Confined remelting treatment method for alloy steel and alloy steel after confined remelting treatment

Through the limited domain remelting treatment method, the problem of large-size carbides in medium and high-carbon alloy steels is solved, and the refinement and uniformization of carbides is achieved, and the mechanical properties and fatigue life of alloy steels are improved.

CN118497508BActive Publication Date: 2024-11-15INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410956930.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-15
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

Large-size primary carbides are common in medium and high-carbon alloy steels, resulting in stress concentration and fatigue cracks, which seriously damage the service performance and life of components.

Method used

The limited-domain remelting treatment method is adopted to heat the alloy steel to the remelting temperature T1 and keep it warm, and then cool to the re-solidation temperature T2 and keep it warm. By controlling the temperature and time, large-sized carbides are dissolved to form fine and uniform carbides.

Benefits of technology

Effectively eliminate or refine large-size carbides in alloy steel, improve the comprehensive mechanical properties and rolling contact fatigue life of alloy steel, and avoid the crushing and residue of carbides during forging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118497508B_ABST
    Figure CN118497508B_ABST
Patent Text Reader

Abstract

The present invention relates to a limited remelting treatment method for alloy steel and the alloy steel after limited remelting treatment, which relates to the field of ferrous metal technology, and solves the problem of how to eliminate and dissolve large-sized primary carbides in medium- and high-carbon alloy steels. The limited remelting treatment method comprises: heating the alloy steel to a remelting temperature T1, and keeping it at the remelting temperature T1 for t1 time; then, cooling the alloy steel to a resolidification temperature T2, and keeping it at the resolidification temperature T2 for t2 time, cooling, and obtaining the alloy steel after limited remelting treatment. Wherein, the remelting temperature T1 is 5-60°C higher than T; the resolidification temperature T2 is 10-200°C lower than T; and T is the melting point temperature of the primary carbide in the alloy steel. The present invention is used to heat treat the alloy steel, dissolve the primary carbide, and obtain an alloy steel with fine and uniform carbides.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ferrous metals, and in particular to a limited remelting treatment method for alloy steel and the alloy steel after the limited remelting treatment. Background Art

[0002] Medium and high carbon alloy steels are widely used in key basic components such as bearings, gears, molds, cutting tools, springs, and drive shafts. They are of great significance in ensuring my country's status as a major and powerful manufacturing country.

[0003] At present, primary carbides with a diameter exceeding 2μm are common in medium and high carbon alloy steels; such micron-sized carbides can cause stress concentration and induce fatigue cracks, thus seriously damaging the service performance and life of components.

[0004] Therefore, there is an urgent need for a method that can eliminate or refine large-sized primary carbides in medium-high carbon alloy steels to obtain medium-high carbon alloy steel materials with fine and uniform carbides. Summary of the invention

[0005] In view of this, the present invention provides a limited remelting treatment method for alloy steel and the alloy steel after the limited remelting treatment. The main purpose is to dissolve the primary carbide by performing limited remelting treatment on the alloy steel, so that the carbide in the alloy steel after the limited remelting treatment is fine and uniform.

[0006] In order to achieve the above object, the present invention mainly provides the following technical solutions:

[0007] On the one hand, an embodiment of the present invention provides a confined remelting method for alloy steel, wherein the confined remelting method for alloy steel comprises the following steps:

[0008] The alloy steel is heated to a remelting temperature T1 and kept at the remelting temperature T1 for a time period of t1; then, the alloy steel is cooled to a resolidification temperature T2 and kept at the resolidification temperature T2 for a time period of t2, and then cooled to obtain the alloy steel after the limited remelting treatment.

[0009] Wherein, the remelting temperature T1 is 5-60°C higher than T; the resolidification temperature T2 is 10-200°C lower than T; and T is the melting point temperature of the primary carbide in the alloy steel.

[0010] Preferably, the melting point temperature T of the primary carbide in the alloy steel is tested by the following method: a sample of the alloy steel is tested by a differential scanning calorimeter DSC, and in the measured temperature rise curve, the temperature corresponding to an endothermic peak before the alloy matrix melting endothermic peak of the alloy steel is the melting point temperature T of the primary carbide in the alloy steel.

