Preparation method and application of subway plugging glue composition
By adding amino-terminated polyurethane additives to subway leak-proofing glue, the problem of poor performance of subway leak-proofing materials in the existing technology under vibration and disturbance environments has been solved, and a low-viscosity, fast-curing subway glue suitable for subway engineering has been developed. The leak-stopping glue achieves high-performance leak-proofing effect and scientific and strategic significance of environmental protection.
Patent Information
- Application Number
- CN202410911408.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-07-09
AI Technical Summary
Existing subway leakage-stopping materials are difficult to achieve good leakage-stopping effects in a vibration-disturbed environment, and the epoxy resin grouting is not soft enough, and the polyurethane foam is prone to secondary leakage, making it unable to meet the high-performance needs of subway projects.
Develop a two-component epoxy resin-type subway leak-proofing adhesive. By adding amino-terminated polyurethane additives, we design a low-viscosity, fast-curing subway leak-proofing adhesive composition, including epoxy resin, amino-terminated polyurethane, diluent and amine. Curing agent ensures curing in humid and underwater environments and provides good toughness and light transmittance.
It achieves rapid curing, strong toughness and light transmittance of the subway leakage sealing glue, which is suitable for leakage plugging applications in subway projects, provides leakage plugging effect in vibration environments, and reduces dependence on petrochemical energy and environmental pollution.
Smart Images

Figure CN118496790B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic polymer materials and products, and in particular to a preparation method and application of a subway leak-proof adhesive composition. Background Art
[0002] The damage to subway projects is not only caused by natural factors such as water damage, frost damage, lining cracks and lining erosion. There are also human factors such as vibration disturbance of the overall roadbed and underground passage when the subway train passes through the underground passage. The seepage of underground passages and subway stations is mainly caused by concrete defects on the structural surface. During pouring, the vibration is not dense, the hydration heat is too high, and the water content of the concrete is high, which will cause segregation and lead to looseness and honeycomb surface. When the external water pressure is greater than the anti-seepage pressure of the concrete here, water leakage will occur, which is mainly manifested as point leakage and surface leakage. In addition, the waterproof sealing treatment of embedded parts such as pipe heads, steel bar heads, and tie rod holes of equipment installation parts is not good, and leakage often occurs. When leakage occurs in underground passages and subway stations, it is necessary to stop the leakage in time.
[0003] In the prior art, inorganic grouting materials, such as ultrafine cement grouting and cement water glass grouting, or organic grouting materials, such as polyurethane foam and epoxy resin grouting, are generally used to plug leaks in underground passages and subway stations. However, existing grouting materials all have certain defects. For example, polyurethane foam is prone to secondary leakage, and epoxy resin grouting and inorganic plugging glue are not soft enough to achieve good plugging effects under vibration disturbance. Therefore, it is very necessary to develop high-performance plugging glue suitable for the special environment of subway engineering. Summary of the invention
[0004] The purpose of the present invention is to provide a preparation method and application of a subway plugging adhesive composition to solve the problems existing in the above-mentioned prior art. The present invention synthesizes an amino-terminated polyurethane additive that can make epoxy resin flexible and elastic and has high strength, and adds it to a two-component epoxy resin subway plugging adhesive to design a subway plugging adhesive composition with low viscosity, fast curing, curing in special environments (humid, underwater and other outdoor environments), and low water absorption.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] One of the technical solutions of the present invention: a subway plugging glue composition, comprising component A and component B; in terms of mass percentage, the raw material composition of component A is: 55-92.5% of epoxy resin, 5-30% of amino-terminated polyurethane and 2.5-15% of diluent; the raw material composition of component B is: 30-60% of amine curing agent and 40-70% of fast curing agent.
[0007] The subway plugging glue composition is a two-component epoxy resin type subway plugging glue, and the amino-terminated polyurethane is used as an additive of the two-component epoxy resin type subway plugging glue.
[0008] Furthermore, the epoxy resin includes one or two of E-51 and E-44; the diluent includes one or more of alkylene glycidyl ether, butyl glycidyl ether, 1,4-butanediol diglycidyl ether, ethylene glycol diglycidyl ether, phenyl glycidyl ether, polypropylene glycol diglycidyl ether, C12-14 fatty glycidyl ether, and benzyl glycidyl ether; the amine curing agent includes one or more of epoxy adducts of diethylenetriamine, phenolic amines, and polyamine-thiourea condensates; and the fast curing agent is a polythiol curing agent.
[0009] Furthermore, the polythiol curing agent includes one of Capcure 3-800, Capcure 3830-81, Capcure40secHV (USA), Capcure WR-6 (Germany), MP-gg90, and QE340-M (Japan).
