A thermoplastic starch / PBAT biodegradable composite material and preparation method thereof

By blending modified starch A and modified starch B with PBAT, the problem of reduced mechanical properties of starch/PBAT composite materials when the proportion of starch is increased is solved, and the high mechanical properties and rapid biodegradation of starch/PBAT composite materials are achieved. It reduces production costs and is suitable for large-scale production.

CN118496637BActive Publication Date: 2024-10-15TAIZHOU ZEYU NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410966187.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-15
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

The mechanical properties of existing starch/PBAT composite materials decrease when the proportion of starch is increased, making it difficult to achieve a good biodegradation rate and reduce costs at the same time.

Method used

Modified starch A and modified starch B are blended with PBAT. Modified calcium carbonate powder and sodium hexametaphosphate are added to the starch raw materials, and electron beam irradiation is applied to combine the water-based acrylic resin aqueous solution and N,N-diphosphate. Methylformamide treatment was used to prepare thermoplastic starch/PBAT biodegradable composite materials to increase the thermal processing performance and compatibility of starch.

Benefits of technology

While increasing the proportion of starch, it can obtain good mechanical properties, reduce production costs, increase the biodegradation rate, and the preparation method is stable and suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The present invention relates to the technical field of environmentally friendly degradable materials, and in particular to a thermoplastic starch / PBAT biodegradable composite material and a preparation method thereof. The weight ratio of each component of the composite material is as follows: 100 parts of PBAT, 120-160 parts of composite modified starch, 8-15 parts of plasticizer, and 1.5-3 parts of lubricant; the composite modified starch comprises modified starch A and modified starch B; the weight ratio of modified starch A and modified starch B is 1:0.6-0.8; a method for preparing a mixture of modified starch A and modified starch B with PBAT in steps can obtain good mechanical properties while increasing the proportion of starch, which is beneficial to reducing production costs, overcoming the problem that a high proportion of starch will lead to poor mechanical properties of the composite material, and is beneficial to improving the biodegradation rate; and the quality of samples prepared by the preparation method is stable, which is beneficial to large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of environmentally friendly degradable materials, and in particular to a thermoplastic starch / PBAT biodegradable composite material and a preparation method thereof. Background Art

[0002] Currently, petroleum-based plastics are widely used, but they are difficult to degrade, causing serious impacts on the environment. An effective way to solve this problem is to develop green and environmentally friendly biodegradable materials. Currently, polybutylene adipate / terephthalate (PBAT) is a new type of artificially synthesized biodegradable material with biodegradability and good mechanical properties, but its cost is relatively high and its biodegradation cycle far exceeds that of starch.

[0003] Although starch is an excellent and easily degradable natural polymer material, there are a large number of hydroxyl groups in its molecules that form strong hydrogen bond interactions, which makes natural starch not thermoplastic and difficult to process by thermoplastics. It also has poor mechanical properties and is very brittle, which is not conducive to its daily use. Therefore, it is currently necessary to modify starch to make it thermoplastic and then mix it with PBAT to reduce costs and improve biodegradability. However, an increase in the starch content in the mixed system will lead to a significant decrease in mechanical properties. Therefore, the mechanical properties, biodegradation rate and cost of the current starch / PBAT composite materials are contradictory, and it is impossible to increase the starch content while obtaining good material mechanical properties.

[0004] In summary, we consider how to increase the proportion of starch while maintaining good mechanical properties of the material, so as to reduce the cost and improve the biodegradability; in view of this, we propose a thermoplastic starch / PBAT biodegradable composite material and a preparation method thereof. Summary of the invention

[0005] The object of the present invention is to solve the deficiencies mentioned in the above background technology and to provide a thermoplastic starch / PBAT biodegradable composite material and a preparation method thereof.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] A thermoplastic starch / PBAT biodegradable composite material, wherein the weight proportions of the components of the composite material are: 100 parts of PBAT, 120-160 parts of composite modified starch, 8-15 parts of plasticizer, and 1.5-3 parts of lubricant;

[0008] The composite modified starch includes modified starch A and modified starch B;

[0009] The mass ratio of the modified starch A to the modified starch B is 1:0.6-0.8;

[0010] The specific mass proportion of each component of the modified starch A is: 100 parts of starch raw material, 10-20 parts of 1250-2000 mesh modified calcium carbonate powder, 3-6 parts of sodium hexametaphosphate, and the above components are mixed and irradiated to obtain modified starch A;

[0011] The specific mass proportion of each component of the modified starch B is: 100 parts of starch raw material, 15-30 parts of 30% solid content aqueous acrylic resin aqueous solution, and 15-30 parts of N,N-dimethylformamide.