[0011] Preferably, the t1 is 1-24h.

[0012] Preferably, the t2 is 0-2h.

[0013] Preferably, the cooling rate of the alloy steel from the remelting temperature T1 to the resolidification temperature T2 is not less than 0.5°C / s.

[0014] Preferably, the cooling rate of the alloy steel from the remelting temperature T1 to the resolidification temperature T2 is 0.5-1°C / s.

[0015] Preferably, the alloy steel is cooled from the remelting temperature T1 to the resolidification temperature T2 by means of air blowing cooling or water mist cooling.

[0016] Preferably, before the confined remelting treatment, carbides with a size greater than 5 μm exist in the alloy steel.

[0017] Preferably, before the confined remelting treatment, the carbides in the alloy steel include one or more of network carbides, large island carbides, and long strip carbides.

[0018] On the other hand, an embodiment of the present invention provides an alloy steel, an alloy steel after confined remelting treatment, wherein the alloy steel after the confined remelting treatment is obtained by confined remelting of the alloy steel using any of the confined remelting treatment methods for alloy steel described above; wherein there is no carbide with an equivalent diameter greater than 2 μm in the alloy steel after the confined remelting treatment.

[0019] Preferably, the alloy steel is any one of high-speed steel, bearing steel, gear steel, mold steel, spring steel and tool steel.

[0020] Compared with the prior art, the limited remelting treatment method of alloy steel and the alloy steel after limited remelting treatment of the present invention have at least the following beneficial effects:

[0021] The present invention proposes the concept of limited remelting treatment for the first time, mainly by utilizing the different degrees of segregation inside the alloy steel, and the characteristics that there are a large number of primary carbides in the area with severe segregation and a low melting point. The alloy steel is heated to the remelting temperature T1, so that the carbide-rich area melts while the alloy matrix does not melt, that is, the melting behavior is limited to the target micro-area by utilizing the micro-segregation of the alloy itself, so as to promote the dissolution and re-precipitation and refinement of carbides. Specifically, the role of the insulation of heating the alloy steel to the remelting temperature T1 is to melt the micro-area with severe segregation, that is, the carbide aggregation area, while the alloy matrix remains solid; the role of insulation when cooling to the resolidification temperature T2 is to re-solidify the melted micro-area and form fine primary carbides. In addition, the cooling rate of the alloy steel from the remelting temperature T1 to the resolidification temperature T2 is not less than 0.5°C / s, so as to suppress the re-segregation during the solidification process and avoid aggravating the problem of carbides. Here, the confined remelting method of the present invention achieves the purpose of the present invention through the coordinated cooperation of two temperatures, one high and one low.

[0022] In addition, the limited remelting treatment method of alloy steel provided in the embodiment of the present invention does not require special equipment and can be implemented using the existing ordinary heat treatment furnace in the factory, which is convenient for technical promotion. Moreover, the limited remelting treatment method of alloy steel provided in the embodiment of the present invention is not only applicable to high-carbon bearing steel, such as: 9Cr18Mo, 8Cr4Mo4V, etc.; it is also applicable to various alloy steels that are prone to produce large-sized carbides, especially high-speed steel, bearing steel, gear steel, mold steel, spring steel and tool steel, such as: H13, T1, W6Mo5Cr4V2, M2, M42 and other grades. It can be seen that the limited remelting method provided in the embodiment of the present invention has wide applicability.

[0023] In addition, an embodiment of the present invention further provides an alloy steel after a confined remelting treatment, wherein the alloy steel after the confined remelting treatment is obtained by confined remelting the alloy steel using any of the confined remelting treatment methods for alloy steel described above. The alloy steel after the confined remelting treatment has no coarse spherical carbides inside, and only contains nanoscale secondary carbides or fine lamellar primary carbides at some grain boundary positions, and such fine lamellar primary carbides can be broken during the later forging process, and no large-sized carbide residues will be formed.