[0010] Furthermore, the structural formula of the amino-terminated polyurethane is:
[0011] , 1≤x≤25, 0≤y≤8, 0<z≤40;
[0012] Among them, R1 is or ;
[0013] R2 is , 1≤m≤15, 1≤n≤60;
[0014] R3 is , , or ;
[0015] R4 is -CH2CH2-, -CH2CH2CH2-, or , 3≤s≤25.
[0016] Furthermore, the preparation method of the amino-terminated polyurethane comprises the following steps:
[0017] (1) Mixing cyclic carbonate and ethylenediamine, heating and performing a ring-opening addition reaction to obtain polyurethane diol (abbreviated as PCD);
[0018] (2) mixing the urethane diol with isocyanate and polypropylene carbonate polyol (PPCD for short), or mixing the urethane diol with isocyanate, heating and performing an addition reaction to obtain a polyurethane prepolymer;
[0019] (3) The polyurethane prepolymer is mixed with a diamine and subjected to a capping reaction to obtain the amino-terminated polyurethane.
[0020] Furthermore, when the cyclic carbonate and ethylenediamine are mixed, the molar ratio of the cyclic carbonate and ethylenediamine is 1:0.5; the temperature of the ring-opening addition reaction is 80° C. and the time is 2 hours; and the ring-opening addition reaction is carried out under nitrogen gas conditions.
[0021] Furthermore, the cyclic carbonate is propylene carbonate (abbreviated as PC, with a structural formula of ) or ethylene carbonate (abbreviated as EC, with the structural formula ); the isocyanate is hexamethylene diisocyanate (abbreviated as HDI, with a structural formula of ), isophorone diisocyanate (abbreviated as IPDI, with a structural formula of ), diphenylmethane diisocyanate (abbreviated as MDI, with a structural formula of ) or toluene diisocyanate (abbreviated as TDI, with the structural formula The diamine is ethylenediamine (EDA, structural formula: )、1,3-propylenediamine (structural formula is ), 4,4'-diaminobiphenyl (abbreviated as DDM, with a structural formula of ) or polyetheramine (structural formula is , s is 3≤s≤25).
[0022] Furthermore, the number average molecular weight of the polyetheramine is 230-600.
[0023] Furthermore, when the cyclic carbonate is propylene carbonate, the structural formula of the obtained urethane diol is When the cyclic carbonate is ethylene carbonate, the structural formula of the obtained urethane diol is .
[0024] Furthermore, the structural formula of the polypropylene carbonate polyol is , 1≤m≤15, 1≤n≤60.
[0025] Furthermore, the number average molecular weight of the polypropylene carbonate polyol is less than 3,000.
[0026] Furthermore, the temperature of the addition reaction is 80°C.
[0027] Furthermore, the polyurethane prepolymer is an isocyanate-terminated polyurethane prepolymer, and its structural formula is , 1≤x≤25, 0≤y≤8, 0<z≤40.
[0028] Furthermore, the number average molecular weight of the polyurethane prepolymer is 1000-10000. When preparing the polyurethane prepolymer, firstly, the molar amounts of the urethane diol, isocyanate and polypropylene carbonate polyol to be used are calculated according to the desired molecular weight of the polyurethane prepolymer, and then the urethane diol, isocyanate and polypropylene carbonate polyol are weighed according to the calculated molar amounts for addition reaction to obtain the polyurethane prepolymer of the desired molecular weight.
[0029] Furthermore, the number average molecular weight of the amino-terminated polyurethane is 1,000-10,000.
[0030] The present invention uses urethane diol and isocyanate as raw materials, or uses urethane diol, isocyanate and polypropylene carbonate polyol as raw materials to prepare a polyurethane prepolymer, and then uses a diamine to end-cap the polyurethane prepolymer to obtain an amino-terminated polyurethane. There are multiple choices for the urethane diol, isocyanate and polypropylene carbonate polyol, so the amino-terminated polyurethane product is named according to three variables. For example, PC-TE3000 in the present invention is a product with a number average molecular weight of 3000 synthesized from PC, TDI and EDA as raw materials, PC-TE10000 is a product with a number average molecular weight of 10000 synthesized from PC, TDI and EDA as raw materials, and PTMG-TE10000 is a polyether diol PTMG2000 (structural formula HO(CH2CH2CH2CH2O) r H, Mn=2000), TDI, EDA as raw materials to synthesize a product with a number average molecular weight of 10000. By controlling the group number ratio of diol to isocyanate, polyurethane prepolymers with different number average molecular weights can be obtained, and then end-capping with diamine can obtain polyurethane with any amino group. Since the smaller the number average molecular weight, the more difficult it is to control the degree of reaction, and the larger the number average molecular weight, the greater the system viscosity, the molecular weight of the polyurethane prepolymer is controlled at 1000-10000.