[0012] Preferably, the starch raw materials of the modified starch A and the modified starch B are at least one of corn starch, rice starch, wheat starch, potato starch, sweet potato starch, cassava starch and lotus root starch.

[0013] Preferably, the plasticizer is glycerol and sorbitol in a mass ratio of 0.2-0.3:1.

[0014] Preferably, the lubricant is at least one of microcrystalline wax, white oil, stearic acid, butyl stearate, oleamide, and ethylene bisstearamide.

[0015] A method for preparing a thermoplastic starch / PBAT biodegradable composite material, wherein the specific steps of the preparation method are:

[0016] Step 1: Dry the starch raw material at 50-60°C until the moisture content of the starch raw material is no more than 3%, and grind it into a particle size of 13-25 μm for later use;

[0017] Step 2: preparing modified starch A and modified starch B respectively for later use;

[0018] Step 3: Mix modified starch A, modified starch B, PBAT, plasticizer and lubricant in proportion, and knead in a banbury mixer for 20-30 minutes, controlling the kneading temperature at 155-165°C and the speed at 65-80r / min;

[0019] Step 4: The mixture after internal mixing is extruded and granulated by a twin-screw extruder to obtain a composite material masterbatch, and the composite material masterbatch is dried at 80-85° C. for use.

[0020] Preferably, the specific steps for preparing the modified starch A are:

[0021] Step 1: weigh 1250-2000 mesh calcium carbonate powder according to proportion, add 0.8-1.5% coupling agent by weight of calcium carbonate powder, and obtain modified calcium carbonate powder by ball milling at 240-300 r / min in a planetary ball mill for 0.5-2h, dry at 60-85°C for 3-6h, and sieve 1250-2000 mesh to obtain modified calcium carbonate powder for standby use;

[0022] Step 2: Weigh the dried starch raw material, mix it with modified calcium carbonate powder and sodium hexametaphosphate according to proportion, and mix them evenly;

[0023] Step 3: During the mixing process, electron beam irradiation treatment is applied with an irradiation dose of 4-6 kGy to obtain modified starch A.

[0024] Preferably, the specific steps for preparing the modified starch B are:

[0025] Step 1: Prepare an aqueous acrylic resin aqueous solution, weigh a unit mass fraction of an aqueous acrylic resin emulsion, and dilute it to a solid content of 30%;

[0026] Step 2: Weigh the dried starch raw material according to the proportion, add distilled water and stir to form starch paste, weigh N,N-dimethylformamide and mix, and treat at 90-95°C for 0.5-1h;

[0027] Step 3: Add the aqueous acrylic resin solution, stir evenly, dry at 50-60°C for 48-72h, and grind with a grinder to obtain modified starch B.

[0028] Preferably, the barrel temperature of the twin-screw extruder in step 4 is set as follows: 130-135°C in zone 1, 135-140°C in zone 2, 140-145°C in zone 3, 145-150°C in zone 4, 150-160°C in zone 5, 160-165°C in zone 6, 165-170°C in zone 7, 165-170°C in zone 8, and 155-160°C in die head, and the screw speed is 60-80r / min.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The thermoplastic starch / PBAT biodegradable composite material can obtain good mechanical properties while increasing the proportion of starch by preparing modified starch A and modified starch B and blending with PBAT in steps, which is beneficial to reducing production costs and overcoming the problem that a high proportion of starch will lead to poor mechanical properties of the composite material. It is beneficial to improve the biodegradation rate, and the quality of samples prepared by the preparation method is stable, which is beneficial to large-scale production. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. In the absence of conflict, the embodiments in this application and the features in the embodiments can be combined with each other. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention.