[0024] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the distribution of carbide morphology in 8Cr4Mo4V steel before confined remelting treatment;

[0026] Figure 2 is a schematic diagram of carbide morphology distribution in 8Cr4Mo4V steel after confined remelting treatment in Example 1 of the present invention;

[0027] Figure 3 This is a schematic diagram of the distribution of carbide morphology in 8Cr4Mo4V steel obtained in Comparative Example 1;

[0028] Figure 4 This is a schematic diagram of the carbide morphology distribution in the 8Cr4Mo4V steel obtained in Comparative Example 2. DETAILED DESCRIPTION

[0029] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention application are described in detail below in conjunction with the accompanying drawings and preferred embodiments. In the following description, different "one embodiment" or "embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures, or characteristics in one or more embodiments may be combined in any suitable form.

[0030] On the one hand, an embodiment of the present invention provides a limited remelting treatment method for alloy steel, which is used to treat the alloy steel to refine the primary carbide, and comprises the following steps: heating the alloy steel to a remelting temperature T1, and keeping it at the remelting temperature T1 for t1 time; then, cooling the alloy steel to a resolidification temperature T2, and keeping it at the resolidification temperature T2 for t2 time, and then cooling to obtain the alloy steel after the limited remelting treatment.

[0031] Wherein, the remelting temperature T1 is 5-60°C higher than T; the resolidification temperature T2 is 10-200°C lower than T; and T is the melting point temperature of the primary carbide in the alloy steel.

[0032] Preferably, the melting point temperature T of the primary carbide in the alloy steel is tested by the following method: a sample of the alloy steel is tested by a differential scanning calorimeter DSC, and in the measured temperature rise curve, the temperature corresponding to an endothermic peak before the alloy matrix melting endothermic peak of the alloy steel is the melting point temperature T of the primary carbide in the alloy steel.

[0033] Preferably, the t1 is 4-8h. The t2 is 0-0.5h. Preferably, the cooling rate of the alloy steel from T1 to T2 is 0.5-1°C / s.

[0034] Here, the present invention proposes the concept of limited remelting for the first time, taking advantage of the different degrees of segregation inside the alloy, and the presence of a large number of large-sized primary carbides with low melting points in the severe segregation area, to heat the alloy steel to a specific temperature, so that the carbide-rich area melts while the alloy matrix does not melt, that is, the micro-segregation of the alloy itself is used to limit the melting behavior to the target micro-area to promote the dissolution of carbides. Furthermore, by accurately controlling the cooling rate from the remelting temperature T1 to the resolidification temperature T2, solidification segregation can be suppressed, and carbides are prompted to precipitate into a refined lamellar structure, and finally an alloy steel with uniform and fine carbides is obtained.

[0035] It should be noted that the term "remelting" in the present invention refers to allowing the primary carbide to melt and then re-precipitate; "confinement" refers to limiting the melting area to a specific location to avoid overburning or grain boundary oxidation of the alloy, and this area limitation is achieved by utilizing the melting point difference caused by the segregation of the alloy itself, and has self-selectivity.

[0036] Specifically, the holding temperature and time are designed according to the type and size of the alloy steel, and the alloy steel is placed in a heating furnace for confined remelting treatment to cause local melting of the carbide-enriched micro-region while the alloy matrix remains solid. The steel is cooled after a period of holding.

[0037] Preferably, an embodiment of the present invention provides a limited remelting method for alloy steel, and the preferred scheme is as follows:

[0038] 1) The alloy steel is placed in a heating furnace, heated to a remelting temperature T1, and kept at the remelting temperature T1 for a time t1.

[0039] Among them, the remelting temperature T1 is 5-60°C higher than T, and t1 is 1-24h.

[0040] Here, the role of this step is to melt the micro-regions with severe segregation, i.e., carbide aggregation regions, while the alloy matrix remains solid.

[0041] 2) Cool the heating furnace to the resolidification temperature T2 and keep it at this temperature for t2 time;

[0042] The resolidification temperature T2 is 10-200°C lower than T, t2 is 0-2h, and the cooling rate is not less than 0.5°C / s, preferably 0.5-1°C / s.

[0043] The function of this step is to rapidly solidify the melted micro-region and form fine primary carbides.