[0031] The second technical solution of the present invention: The preparation method of the above-mentioned subway plugging glue composition comprises the following steps: heating and mixing the amino-terminated polyurethane and the epoxy resin, and then adding a diluent to obtain component A; mixing a fast curing agent and an amine curing agent to obtain component B; and mixing component A and component B when using.
[0032] The third technical solution of the present invention: application of the above subway leak-proof adhesive composition in leak-proofing.
[0033] Furthermore, component A and component B are mixed and poured into the leaking area.
[0034] Furthermore, component A and component B are mixed in a mass ratio of 100:20-30. The more component B is used, the faster the curing speed.
[0035] Furthermore, the application of the subway plugging adhesive composition in plugging is preferably application in plugging in subway projects.
[0036] The subway plugging adhesive composition of the present invention uses epoxy resin as the main body, adds amino-terminated polyurethane to make it tough and strong, adds diluent to control the viscosity of the system to an injectable viscosity, and a mixed curing agent of a specific component allows it to dry on the surface in 25-50 minutes. The construction time and penetration range of the subway plugging adhesive composition can be determined by the surface drying time.
[0037] Adding more amino-terminated polyurethane to epoxy resin will increase the viscosity to a certain extent, affecting the penetration ability of the subway plugging glue composition into ground cracks and the like during operation, resulting in incomplete plugging. The present invention reduces the viscosity of the entire subway plugging glue composition system by adding a diluent, thereby improving the penetration ability of the subway plugging glue composition.
[0038] The present invention discloses the following technical effects:
[0039] The subway leak-proof adhesive composition of the present invention has a fast curing speed and an adjustable surface drying time, can be cured in special environments (humid, underwater and other outdoor environments), has good toughness after curing, acceptable bonding strength, and excellent light transmittance, and is suitable for leak-proofing in subway projects.
[0040] The amino-terminated polyurethane provided by the present invention contains carbamate groups and urea groups. When it is used as an additive for epoxy resin-type subway plugging glue, the carbamate groups and urea groups therein can be utilized to improve the cross-linking network of the epoxy resin, strengthen and toughen the epoxy resin, and the high light transmittance of the epoxy resin can be ensured while strengthening and toughening the epoxy resin.
[0041] The present invention adopts environmentally friendly CO2-based raw materials (PC, EC and PPCD) to replace non-renewable petroleum-based raw materials, and adopts the method of synthesizing polyurethane prepolymer to synthesize the reactive additive-terminated amino polyurethane, which can not only reduce the dependence on petrochemical energy, but also reduce pollution to the environment, and has important scientific and strategic significance.
[0042] The present invention can obtain a composite curing agent (component B) with adjustable surface drying time by performing a series of proportions on an amine curing agent and a fast curing agent (polythiol curing agent).
[0043] The present invention designs a subway plugging adhesive composition with better comprehensive performance by properly proportioning component A and component B. After the components A and B are mixed, there is sufficient operating time, and then the surface is dry, and the use strength is reached after 48 hours, and it is completely cured in 7 days, and it can be cured in complex outdoor environments such as humidity and underwater. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0045] Figure 1 The relationship curve between the light transmittance and wavelength of the film prepared from the subway plugging adhesive composition of Application Example 1 and Application Example 4;
[0046] Figure 2 This is a physical picture of the film prepared from the subway leak-proof adhesive composition of Application Example 1 and Application Example 4. DETAILED DESCRIPTION
[0047] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0048] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0049] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0050] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0051] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0052] The room temperature involved in the present invention specifically refers to 25°C ± 5°C. The amine curing agent used in the present invention is the epoxy adduct 593 of phenolic amine T-31 (referred to as T-31 curing agent) and diethylenetriamine 593 (referred to as 593 curing agent) produced by Shanghai Anpu Experimental Technology Co., Ltd., and the polythiol curing agent used is polythiol QE-340M produced by Toray Fine Chemicals Co., Ltd. of Japan.
[0053] Example 1
[0054] The preparation steps of amino-terminated polyurethane (PC-TE10000) are as follows:
[0055] (1) Add 1 mol of propylene carbonate (PC) to a three-necked flask, then dropwise add 0.5 mol of ethylenediamine, pass nitrogen, react at 80°C for 2 h, and then remove the unreacted raw materials by rotary evaporation to obtain urethane diol PCD264 (structural formula: ), add N,N'-dimethylformamide (DMF) as solvent in an amount equal to that of PCD264 to obtain a PCD264 solution, and store it in a dry place for later use.
[0056] (2) Add 0.1 mol (17.4 g) of toluene diisocyanate (TDI) into a three-necked flask and distill under reduced pressure at 80°C for 10 min to remove water. Then, add 50.52 g of PCD264 solution (containing 0.0957 mol PCD264) dropwise into the TDI at 80°C and keep the temperature at 80°C for 4 h to obtain a polyurethane prepolymer (structural formula: , x is any integer from 1 to 25, the average degree of polymerization of the whole system is 22.16, and the number average molecular weight is about 9880).