[0032] The present invention describes the above technical solution in detail through the following embodiments:

[0033] Example 1

[0034] A thermoplastic starch / PBAT biodegradable composite material, wherein the weight proportions of the components of the composite material are as follows: 100 parts of PBAT, 120 parts of composite modified starch, 15 parts of plasticizer, and 3 parts of white oil;

[0035] In this embodiment, the mass ratio of modified starch A and modified starch B in 120 parts of composite modified starch is 1:0.8, and the starch raw materials of modified starch A and modified starch B are both corn starch; wherein the mass ratio of each component of modified starch A is specifically: 100 parts of starch raw material, 20 parts of modified calcium carbonate powder, and 6 parts of sodium hexametaphosphate; the mass ratio of each component of modified starch B is specifically: 100 parts of starch raw material, 30 parts of 30% solid content aqueous acrylic resin aqueous solution, and 15 parts of N,N-dimethylformamide.

[0036] Specifically, in this embodiment, PBAT adopts THJS-5801 PBAT sold by Xinjiang Lanshan Tunhe Chemical Industry with a density of 1.27 g / cm3; the starch raw materials used in modified starch A and modified starch B are both industrial-grade corn starch with a content of 95% and a particle size specification range of 70-100 mesh sold by Ningjin Jiahe Energy Saving Materials Co., Ltd.; the dilution raw material of the aqueous solution of the aqueous acrylic resin adopts AA-8675S aqueous acrylic resin emulsion sold by Suzhou Qingtian New Materials Co., Ltd. with a solid content of 75%, which is diluted to 30% solid content before use.

[0037] It should be explained that the present embodiment creatively prepares two states of modified starch separately, wherein the modified calcium carbonate powder is a well-known filler aggregate and can be used as a reinforcing agent for the material, and the sodium hexametaphosphate is a dispersant, the purpose of which is to make the filler aggregate dispersed evenly during the thermoplastic process; the modified starch B is modified with N,N-dimethylformamide starch, but an aqueous acrylic resin aqueous solution is introduced, and the aqueous acrylic resin aqueous solution is a water-soluble resin, the purpose of which is to be pre-mixed with the corn starch modified with N,N-dimethylformamide, so that the aqueous acrylic resin is dispersed in the mixture, thereby improving the compatibility with PBAT; it should be noted that it is very necessary to prepare modified starch A and modified starch B separately in the preparation method. Referring to the specific preparation steps below, it can be clearly judged that the process states of the preparation of the two are respectively in the dry solid state and the solid-liquid mixture. If the components of modified starch A and modified starch B are directly blended during the preparation process, the filler aggregate cannot be evenly distributed in the solid-liquid mixture, and the content distribution in the final dry product is uneven, which is not conducive to controlling the stability of the subsequent prepared materials.

[0038] Specifically, in this embodiment, the plasticizer uses glycerol and sorbitol in a mass ratio of 0.3:1; the working principle of the above plasticizer is to weaken the van der Waals force between the composite modified starch and PBAT, increase the plasticity of the blend, and then improve the compatibility of the mixture of the two, so as to improve the overall mechanical properties of the composite material; at the same time, because in order to increase the amount of starch in the composite material, calcium carbonate powder is introduced as an aggregate support in the modified starch A, which will cause the material to become more brittle, and the introduction of plasticizers can increase the peak value of the calcium carbonate powder that can be added, thereby improving the mechanical properties of the material; the glycerol selected in this process is safe and harmless, the sorbitol molecule is stable, and the molecular chain contains more hydroxyl groups, which can fully form a large number of hydrogen bonds with the hydroxyl groups of starch to further enhance the thermal processing performance.

