Example 4 were melt-blended at 180° C. for 15 minutes, and then pressed and cooled to obtain a polypropylene composite flame retardant material; the highly dispersed magnesium-based flame retardant accounted for 35.0 wt % in the blend.

[0069] Application Example 4

[0070] The highly dispersed magnesium-based flame retardant and polypropylene (PP) prepared in the above Example 4 were melt-blended at 180° C. for 15 minutes, and then pressed and cooled to obtain a polypropylene composite flame retardant material; the highly dispersed magnesium-based flame retardant accounted for 40.0 wt % in the blend.

[0071] Application Example 5

[0072] The highly dispersed magnesium-based flame retardant and polypropylene (PP) prepared in the above Example 4 were melt-blended at 180° C. for 15 minutes, and then pressed and cooled to obtain a polypropylene composite flame retardant material; the highly dispersed magnesium-based flame retardant accounted for 45.0 wt % in the blend.

[0073] The polypropylene composite flame retardant material prepared in Application Examples 1-5 was cut into standard specimens of 130 mm × 13 mm × 3 mm and 130 mm × 6.5 mm × 3 mm, and subjected to UL-94 vertical combustion test on a CZF-3 horizontal combustion tester according to ASTM D635-77 standard; the limiting oxygen index was tested on an HC-2 oxygen index instrument according to ASTM D2863-77 standard; and its physical properties were tested according to Chinese national standards. The specific results are shown in Table 2:

[0074] Table 2 Test results of polypropylene composite flame retardant materials and polypropylene physical properties made from various application examples

[0075]

[0076] It can be seen from the data in Table 2 that the polypropylene composite flame retardant material prepared by adding highly dispersed magnesium-based flame retardant in Application Examples 1-5 has good flame retardancy, and the flame retardancy reaches UL-94V-0 level, the dispersed magnesium-based flame retardant accounts for 25.0wt%, and the limiting oxygen index can reach 36.6%. In addition, the smoke and dripping of the polypropylene composite flame retardant material prepared by adding highly dispersed magnesium-based flame retardant are significantly improved when compared with the combustion of pure polyethylene. The mechanical properties of the polypropylene composite flame retardant material prepared by adding highly dispersed magnesium-based flame retardant are compared with the mechanical properties of polypropylene, among which the tensile strength and elongation at break are reduced, but the impact is small; the flexural strength and flexural modulus are enhanced.

[0077] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a highly dispersed magnesium-based flame retardant, It is characterized in that The following steps are involved: Solution preparation, magnesium hydroxide preparation, ultrasonic treatment, wet grinding, and drying; S1. The method for preparing the solution is to dissolve magnesium chloride in water to form a magnesium chloride aqueous solution with a concentration of 2 mol / L; dissolve sodium hydroxide in water to form a sodium hydroxide aqueous solution with a concentration of 4 mol / L; and dissolve urea in water to form a urea aqueous solution with a concentration of 2 mol / L; S2, the preparation method of magnesium hydroxide is: using a liquid pump to add the magnesium chloride aqueous solution, sodium hydroxide aqueous solution and urea aqueous solution prepared in step S1 to a reactor with a stirring speed of 90-100rpm at the same time, the temperature in the reactor is controlled at 60°C-80°C, after the magnesium chloride aqueous solution, sodium hydroxide aqueous solution and urea aqueous solution prepared in step S1 are completely added to the reactor, stirring is continued for 60-70min, the stirring speed is 90-100rpm, and magnesium hydroxide slurry is obtained after the reaction is completed; the magnesium hydroxide slurry is transferred to an aging device, after standing for 3-6h, the filter cake is filtered and washed with water to wash away water-soluble impurities in the filter cake, and the filter cake is collected to obtain a magnesium hydroxide filter cake; 5 portions of 1-5g of magnesium hydroxide filter cake are randomly selected for moisture content determination, and the weight of the magnesium hydroxide filter cake material is calculated; S3, the method of ultrasonic treatment is: mixing the magnesium hydroxide filter cake, water and silane coupling agent by weight and then ultrasonically treating for 60 minutes to obtain a magnesium hydroxide dispersion; S4, the wet grinding method is, the magnesium hydroxide dispersion, grinding aid, surfactant, grinding spheres into a ball mill for wet grinding, the grinding time is 60min; S5. The drying method is to filter the grinding product to a moisture content of 20% to 30%, collect the grinding product material cake, perform flash drying treatment, flash dry at 140°C to 160°C to a material moisture content of ≤0.5wt%, and obtain a highly dispersed magnesium-based flame retardant. The polypropylene composite flame retardant material prepared by the highly dispersed magnesium-based flame retardant and polypropylene (PP) has a limiting oxygen index of 36.6% when the highly dispersed magnesium-based flame retardant accounts for 25.0wt%, a limiting oxygen index of 37.9% when the highly dispersed magnesium-based flame retardant accounts for 30.0wt%, and a limiting oxygen index of 41.5% when the highly dispersed magnesium-based flame retardant accounts for 40.0wt%; the highly dispersed magnesium-based flame retardant The activity index is 97.6% to 98.2%, the sedimentation mass fraction of the highly dispersed magnesium-based flame retardant is 89% to 91%, and the polypropylene composite flame retardant material prepared by adding the highly dispersed magnesium-based flame retardant has good flame retardancy, and the flame retardant performance reaches UL-94V-0 level; in addition, the smoke and dripping conditions of the polypropylene composite flame retardant material prepared by adding the highly dispersed magnesium-based flame retardant are significantly improved when compared with the combustion of pure polyethylene. The mechanical properties of the polypropylene composite flame retardant material prepared by adding the highly dispersed magnesium-based flame retardant are compared with the mechanical properties of polypropylene, among which the tensile strength and elongation at break are reduced, but the impact is small; the flexural strength and flexural modulus are enhanced.