[0057] (3) At room temperature, 0.01 mol (0.6 g) of ethylenediamine was added dropwise to the polyurethane prepolymer and reacted for 2 h to terminate the polyurethane prepolymer. Excess ethylenediamine was removed by vacuum distillation at 80 °C for 1 h to obtain amino-terminated polyurethane (PC-TE10000, structural formula:
[0058] , number average molecular weight is about 10000).
[0059] Example 2
[0060] The preparation steps of amino-terminated polyurethane (PC-TE3000) are as follows:
[0061] (1) 0.1 mol (17.4 g) of TDI was added to a three-necked flask, and water was removed by vacuum distillation at 80°C for 10 min. Then, 45.45 g of the PCD264 solution (containing 0.0861 mol of PCD264) obtained in step (1) of Example 1 was added dropwise to the TDI at 80°C, and the reaction was maintained at 80°C for 4 h to obtain a polyurethane prepolymer (structural formula: , x is any integer from 1 to 12, the average degree of polymerization of the entire system is 6.18, and the number average molecular weight is about 2880).
[0062] (2) At room temperature, 0.03 mol (1.8 g) of ethylenediamine was added dropwise to the polyurethane prepolymer and reacted for 2 h to terminate the polyurethane prepolymer. Excess ethylenediamine was removed by vacuum distillation at 80 °C for 1 h to obtain amino-terminated polyurethane (PC-TE3000, structural formula:
[0063] , number average molecular weight is about 3000).
[0064] Example 3
[0065] The preparation steps of amino-terminated polyurethane (PC / PPCD-TE10000) are as follows:
[0066] (1) Add 1 mol of propylene carbonate (PC) to a three-necked flask, then dropwise add 0.5 mol of ethylenediamine, pass nitrogen gas, react at 80°C for 2 h, and then remove the unreacted raw materials by rotary evaporation to obtain urethane diol PCD264.
[0067] (2) Add 5.1 g of toluene diisocyanate (TDI) to a three-necked flask, remove water by vacuum distillation at 80°C, and dropwise add a mixed solution of 6.6 g of PCD264, 2.78 g of PPCD1000 and 7.8 g of DMF to TDI at 80°C. Keep the temperature at 80°C for 4 h to obtain a polyurethane prepolymer (structural formula: , where R1 is ; R2 is , 1≤m≤5, 1≤n≤20, the number average molecular weight is about 1000; R3 is ; x:y=9:1, z is any integer from 1 to 3, the average degree of polymerization of the entire system is 1.93, and the number average molecular weight is about 9880).
[0068] (3) At room temperature, 0.01 mol (0.6 g) of ethylenediamine was added dropwise to the polyurethane prepolymer and reacted for 2 h to terminate the polyurethane prepolymer. Excess ethylenediamine was removed by vacuum distillation at 80 °C for 1 h to obtain amino-terminated polyurethane (PC / PPCD-TE10000, with the structural formula
[0069] , number average molecular weight is about 10000).
[0070] Comparative Example 1
[0071] The preparation steps of amino-terminated polyurethane (PTMG-TE10000) are as follows:
[0072] (1) Add 0.05 mol (4.35 g) of TDI to a three-necked flask and distill under reduced pressure at 80°C for 10 min to remove water. Then, pour 0.04 mol (40 g) of PTMG2000 (polytetramethylene glycol with a molecular weight of 2000, to which dry molecular sieves have been added to remove water) and 20 g of DMF into the TDI at 80°C and keep the temperature at 80°C for 4 h to obtain a polyurethane prepolymer (structural formula: , p is any integer between 1 and 55, and the average is 27.52; f is any integer between 1 and 10, and the average is 4.46; the number average molecular weight of the whole system is about 9880).
[0073] (2) At room temperature, 0.03 mol (1.8 g) of ethylenediamine was added dropwise to the polyurethane prepolymer and reacted for 2 h to terminate the polyurethane prepolymer. Excess ethylenediamine was removed by vacuum distillation at 80 °C for 1 h to obtain amino-terminated polyurethane (PTMG-TE10000, with the structural formula
[0074] , number average molecular weight is about 10000).
[0075] Application Example 1
[0076] A subway plugging glue composition is composed of a component A and a component B, wherein the raw materials of the component A are composed by mass percentage of: 60% epoxy resin E-51, 30% amino-terminated polyurethane PC-TE10000 (prepared in Example 1) and 10% diluent butyl glycidyl ether 660A; the raw materials of the component B are composed by mass percentage of: 40% 593 type curing agent and 60% polythiol QE-340M.