[0039] The preparation method of the thermoplastic starch / PBAT biodegradable composite material in this embodiment has the following specific steps:

[0040] Step 1: Dry the corn starch raw material at 55°C until the moisture content of the corn starch raw material reaches 2.8%, grind the corn starch raw material, and sieve it through 500 mesh and 1000 mesh sieves in sequence, and keep the corn starch sieved on the 1000 mesh sieve for later use;

[0041] Step 2: preparing modified starch A, firstly weighing 2000 mesh calcium carbonate powder according to proportion, adding 1.5% of titanate coupling agent 201 by mass of calcium carbonate powder, ball milling for 1.5 hours at 300 r / min in a planetary ball mill, drying at 85° C. for 6 hours, sieving 2000 mesh to obtain modified calcium carbonate powder for standby use; weighing the dried standby corn starch raw material, mixing the modified calcium carbonate powder and sodium hexametaphosphate according to proportion, mixing evenly, applying electron beam irradiation treatment during the mixing process, and the irradiation dose of 6 kGy to obtain modified starch A;

[0042] Step 3: preparing modified starch B. In this embodiment, a 30% solid content aqueous acrylic resin emulsion is directly used as the aqueous acrylic resin solution. In other embodiments, the aqueous solution can be diluted according to the calibrated solid content. Weigh the dried and reserved corn starch raw material according to the proportion, add distilled water and stir to form a starch paste, mix it with the weighed N,N-dimethylformamide, and treat it at 95° C. for 1 hour. The modification mechanism of N,N-dimethylformamide used in this embodiment is that N,N-dimethylformamide can react with the hydroxyl groups in the starch molecules to form hydrogen bonds, thereby reducing the intermolecular force of the starch, improving the thermal processing property of the starch and making it thermoplastic. Then, mix the aqueous acrylic resin solution, stir evenly, dry at 60° C. for 72 hours, and grind it in a grinder to obtain modified starch B.

[0043] Step 4: Mix modified starch A, modified starch B, PBAT, plasticizer and white oil in proportion, and mix them in a mixer for 0.5 min, with the mixing temperature at 155°C and the speed at 75 r / min;

[0044] Step 5: After the internal mixing, the mixture is extruded and granulated through a TSJ50 twin-screw extruder to obtain a composite material masterbatch, and the temperature is set to 130°C for zone 1, 135°C for zone 2, 140°C for zone 3, 145°C for zone 4, 150°C for zone 5, 160°C for zone 6, 165°C for zone 7, 165°C for zone 8, and 160°C for the die head, and the screw speed is 60r / min; the composite material is extruded and water-cooled, cut and granulated to obtain a composite material masterbatch, and dried at 85°C for use.

[0045] Example 2

[0046] The difference between this embodiment and embodiment 1 is that in this embodiment, the mass ratio of modified starch A to modified starch B is 1:0.6, that is, 75 parts of modified starch A and 45 parts of modified starch B, and other conditions are the same.

[0047] Example 3

[0048] The difference between this embodiment and embodiment 1 is that the amount of the composite modified starch used in this embodiment is 160 parts, and other conditions are the same.

[0049] Example 4

[0050] The difference between this embodiment and embodiment 1 is that the ratio of glycerol to sorbitol in the plasticizer in this embodiment is 0.2:1, and other conditions are the same.

[0051] Example 5

[0052] The difference between this embodiment and embodiment 1 is that in this embodiment, only 15 parts of propylene glycol is used as the plasticizer, and other conditions are the same.

[0053] Example 6

[0054] The difference between this embodiment and embodiment 1 is that in this embodiment, only 15 parts of sorbitol are used as the plasticizer, and other conditions are the same.

[0055] Comparative Example 1

[0056] The difference between this comparative example and Example 1 is that in the preparation method of this comparative example, the specific steps for preparing the composite modified starch are: first, the prepared modified starch A and the aqueous acrylic resin solution with a solid content of 30% are set aside; then, the dried and reserved corn starch raw material is weighed, distilled water is added and stirred into a starch paste, mixed with N,N-dimethylformamide, and treated at 95°C for 1 hour to obtain the modified corn starch; then, the reserved modified starch A, the aqueous acrylic resin solution with a solid content of 30%, and the modified corn starch are mixed and stirred, and finally, the composite modified starch in an integrated mixed state is obtained after drying at 60°C for 72 hours, and then crushed, and other conditions are the same.

[0057] Comparative Example 2

[0058] The difference between this comparative example and Example 1 is that in this comparative example, the modified calcium carbonate powder in the modified starch A is placed in a banburying mixer and mixed with other components during banburying, and other conditions are the same.