2. A method for preparing a highly dispersed magnesium-based flame retardant according to claim 1, Features: The volume ratio of the magnesium chloride aqueous solution, the sodium hydroxide aqueous solution and the urea aqueous solution is 1:0.6 to 1:0.25 to 0.

8.

3. A method for preparing a highly dispersed magnesium-based flame retardant according to claim 1, Features: In the step S3, the water accounts for 80% to 90% of the weight of the magnesium hydroxide filter biscuit material; and the silane coupling agent accounts for 2% of the weight of the magnesium hydroxide filter biscuit material.

4. The method for preparing a highly dispersed magnesium-based flame retardant according to claim 1, Features: The silane coupling agent is at least one of γ-aminopropyl triethoxysilane, γ-glycidyloxypropyl trimethoxysilane, γ-(methacryloyloxy)propyl trimethoxysilane, N-(β-aminoethoxy)-γ-aminopropyl trimethyl(ethyl)oxysilane, N-β-(aminoethoxy)-γ-aminopropyl methyldimethoxysilane, γ-(2,3-epoxypropyloxy)propyl trimethoxysilane, vinyl trimethoxysilane and vinyl triacetoxysilane.

5. The method for preparing a highly dispersed magnesium-based flame retardant according to claim 1, Features: The material of the grinding spheres is zirconia spheres, with zirconia spheres with a diameter of 2 mm accounting for 40-50wt%, and zirconia spheres with a diameter of 3 mm accounting for 50-60wt%; the grinding temperature is controlled at 50°C-70°C, and the grinding speed is 800-1200r / min. During wet grinding, the filling rate of the grinding spheres in the ball mill is 60%-70%, and the remaining gaps in the ball mill are filled with a magnesium hydroxide mixture consisting of a magnesium hydroxide dispersion, a grinding aid, and a surfactant.

6. The method for preparing a highly dispersed magnesium-based flame retardant according to claim 1, Features: The surfactant is 4% to 6% by weight of the magnesium hydroxide filter biscuit material.

7. A method for preparing a highly dispersed magnesium-based flame retardant according to claim 4, Features: The grinding aid accounts for 1% to 2% of the weight of the magnesium hydroxide filter biscuit material.

8. The method for preparing a highly dispersed magnesium-based flame retardant according to claim 1, Features: The surfactant is selected from one or more of stearic acid, sodium stearate, zinc stearate, calcium stearate and magnesium stearate.

9. The method for preparing a highly dispersed magnesium-based flame retardant according to claim 7, Features: The grinding aid is polyethylene glycol with a molecular weight of 6000.

10. A highly dispersed magnesium-based flame retardant, It is characterized in that The highly dispersed magnesium-based flame retardant is obtained by the preparation method of any one of claims 1 to 9.