[0077] The viscosity of components A and B was tested using an MCR301 rotational rheometer at a rotation speed of 200 r / min. The viscosity of component A was measured to be 8800 mPas and the viscosity of component B was 3830 mPas.
[0078] The preparation method of the subway plugging glue composition comprises the following steps:
[0079] 1) Weigh the raw materials according to the raw material ratio of component A, stir the amino-terminated polyurethane and epoxy resin at 80°C for 2h and 120°C for 2h, then add the diluent and stir evenly to obtain component A.
[0080] 2) Weigh the raw materials according to the ratio of component B, mix and stir thoroughly to obtain component B.
[0081] 3) Components A and B are fully mixed at a mass ratio of 100:25 and are ready for use.
[0082] After the A and B components were fully mixed at a mass ratio of 100:25, the surface drying time was measured to be 45 minutes according to GB / T 13477.5-2002.
[0083] Application Example 2
[0084] A subway plugging glue composition is composed of a component A and a component B, wherein the raw materials of the component A are composed by mass percentage of: 60% epoxy resin E-51, 30% amino-terminated polyurethane PC-TE3000 (prepared in Example 2) and 10% diluent butyl glycidyl ether 660A; the raw materials of the component B are composed by mass percentage of: 40% 593 type curing agent and 60% polythiol QE-340M.
[0085] The viscosity of components A and B was tested using an MCR301 rotational rheometer at a rotation speed of 200 r / min. The viscosity of component A was measured to be 6800 mPas and the viscosity of component B was 3830 mPas.
[0086] The preparation method of the subway plugging glue composition is the same as that of Application Example 1.
[0087] After the A and B components were fully mixed at a mass ratio of 100:25, the surface drying time was measured to be 45 minutes according to GB / T 13477.5-2002.
[0088] Application Example 3
[0089] A subway plugging glue composition is composed of a component A and a component B, wherein the raw materials of the component A are composed by mass percentage of: 70% epoxy resin E-51, 20% amino-terminated polyurethane PC-TE3000 (prepared in Example 2) and 10% diluent butyl glycidyl ether 660A; the raw materials of the component B are composed by mass percentage of: 40% 593 curing agent and 60% polythiol QE-340M.
[0090] The viscosity of components A and B was tested using an MCR301 rotational rheometer at a rotation speed of 200 r / min. The viscosity of component A was measured to be 6500 mPas and the viscosity of component B was 3830 mPas.
[0091] The preparation method of the subway plugging glue composition is the same as that of Application Example 1.
[0092] After the A and B components were fully mixed at a mass ratio of 100:25, the surface drying time was measured to be 50 minutes according to GB / T 13477.5-2002.
[0093] Application Example 4
[0094] A subway plugging glue composition, consisting of a component A and a component B, wherein the raw materials of the component A are composed by mass percentage of: 60% epoxy resin E-51, 30% amino-terminated polyurethane PC-TE10000 (prepared in Example 1) and 10% diluent butyl glycidyl ether 660A; the raw materials of the component B are composed by mass percentage of: 40% T-31 curing agent and 60% polythiol QE-340M.
[0095] The viscosity of components A and B was tested using an MCR301 rotational rheometer at a rotation speed of 200 r / min. The viscosity of component A was measured to be 8800 mPas and the viscosity of component B was 5600 mPas.
[0096] The preparation method of the subway plugging glue composition is the same as that of Application Example 1.
[0097] After the A and B components were fully mixed at a mass ratio of 100:25, the surface drying time was measured to be 30 minutes according to GB / T 13477.5-2002.
[0098] Application Example 5
[0099] A subway plugging glue composition is composed of a component A and a component B, wherein the raw materials of the component A are composed by mass percentage of: 60% epoxy resin E-51, 30% amino-terminated polyurethane PC-TE3000 (prepared in Example 2) and 10% diluent butyl glycidyl ether 660A; the raw materials of the component B are composed by mass percentage of: 40% T-31 curing agent and 60% polythiol QE-340M.
[0100] The viscosity of components A and B was tested using an MCR301 rotational rheometer at a rotation speed of 200 r / min. The viscosity of component A was measured to be 6800 mPas and the viscosity of component B was 5600 mPas.
[0101] The preparation method of the subway plugging glue composition is the same as that of Application Example 1.
[0102] After the A and B components were fully mixed at a mass ratio of 100:25, the surface drying time was measured to be 30 minutes according to GB / T 13477.5-2002.
[0103] Application Example 6
[0104] A subway plugging glue composition, consisting of a component A and a component B, wherein the raw materials of the component A are composed by mass percentage of: 70% epoxy resin E-51, 20% amino-terminated polyurethane PC-TE3000 (prepared in Example 2) and 10% diluent butyl glycidyl ether 660A; the raw materials of the component B are composed by mass percentage of: 40% T-31 curing agent and 60% polythiol QE-340M.