[0059] Comparative Example 3

[0060] The difference between this comparative example and Example 1 is that in the preparation method of this comparative example, the mass ratio of modified starch A and modified starch B in this example is 1:1, that is, 60 parts of modified starch A and 60 parts of modified starch B, and other conditions are the same.

[0061] Comparative Example 4

[0062] The difference between this comparative example and Example 1 is that in the preparation method of this comparative example, the mass ratio of modified starch A and modified starch B in this example is 1:0.5, that is, 80 parts of modified starch A and 40 parts of modified starch B, and other conditions are the same.

[0063] Comparative Example 5

[0064] The difference between this comparative example and Example 1 is that: modified calcium carbonate powder and sodium hexametaphosphate are not added to the modified starch A in this comparative example, that is, the modified starch A is modified corn starch after irradiation with a dose of 6 kGy, and other conditions are the same.

[0065] Comparative Example 6

[0066] The difference between this comparative example and Example 1 is that no aqueous acrylic resin solution is added to the modified starch B in this comparative example, and other conditions are the same.

[0067] Comparative Example 7

[0068] The difference between this comparative example and Example 1 is that the comparative example reduces the amount of composite modified starch, using a total of 90 parts of composite modified starch, and other conditions are the same.

[0069] Comparative Example 8

[0070] The difference between this comparative example and Example 1 is that the comparative example increases the amount of composite modified starch, using a total of 190 parts of composite modified starch, and other conditions are the same.

[0071] Comparative Example 9

[0072] The difference between this comparative example and Example 1 is that this comparative example uses 120 parts of modified corn starch irradiated with 6 kGy, and other conditions are the same.

[0073] In summary, the composite masterbatches prepared in the above embodiments and comparative examples were sampled and tested as follows:

[0074] (1) Mechanical properties test

[0075] The tensile performance test was carried out using a WDW universal tensile testing machine. The tensile test was carried out with reference to the standard GB / T 1040.1-2018. The tensile strength and elongation at break were tested. The sample specifications were 150 mm long, 20 mm wide, and 1 mm thick. The elongation at break was the ratio of the increased length at break to the initial length, reflecting the tensile performance. The tensile strength was the maximum load borne by the original cross-sectional area of ​​the effective part of the sample during the test. It was the maximum tensile stress borne by the material until the sample broke when the tensile rate remained unchanged. The tensile rate was controlled to be 20 mm / min, and the gauge length of the sample was 50 mm.

[0076] The calculation formula is:

[0077]

[0078] Where: σ1 is the tensile strength, unit is MPa;

[0079] p is the maximum load or maximum force, in N;

[0080] d is the specimen thickness, in mm; b is the specimen width, in mm.

[0081] (2) Water absorption test

[0082] Prepare a sheet sample with a thickness of 20 mm and a width of 30 mm, dry it in an oven at 85°C until the weight no longer changes, then immerse the sample in 200 ml of water for 24 hours and take it out, wipe off the water on the surface with filter paper, and record the final mass by weighing on an analytical balance to calculate the water absorption rate; the calculation formula is:

[0083]

[0084] Where: w is the water absorption rate of the sample, unit is %;

[0085] m1 is the dry mass of the sample before water absorption, in g;

[0086] m2 is the wet mass of the sample after absorbing water, in g.

[0087] (3) Biodegradability test

[0088] Weigh 5kg of soil, place it in a vacuum drying oven at 80℃ and dry it to constant weight, sprinkle water to form a soil burial environment with a moisture content of 35%, prepare the sample into a 10cm wide and 0.1cm thick positive direction membrane sheet sample, lay 20cm thick soil at the bottom of the experimental container, place the sample on the soil and lay 20cm thick soil again; set up 3 groups of parallel samples, take them out after an interval of 50 days, rinse them, dry them, weigh them, and record the degradation rate. This test method is to determine its degradation rate per unit time; its calculation formula is:

[0089]

[0090] Where: N is the degradation rate of the sample, in units of %; n0 is the initial mass of the sample, in units of g;

[0091] n t It is the mass of the sample after 50 days of degradation, in g.