[0044] It should be noted that: at the remelting temperature T1, the carbides melt to form a micro-molten pool, and the rich alloy atoms in the molten pool quickly diffuse into the surrounding matrix. After a period of insulation, the area of ​​the micro-molten pool expands, and the alloy concentration in the molten pool decreases. According to the phase diagram thermodynamics, when the alloy concentration in the molten pool is high, large-sized primary carbides will be produced, and when the alloy concentration is low, the molten pool will solidify rapidly to form fine primary carbides.

[0045] 3) Cooling the alloy steel to room temperature to obtain alloy steel.

[0046] Here, the obtained alloy steel does not contain primary carbides with a diameter greater than 2 μm. Preferably, the alloy steel does not contain primary carbides.

[0047] It is mainly explained that the method of the present invention is not only applicable to high-carbon bearing steels, such as 9Cr18Mo, 8Cr4Mo4V, etc.; it is also applicable to various alloy steels that are prone to produce large-sized spherical carbides, especially high-speed steel, bearing steel, gear steel, mold steel, spring steel and tool steel, such as H13, T1, W6Mo5Cr4V2, M2, M42 and other grades.

[0048] Here, the confined remelting treatment method of the present invention is mainly used to perform carbide control treatment on alloy ingots (alloy steel), but is not limited to this. Carbide control treatment can also be performed on alloy steel ingots (alloy steel) after heat processing or heat treatment.

[0049] The present invention is further described below by specific embodiments:

[0050] Example 1

[0051] This embodiment mainly performs confined remelting treatment on 8Cr4Mo4V alloy steel (i.e., 8Cr4Mo4V steel ingot) to obtain 8Cr4Mo4V alloy steel; wherein, the alloy steel is an 8Cr4Mo4V steel ingot with a diameter of 220 mm obtained after vacuum induction melting and vacuum consumable melting; here, the melting point T of the primary carbide in the 8Cr4Mo4V steel ingot is 1185°C as determined by DSC. The main steps are as follows:

[0052] 1) Place the alloy steel in a heating furnace, heat it to 1190°C (i.e., remelting temperature T1), and keep it at this temperature for 4 hours.

[0053] 2) Cool the alloy steel to 1000℃ (resolidification temperature T2) at a cooling rate of 1℃ / s and keep it at this temperature for 0.2h.

[0054] 3) Turn off the power of the heating furnace and cool the alloy steel to room temperature along with the furnace to obtain 8Cr4Mo4V alloy steel after limited remelting treatment.

[0055] Figure 1 This is a schematic diagram of the carbide morphology distribution in 8Cr4Mo4V steel before confined remelting treatment. It can be seen that there are network-like coarse carbides inside it. The size of a single carbide exceeds 30μm, and the size of cluster carbides exceeds 100μm.

[0056] Figure 2 Schematic diagram of carbide morphology distribution in 8Cr4Mo4V steel after confined remelting treatment in Example 1 of the present invention. Figure 2 It can be seen that there are no coarse primary carbides inside the 8Cr4Mo4V steel after confined remelting treatment, and only fine lamellar primary carbides exist at the grain boundaries. Such lamellar primary carbides can be broken during the later forging process and no large-sized carbide residues will be formed.

[0057] Example 2

[0058] This embodiment mainly performs confined remelting treatment on alloy steel (9Cr18Mo steel ingot) to obtain 9Cr18Mo alloy steel; wherein the alloy steel is a 9Cr18Mo steel ingot with a diameter of 250 mm obtained after vacuum induction melting and vacuum consumable melting; here, the melting point T of the primary carbide of the 9Cr18Mo steel ingot is 1210°C. The main confined remelting steps are as follows:

[0059] 1) Place the alloy steel in a heating furnace, heat it to 1230°C (i.e., remelting temperature T1), and keep it at this temperature for 6 hours.

[0060] 2) Cool the alloy steel to 1100°C (resolidification temperature T2) at a cooling rate of 1°C / s and keep it at this temperature for 0.1h.

[0061] 3) Turn off the power of the heating furnace and cool the alloy steel furnace to room temperature to obtain 8Cr4Mo4V alloy steel after limited remelting.