[0105] The viscosity of components A and B was tested using an MCR301 rotational rheometer at a rotation speed of 200 r / min. The viscosity of component A was measured to be 6500 mPas and the viscosity of component B was 5600 mPas.
[0106] The preparation method of the subway plugging glue composition is the same as that of Application Example 1.
[0107] After the A and B components were fully mixed at a mass ratio of 100:25, the surface drying time was measured to be 30 minutes according to GB / T 13477.5-2002.
[0108] Application Example 7
[0109] A subway plugging glue composition is composed of a component A and a component B, wherein the raw materials of the component A are composed by mass percentage of: 60% epoxy resin E-51, 30% amino-terminated polyurethane PC / PPCD-TE10000 (prepared in Example 3) and 10% diluent butyl glycidyl ether 660A; the raw materials of the component B are composed by mass percentage of: 40% T-31 curing agent and 60% polythiol QE-340M.
[0110] The viscosity of components A and B was tested using an MCR301 rotational rheometer at a rotation speed of 200 r / min. The viscosity of component A was measured to be 8900 mPas and the viscosity of component B was 5600 mPas.
[0111] The preparation method of the subway plugging glue composition is the same as that of Application Example 1.
[0112] After the A and B components were fully mixed at a mass ratio of 100:25, the surface drying time was measured to be 40 minutes according to GB / T 13477.5-2002.
[0113] Application Example 8
[0114] A subway plugging glue composition, consisting of a component A and a component B, wherein the raw materials of the component A are composed by mass percentage: 60% epoxy resin E-51, 30% amino-terminated polyurethane PC-TE10000 (prepared in Example 1) and 10% diluent butyl glycidyl ether 660A; the raw materials of the component B are composed by mass percentage: 30% T-31 curing agent, 30% 593 curing agent and 40% polythiol QE-340M.
[0115] The viscosity of components A and B was tested using an MCR301 rotational rheometer at a rotation speed of 200 r / min. The viscosity of component A was measured to be 8800 mPas and the viscosity of component B was 4230 mPas.
[0116] The preparation method of the subway plugging glue composition is the same as that of Application Example 1.
[0117] After the A and B components were fully mixed at a mass ratio of 100:25, the surface drying time was measured to be 25 minutes according to GB / T 13477.5-2002.
[0118] Comparative application example 1
[0119] A subway plugging glue composition consists of a component A and a component B, wherein the raw materials of the component A are composed by mass percentage of: 90% epoxy resin E-51 and 10% diluent butyl glycidyl ether 660A; the raw materials of the component B are composed by mass percentage of: 40% 593 type curing agent and 60% polythiol QE-340M.
[0120] The preparation method of the subway plugging glue composition is the same as that of Application Example 1.
[0121] The viscosity of components A and B was tested using an MCR301 rotational rheometer at a rotation speed of 200 r / min. The viscosity of component A was measured to be 1450 mPas and the viscosity of component B was 3830 mPas.
[0122] After the A and B components were fully mixed at a mass ratio of 100:25, the surface drying time was measured to be 45 min according to GB / T 13477.5-2002.
[0123] Comparative Application Example 2
[0124] A subway plugging glue composition consists of a component A and a component B, wherein the raw materials of the component A are composed by mass percentage of: 90% epoxy resin E-51 and 10% diluent butyl glycidyl ether 660A; the raw materials of the component B are composed by mass percentage of: 40% T-31 curing agent and 60% polythiol QE-340M.
[0125] The preparation method of the subway plugging glue composition is the same as that of Application Example 1.
[0126] The viscosity of components A and B was tested using an MCR301 rotational rheometer at a rotation speed of 200 r / min. The viscosity of component A was measured to be 1450 mPas and the viscosity of component B was 5600 mPas.
[0127] After the A and B components were fully mixed at a mass ratio of 100:25, the surface drying time was measured according to GB / T 13477.5-2002 to be 25 min.
[0128] Comparative Application Example 3
[0129] A subway plugging glue composition consists of a component A and a component B, wherein the raw materials of the component A are composed by mass percentage of: 60% epoxy resin E-51, 30% amino-terminated polyurethane PTMG-TE10000 (prepared in comparative example 1) and 10% diluent butyl glycidyl ether 660A; the raw materials of the component B are composed by mass percentage of: 40% 593 curing agent and 60% polythiol QE-340M.
[0130] The preparation method of the subway plugging glue composition is the same as that of Application Example 1.
[0131] The viscosity of components A and B was tested using an MCR301 rotational rheometer at a rotation speed of 200 r / min. The viscosity of component A was measured to be 4950 mPas and the viscosity of component B was 3830 mPas.