[0092] It should be noted that before testing, each test sample should be placed in a test environment with a temperature of 23℃±2℃ and a humidity of 50±10% for 48 hours according to the standard GB / T 2918-2018 before being taken out for testing;

[0093] The test data is as follows:

[0094]

[0095] According to the data of Example 1, Example 2, Comparative Example 3 and Comparative Example 4, when the total mass of modified starch A and modified starch B is the same, the mass ratio has an influence on the performance of the composite material: when the content of modified starch A increases, its performance is characterized by a significant improvement trend in tensile strength and water absorption, lower elongation at break, and a significant improvement in degradation rate; when the proportion of modified starch A is too high, the tensile strength tends to be stable without significant improvement, and the elongation at break becomes significantly lower and the water absorption becomes higher; therefore, the performance of Comparative Examples 3 and 4 is significantly worse than that of Example 1 and Example 2.

[0096] Referring to the data of Comparative Examples 1 and 2, it can be seen that if the steps of the preparation method are changed, the tensile strength of the material will be affected, but there will be no obvious effect on biodegradation. In Comparative Example 1, the integrated composite modified starch is directly blended. Although the other data except the tensile strength are similar, extreme value samples appear when testing the samples, which are judged to be invalid and removed. Considering the reasons, it is found that the method of the comparative example is easy to cause the modified calcium carbonate powder as an aggregate to settle in the aqueous solution, resulting in uneven distribution after drying. Although this preparation method can also obtain products with similar performance, it is not conducive to stable quality production, so this method is not preferred in actual production; while in Comparative Example 2, the modified calcium carbonate powder is directly mixed and kneaded. Although the elongation at break is close, the tensile strength is significantly reduced and the water absorption is increased. Considering that the surface modified molecules of the modified calcium carbonate powder can be grafted with the modified corn starch during irradiation, the modified calcium carbonate powder obtains a better pre-dispersion effect with the starch molecules in the solid state, so that the compatibility with PBAT during preparation is better, which is beneficial to improve the mechanical strength.

[0097] Referring to the data of Example 1, Comparative Example 7 and Comparative Example 8, it can be seen that: as the content of the composite modified starch increases, its tensile strength tends to gradually decrease, and the elongation at break becomes smaller, the water absorption rate becomes larger, but the biodegradability is significantly improved. The reason is that the high proportion of starch makes its biodegradation rate better; however, if the proportion of starch is too high, although the degradation performance is excellent, good material mechanical properties cannot be obtained.

[0098] Referring to the data of Example 4 to Example 6, it can be seen that when propylene glycol is used alone, the performance of the composite material is slightly better than that of sorbitol, and it has a better elongation at break. When the two are mixed, the elongation at break of the material can be further improved, and it has little effect on the tensile strength, water absorption rate and degradation rate. The high elongation at break is beneficial to the preparation of membrane structures in production.

[0099] Referring to the data of Comparative Examples 5, 6 and 9, it can be seen that the performance of Comparative Examples 5 and 6 is greatly reduced compared with that of Example 1, indicating that the modified calcium carbonate powder and the aqueous acrylic resin solution have an improvement effect on the material performance, while the biodegradability of Comparative Example 6 is improved, indicating that the aqueous acrylic resin solution affects the biodegradation to a certain extent; the data of Comparative Example 9 show that the mechanical properties of the composite material prepared by directly mixing a higher proportion of modified corn starch are poor, but the degradation performance is related to the proportion of starch. Although a high proportion of starch is beneficial to reducing costs, it does not have good application performance and is only used as a blank control.

[0100] In summary, it is important to explain that: although PBAT also has biodegradability, its degradation cycle is longer than that of starch. The thermoplastic starch / PBAT biodegradable composite material and its preparation method of this embodiment obtain a good biodegradation rate by increasing the proportion of corn starch, thereby reducing its preparation cost, which is conducive to large-scale production; taking Examples 1 to 3 as examples, the proportion of corn starch in the total mass of corn starch and PBAT in Examples 1 to 3 is taken as integers: 47%, 60%, and 55%, respectively. From the data, it can be seen that the corn starch content is positively correlated with the degradation rate; and the composite material creatively uses a composite modified starch mixed with PBAT, so that the composite material also has good mechanical properties. According to the data in the above table, Example 2 can be preferred.