[0062] In this embodiment, before the confined remelting treatment, a large number of linear twin carbides with a size greater than 20 μm exist in the 9Cr18Mo steel ingot. The performance indicators of the 9Cr18Mo alloy steel obtained after the confined remelting treatment are as follows: there are no coarse primary carbides inside, and only fine lamellar primary carbides exist at the grain boundary position. Such lamellar primary carbides can be broken in the later forging process, and no large-sized carbide residues will be formed.

[0063] Example 3

[0064] This embodiment mainly performs confined remelting treatment on alloy steel (M2 steel ingot) to obtain M2 alloy steel; wherein the alloy steel is an M2 steel ingot with a diameter of 200 mm obtained after vacuum induction melting and electroslag remelting; here, the melting point T of the primary carbide of the M2 steel ingot is 1190°C. The main confined remelting steps are as follows:

[0065] 1) Place the alloy steel in a heating furnace, heat it to 1200°C (i.e., remelting temperature T1), and keep it at this temperature for 12 hours.

[0066] 2) Cool the alloy steel to 1100°C (resolidification temperature T2) at a cooling rate of 0.8°C / s and keep it at this temperature for 10 h.

[0067] 3) Turn off the power of the heating furnace and cool the alloy steel furnace to room temperature to obtain the M2 alloy steel after limited remelting.

[0068] In this embodiment, a large number of network and island carbides with a size greater than 15 μm are present in the M2 steel before confined remelting treatment. The performance indicators of the M2 alloy steel obtained after confined remelting are as follows: there are no coarse primary carbides inside, only fine lamellar primary carbides exist at the grain boundaries, and no large-sized carbides remain.

[0069] Example 4

[0070] In this embodiment, alloy steel (W6Mo5Cr4V2 steel) is mainly subjected to confined remelting treatment to obtain W6Mo5Cr4V2 alloy steel; wherein the alloy steel is a W6Mo5Cr4V2 steel ingot with a diameter of 160 mm obtained after vacuum induction melting and electroslag remelting; here, the melting point T of the primary carbide of the W6Mo5Cr4V2 steel ingot is 1220°C. The main confined remelting steps are as follows:

[0071] 1) Place the alloy steel in a heating furnace, heat it to 1240°C (i.e., remelting temperature T1), and keep it at this temperature for 20 hours.

[0072] 2) Cool the alloy steel to 1140°C (resolidification temperature T2) at a cooling rate of 0.6°C / s and keep it at this temperature for 0.5h.

[0073] 3) Turn off the power of the heating furnace and cool the alloy steel furnace to room temperature to obtain W6Mo5Cr4V2 alloy steel after limited remelting.

[0074] In this embodiment, a large number of network and island carbides with a size greater than 10 μm exist in the W6Mo5Cr4V2 steel before the confined remelting treatment. The performance indicators of the W6Mo5Cr4V2 alloy steel obtained after the confined remelting treatment are as follows: there are no coarse primary carbides inside, only fine lamellar primary carbides exist at the grain boundary position, and no large-sized carbides remain.

[0075] Comparative Example 1

[0076] Comparative Example 1 is to use a conventional process to perform carbide control treatment (homogenization heat treatment) on alloy steel (i.e., 8Cr4Mo4V steel ingot) to obtain 8Cr4Mo4V alloy steel; wherein the alloy steel is an 8Cr4Mo4V steel ingot with a diameter of 220 mm obtained after vacuum induction melting and vacuum consumable melting. The conventional process steps are as follows:

[0077] The 8Cr4Mo4V steel ingot is placed in a heating furnace and heated to 1210°C, kept warm for 48 hours, and then furnace cooled to room temperature to obtain 8Cr4Mo4V steel.

[0078] Figure 3 This is a schematic diagram of the distribution of carbide morphology in 8Cr4Mo4V steel obtained in Comparative Example 1. Figure 3 It can be seen that a large number of large-sized primary carbides with a size exceeding 20μm appear in the 8Cr4Mo4V steel casting after traditional processing. Some are spherical and some are lamellar. The spherical carbides cannot be broken during the subsequent hot deformation process, so they will remain in the alloy steel product, reducing product quality and service life.