[0132] After the A and B components were fully mixed at a mass ratio of 100:25, the surface drying time was measured to be 35 min according to GB / T 13477.5-2002.
[0133] Comparative Application Example 4
[0134] A subway plugging adhesive composition consists of a component A and a component B, wherein the raw materials of the component A are composed by mass percentage of: 60% epoxy resin E-51, 30% amino-terminated polyurethane PC-TE10000 (prepared in Example 1) and 10% diluent butyl glycidyl ether 660A; the raw materials of the component B are composed of polythiol QE-340M.
[0135] The preparation method of the subway plugging glue composition is the same as that of Application Example 1.
[0136] The viscosity of components A and B was tested using an MCR301 rotational rheometer at a rotation speed of 200 r / min. The viscosity of component A was measured to be 8800 mPas and the viscosity of component B was 14300 mPas.
[0137] After the A and B components were fully mixed at a mass ratio of 100:25, the surface drying time was measured according to GB / T 13477.5-2002 to be 60 min.
[0138] Test Case
[0139] 1. Tensile shear strength test
[0140] The subway plugging adhesive compositions of each application example and comparative application example were used to prepare tensile shear specimens, and the tensile shear strength of the tensile shear specimens was tested using an electronic universal tensile machine according to the GB / T7124-2008 standard, with a test rate of 5 mm / min. The high-permeability epoxy resin caulking adhesive DK-1 produced by Reinforcement Doctor (Shanghai) Construction Technology Co., Ltd. was used as the control group.
[0141] The preparation method of tensile shear specimens is as follows: mix component A and component B, stir evenly, and then evenly coat them on a polished 304 stainless steel plate (10 mm × 25 mm), keeping the adhesive layer size at 25 mm × 12.5 mm × 0.2 mm (size after curing), and place them at room temperature (80% humidity) for 48 hours.
[0142] 2. Tensile strength and elongation at break test
[0143] The subway plugging adhesive compositions of each application example and comparative application example were used to prepare dumbbell type 2 specimens, and the tensile strength and elongation at break of the dumbbell type 2 specimens were tested using an electronic universal tensile machine according to the GB / T1040-2006 standard, with a test rate of 20 mm / min. The high-permeability epoxy resin caulking adhesive DK-1 produced by Reinforcement Doctor (Shanghai) Construction Technology Co., Ltd. was used as the control group.
[0144] The preparation method of dumbbell type 2 specimen is as follows: mix component A and component B, inject into a mold for making dumbbell type 2 specimen, and place at room temperature (80% humidity) for 48 hours.
[0145] The test results of tensile shear strength, tensile strength and elongation at break are shown in Table 1:
[0146] Table 1 Mechanical properties of various application examples and comparative application examples
[0147] Tensile shear strength / MPa Tensile strength / MPa Elongation at break Application Example 1 5.68 13.71 70% Application Example 2 3.09 3.33 61% Application Example 3 3.38 10.23 67% Application Example 4 4.38 5.8 47% Application Example 5 1.99 8.02 49% Application Example 6 5.25 11.72 52% Application Example 7 5.71 5.90 60% Application Example 8 8.21 15.15 51% Comparative application example 1 5.95 2.26 94% Comparative Application Example 2 1.94 1.79 96% Comparative Application Example 3 3.34 18.8 18% Comparative Application Example 4 0.89 3.89 34% Control group 8.33 51.59 12%
[0148] As can be seen from Table 1, the tensile strength of the subway plugging adhesive composition of application examples 1-8 is weaker than that of the plugging adhesive (DK-1) on the market, but the elongation at break is better. And compared with the comparative application examples without amino-terminated polyurethane, the tensile strength and tensile shear strength of the application examples modified with amino-terminated polyurethane are higher. In addition, the toughness of the polyurethane modified plugging adhesive prepared by polyether diol is not much improved, but the rigidity is significantly reduced. Finally, the composite curing agent makes the performance of the plugging adhesive composition more excellent, rather than only the weakness of polythiol.
[0149] 3. Concrete bond test
[0150] The subway leak-proof adhesive composition blended in Application Example 1 was coated on a concrete slab that had been soaked in water for 2 hours in advance, and then a customized hook was adhered to the adhesive. The hook and the concrete formed an adhesive layer with a radius of 11 mm. After curing in a water bath at room temperature for 48 hours, the adhesion test was carried out by adding a weight to the hook.
[0151] The final result is: the adhesive layer is not damaged when a 95kg weight is hung, and the adhesive layer interface is damaged when a 100kg weight is hung. Through calculation, the tensile shear strength is about 2.45MPa.