Claims

1. A thermoplastic starch / PBAT biodegradable composite material, Features: The specific mass proportions of the components of the composite material are: 100 parts of PBAT, 120-160 parts of composite modified starch, 8-15 parts of plasticizer, and 1.5-3 parts of lubricant; The composite modified starch includes modified starch A and modified starch B; The mass ratio of the modified starch A to the modified starch B is 1:0.6-0.8; The specific mass proportion of each component of the modified starch A is: 100 parts of starch raw material, 10-20 parts of 1250-2000 mesh modified calcium carbonate powder, 3-6 parts of sodium hexametaphosphate, and the above components are mixed and irradiated to obtain modified starch A; The specific mass proportion of each component of the modified starch B is: 100 parts of starch raw material, 15-30 parts of 30% solid content aqueous acrylic resin aqueous solution, and 15-30 parts of N,N-dimethylformamide; The preparation method of the modified starch A is as follows: firstly, calcium carbonate powder of 1250-2000 mesh is weighed in proportion, a coupling agent accounting for 0.8-1.5% of the mass of the calcium carbonate powder is added, and the modified calcium carbonate powder is obtained after ball milling at 240-300r / min by a planetary ball mill for 0.5-2h, drying at 60-85°C for 3-6h, and sieving 1250-2000 mesh to obtain the modified calcium carbonate powder for standby use; then, the dried starch raw material is weighed, and the modified calcium carbonate powder and sodium hexametaphosphate are mixed in proportion, and mixed evenly; during the mixing process, electron beam irradiation treatment is applied, and the irradiation dose is 4-6kGy to obtain the modified starch A; The preparation method of the modified starch B is as follows: firstly, an aqueous acrylic resin aqueous solution is prepared, and a unit mass fraction of the aqueous acrylic resin emulsion is weighed and diluted to a solid content of 30%; then, a dry starch raw material is weighed in proportion, and distilled water is added and stirred into a starch paste, and N,N-dimethylformamide is weighed and mixed, and the mixture is treated at 90-95° C. for 0.5-1 h; finally, the aqueous acrylic resin aqueous solution is mixed, stirred evenly, dried at 50-60° C. for 48-72 h, and crushed by a pulverizer to obtain the modified starch B.

2. The thermoplastic starch / PBAT biodegradable composite material according to claim 1, Features: The starch raw materials of the modified starch A and the modified starch B are at least one of corn starch, rice starch, wheat starch, potato starch, sweet potato starch, cassava starch and lotus root starch.

3. The thermoplastic starch / PBAT biodegradable composite material according to claim 1, Features: The plasticizer is glycerol and sorbitol in a mass ratio of 0.2-0.3:

1.

4. The thermoplastic starch / PBAT biodegradable composite material according to claim 1, Features: The lubricant is at least one of microcrystalline wax, white oil, stearic acid, butyl stearate, oleamide, and ethylene bisstearamide.

5. A method for preparing the thermoplastic starch / PBAT biodegradable composite material according to any one of claims 1 to 4, Features: The specific steps of the preparation method are: Step 1: Dry the starch raw material at 50-60°C until the moisture content of the starch raw material is no more than 3%, and grind it into a particle size of 13-25 μm for later use; Step 2: preparing modified starch A and modified starch B respectively for later use; Step 3: Blend the modified starch A, modified starch B, PBAT, plasticizer and lubricant in proportion, and knead them in a banbury mixer for 20-30 minutes, with the kneading temperature at 155-165°C and the speed at 65-80r / min; Step 4: The mixture after internal mixing is extruded and granulated by a twin-screw extruder to obtain a composite material masterbatch, and the composite material masterbatch is dried at 80-85° C. for standby use.

6. The method for preparing the thermoplastic starch / PBAT biodegradable composite material according to claim 5, Features: In the step 4, the barrel temperature of the twin-screw extruder is set as follows: 130-135°C for zone 1, 135-140°C for zone 2, 140-145°C for zone 3, 145-150°C for zone 4, 150-160°C for zone 5, 160-165°C for zone 6, 165-170°C for zone 7, 165-170°C for zone 8, and 155-160°C for die head, and the screw speed is 60-80r / min.