[0079] Comparative Example 2

[0080] Comparative Example 2 is to perform confined remelting treatment on alloy steel (8Cr4Mo4V steel ingot), wherein the alloy steel is an 8Cr4Mo4V steel ingot with a diameter of 250 mm obtained after vacuum induction melting and vacuum consumable melting; here, the melting point T of the primary carbide of the 8Cr4Mo4V steel ingot is 1185°C. The main confined remelting steps are as follows:

[0081] 1) Place the alloy steel in a heating furnace, heat it to 1230°C (i.e., remelting temperature T1), and keep it at this temperature for 6 hours.

[0082] 2) Cool the alloy steel to 1100°C (resolidification temperature T2) at a cooling rate of 0.1°C / s and keep it at this temperature for 0.1h.

[0083] 3) Turn off the power of the heating furnace and cool the alloy steel furnace to room temperature to obtain 8Cr4Mo4V alloy steel after limited remelting.

[0084] Figure 4This is a schematic diagram of the distribution of carbide morphology in 8Cr4Mo4V steel obtained in Comparative Example 2. Figure 4 It can be seen that due to the slow cooling rate in step 2), carbide segregation occurred again during the cooling process.

[0085] In summary, the confined remelting method of alloy steel proposed in an embodiment of the present invention can significantly refine the carbides in medium-high carbon alloy steels, thereby obtaining medium-high carbon alloy steel materials with fine and uniform carbides, which is beneficial to improving the comprehensive mechanical properties of alloy steels and increasing the rolling contact fatigue life by more than 2 times.

[0086] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A limited remelting method for alloy steel, characterized in that: The limited remelting treatment method of the alloy steel comprises the following steps: The alloy steel is heated to a remelting temperature T1, and kept at the remelting temperature T1 for a time of t1; then, the alloy steel is cooled to a resolidification temperature T2, and kept at the resolidification temperature T2 for a time of t2, and then cooled to obtain an alloy steel after limited remelting treatment; wherein the cooling rate of the alloy steel from the remelting temperature T1 to the resolidification temperature T2 is not less than 0.5°C / s; Wherein, the remelting temperature T1 is 5-60°C higher than T; the resolidification temperature T2 is 10-200°C lower than T; and T is the melting point temperature of the primary carbide in the alloy steel.

2. The method for confined remelting of alloy steel according to claim 1, characterized in that: The melting point temperature T of the primary carbide in the alloy steel is tested by the following method: a sample of the alloy steel is tested by a differential scanning calorimeter DSC, and in the measured temperature rise curve, the temperature corresponding to an endothermic peak before the alloy matrix melting endothermic peak of the alloy steel is the melting point temperature T of the primary carbide in the alloy steel.

3. The method for confined remelting of alloy steel according to claim 1, characterized in that: The t1 is 1-24h.

4. The method for confined remelting of alloy steel according to claim 1, characterized in that: The t2 is 0-2h.

5. The method for confined remelting of alloy steel according to claim 1, characterized in that: The cooling rate of the alloy steel from the remelting temperature T1 to the resolidification temperature T2 is 0.5-1°C / s.

6. The method for confined remelting of alloy steel according to any one of claims 1 to 5, characterized in that: The alloy steel is cooled from the remelting temperature T1 to the resolidification temperature T2 by means of air blowing cooling or water mist cooling.

7. The limited remelting treatment method for alloy steel according to claim 1, characterized in that: Before the confined remelting treatment, carbides with a size greater than 5 μm exist in the alloy steel.

8. The method for confined remelting of alloy steel according to claim 7, characterized in that: Before the confined remelting treatment, the carbides in the alloy steel include one or more of network carbides, large island carbides, and long strip carbides.

9. An alloy steel after confined remelting treatment, characterized in that: The alloy steel after the confined remelting treatment is obtained by confined remelting the alloy steel using the confined remelting treatment method for alloy steel described in any one of claims 1 to 8; wherein, there is no carbide with an equivalent diameter greater than 2 μm in the alloy steel after the confined remelting treatment.

10. The alloy steel after confined remelting treatment according to claim 9, characterized in that: The alloy steel is any one of high-speed steel, bearing steel, gear steel, mold steel, and spring steel.

11. The alloy steel after confined remelting treatment according to claim 9, characterized in that: The alloy steel is tool steel.