[0152] 4. Test of insoluble content of solidified material
[0153] Take 10g of each of the subway plugging adhesive compositions blended in Application Example 1 and Application Example 4, of which 5g is used for curing at room temperature with a humidity of 80% for 2 days, and the other 5g is used for underwater curing at room temperature for 2 days. After 2 days, the insoluble content of the cured product is tested according to GB / T 2576-2005. The calculation formula for the insoluble content is as follows:
[0154]
[0155] The test results are shown in Table 2. As can be seen from the table, the insoluble content of the underwater cured subway plugging adhesive composition has not decreased much, and is still above 85%, indicating that the subway plugging adhesive composition can be used in subway water seepage areas.
[0156] Table 2 Insoluble content
[0157] Application Examples Humidity 80% room temperature Underwater room temperature 1 88.34% 87.51% 4 91.41% 91.05%
[0158] 5. Light transmittance test
[0159] The subway plugging glue of Application Example 1 and Application Example 4 was used to prepare a 0.1 mm thick film (see the actual picture). Figure 2 As shown, Figure 2In the figure, letter a is placed under the sample of application example 1, and letter b is placed under the sample of application example 4). Lambda 950 UV-visible spectrophotometer was used to test the transmittance of the film in the test range of 200nm-800nm. The results are as follows Figure 1 As shown in the figure, in the visible light range of 400nm-760nm, the transmittance of Application Example 4 is as high as 99%. Figure 2 As can be seen from the actual pictures, both are highly transparent and can clearly show the letter content below the sample.
[0160] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A subway plugging adhesive composition, characterized in that: The invention comprises component A and component B; the raw materials of component A are composed of 55-92.5% epoxy resin, 5-30% amino-terminated polyurethane and 2.5-15% diluent by mass percentage; the raw materials of component B are composed of 30-60% amine curing agent and 40-70% fast curing agent; The structural formula of the amino-terminated polyurethane is: ,1≤x≤25,0≤y≤8,0<z≤40; Among them, R1 is or ; R2 is , 1≤m≤15, 1≤n≤60; R3 is , , or ; R4 is -CH2CH2-, -CH2CH2CH2-, or , 3≤s≤25; The epoxy resin includes one or two of E-51 and E-44; the diluent includes one or more of alkylene glycidyl ether, butyl glycidyl ether, 1,4-butanediol diglycidyl ether, ethylene glycol diglycidyl ether, phenyl glycidyl ether, polypropylene glycol diglycidyl ether, C12-14 fatty glycidyl ether, and benzyl glycidyl ether; the amine curing agent includes one or more of epoxy adducts of diethylenetriamine, phenolic amines, and polyamine-thiourea condensates; and the fast curing agent is a polythiol curing agent.
2. The subway plugging adhesive composition according to claim 1, characterized in that: The preparation method of the amino-terminated polyurethane comprises the following steps: (1) mixing a cyclic carbonate and ethylenediamine, heating and performing a ring-opening addition reaction to obtain urethane diol; (2) mixing the urethane diol with isocyanate and polypropylene carbonate polyol, or mixing the urethane diol with isocyanate, heating and performing an addition reaction to obtain a polyurethane prepolymer; (3) The polyurethane prepolymer is mixed with a diamine and subjected to a capping reaction to obtain the amino-terminated polyurethane.
3. The subway plugging adhesive composition according to claim 2, characterized in that: The cyclic carbonate is propylene carbonate or ethylene carbonate; the isocyanate is hexamethylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate or toluene diisocyanate; the diamine is ethylenediamine, 1,3-propylenediamine, 4,4'-diaminobiphenyl or polyetheramine.
4. The subway plugging adhesive composition according to claim 2, characterized in that: The structural formula of the polypropylene carbonate polyol is , 1≤m≤15, 1≤n≤60.
5. The subway plugging adhesive composition according to claim 3, characterized in that: The structural formula of the polyetheramine is , 3≤s≤25.
6. The method for preparing the subway plugging adhesive composition according to any one of claims 1 to 5, characterized in that: The following steps are involved: The amino-terminated polyurethane and epoxy resin are heated and mixed, and then a diluent is added to obtain component A; a fast curing agent and an amine curing agent are mixed to obtain component B; and components A and B are mixed when used.
7. Use of the subway plugging adhesive composition as described in any one of claims 1 to 5 in plugging leaks.
8. The use according to claim 7, characterized in that Mix component A and component B and pour into the leak.
Citation Information
Patent Citations
Alcohol amine chain extender, and preparation method and applications thereof
CN110862336A
Environment-friendly polyurethane chain extender as well as preparation method and application thereof
CN110894275A
Preparation of polyfunctional cyclic carbonate and application of polyfunctional cyclic carbonate in epoxy adhesive
CN117603180A
Toughened epoxy adhesive composition
KR102377780B1
KR20230000603A