A lightweight, high-modulus, high-toughness, corrosion-resistant aluminum alloy material and a preparation method thereof

By adding Li and other trace elements to the Al-Mg-Zn series aluminum alloys, a specific precipitation sequence and structure are formed, which solves the problem of increased density of existing aluminum alloys when improving strength and corrosion resistance, and achieves low density, The comprehensive performance matching of high modulus and high toughness is suitable for the material needs of high-end manufacturing.

CN118497566BActive Publication Date: 2024-10-18GRIMAT ENG INST CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410954764.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-18
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

While improving the strength and corrosion resistance of the existing Al-Mg-Zn series aluminum alloys, it is difficult to achieve a comprehensive performance match of low density, high modulus and high toughness, and adding heavy elements such as Cu will lead to increased density and corrosion resistance. Corrosion performance deteriorates.

Method used

By controlling the contents of Mg and Zn in the Al-Mg-Zn series aluminum alloys and adding a higher content of Li, an Al3Li aging precipitation sequence is formed, which cooperatively precipitates T-Mg32(Al,Zn)49 and δ′-Al3Li structures. Precipitation strengthening phase, combined with lower content of Zr, Mn, Sc, Er and other elements for micro-alloying, controlling Cu, Fe, Si impurity content, and optimizing the component ratio to improve the aging strengthening response ability and elastic modulus of the alloy.

Benefits of technology

It significantly improves the strength and elastic modulus of the alloy while maintaining good corrosion resistance, achieving a comprehensive performance match of light weight, high strength, and damage resistance, and is suitable for the material needs of high-end manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118497566B_ABST
    Figure CN118497566B_ABST
Patent Text Reader

Abstract

The present invention discloses a lightweight, high modulus, high toughness and corrosion resistant aluminum alloy material and a preparation method thereof. The aluminum alloy contains: Mg 5.0-7.9wt%, Zn 2.2-4.6wt%, Li 0.5-1.9wt%, and at least one of Mn, Ti, Zr, Sc and Er elements with a total content not exceeding 0.7wt%, and the remainder is Al and unavoidable impurities, wherein each impurity element is ≤0.25wt% and the total is ≤0.50wt%. The preparation method of the alloy deformed material comprises the following steps: (1) manufacturing an aluminum alloy ingot under atmosphere protection; (2) performing homogenization heat treatment and / or preheating on the obtained ingot; (3) hot processing the ingot into a desired processed material form or pre-processed material by a hot deformation processing method; (4) reheating the pre-processed material and performing cold deformation processing on the desired processed material form; (5) performing solid solution heat treatment on the processed material; (6) rapidly cooling the processed material after the solid solution heat treatment to room temperature; and (7) performing aging treatment on the processed material to obtain an alloy aged processed material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of aluminum alloy and its preparation and processing, and particularly relates to Al-Mg-Zn-Li series aluminum alloy. More specifically, the present invention relates to a lightweight, high modulus, high toughness and corrosion-resistant Al-Mg-Zn-Li series aluminum alloy material and a preparation method thereof. Background Art

[0002] As a high-quality, high-specific-strength, lightweight structural material, aluminum alloy has become the second largest metal material in the world after steel after more than a hundred years of development. It is developing towards high strength, high modulus, high toughness, corrosion resistance, precision and other applications. 3 ), high specific strength, easy processing and low cost, it is widely used in aviation, aerospace, high-speed rail, automobile, shipbuilding and other fields. In order to better support the weight reduction design of aluminum alloy structural parts, it is necessary to further develop new aluminum alloys with low density, high strength, high modulus, high toughness and corrosion resistance.

[0003] The existing commercial deformed aluminum alloys mainly include Al-Cu series (2xxx series), Al-Mn series (3xxx series), Al-Si series (4xxx series), Al-Mg series (5xxx series), Al-Mg-Si series (6xxx series) and Al-Zn-Mg-Cu series (7xxx series) aluminum alloys. Among them, Al-Mg series alloys use Mg as the main alloying element. They have medium strength, excellent corrosion resistance and welding performance, and are the second largest aluminum alloy variety after Al-Mg-Si series. The commonly used Al-Mg series aluminum alloy grades at home and abroad mainly include 5052, 5056, 5083, 5182, 5A02, 5A06, etc., and their Mg content is generally between 2.5~5.5wt.%. Among all commercial deformed aluminum alloys, the Mg content is the highest and the density is the lowest. Moreover, for every 1wt.% increase in Mg content, the density decreases by nearly 0.4%. When the Mg content exceeds the normal range and further increases, a large amount of β-Al3Mg2 phase will be produced in the alloy matrix along the grain boundaries, which will not only fail to produce the dispersion strengthening effect, but will also corrode before the matrix, causing severe exfoliation corrosion and intergranular corrosion. Therefore, for Al-Mg aluminum alloys, simply increasing the Mg content to improve the alloy strength will generally cause a serious deterioration in the overall performance of the alloy. If the Mg content in the Al-Mg aluminum alloy can be increased while adding appropriate alloying elements to form a precipitation strengthening phase with excess Mg elements, effectively inhibiting the formation of β phases precipitated along the grain boundaries, it is possible to significantly improve the strength of the Al-Mg aluminum alloy while maintaining its low density characteristics and avoid serious deterioration in corrosion resistance.

[0004] In order to achieve aging precipitation strengthening of Al-Mg aluminum alloys, existing studies have shown that Ag and Zn can be added to form T-Mg 32 (Al,Ag) 49 and T-Mg 32 (Al, Zn) 49 Since the 1960s, studies have found and confirmed that adding trace Ag elements to Al-Mg alloys will precipitate T-Mg 32( Al, Ag) 49 Although the addition of Ag can effectively improve the precipitation strengthening reaction of Al-Mg alloys, and the reasonable combination of pretreatment and aging treatment can make Al-Mg-Ag alloys obtain good strength and plasticity matching, it is difficult to apply Ag in large quantities in industrial production due to its high price. Since the beginning of this century, studies have found that after adding Zn to conventional Al-Mg aluminum alloys, T-Mg can be formed in the alloy grains and grain boundaries through toughening heat treatment. 32 (Al, Zn) 49Precipitation phase, inhibiting the formation of β phase, thereby effectively improving the strength of Al-Mg aluminum alloys and avoiding serious deterioration of their corrosion resistance, showing important application value. For example: Patent document CN103866167A discloses an aluminum alloy and its alloy plate, as well as a preparation method of the alloy plate, the basic composition range of which is: Mg: 5.5~6.0wt%, Zn: 0.6~1.2wt%, Cu: 0.1~0.2wt%, Mn: 0.6~1.0wt%, Zr: 0.05~0.25wt%, Cr≤0.1wt%, Ti≤0.15wt%, Fe≤0.25wt%, Li≤0.2wt%, and the rest is Al. By adding Zn, the alloy greatly reduces the ability of Al3Mg2 to precipitate continuously at the grain boundary, and shows higher strength and corrosion resistance than traditional AA5059-H321 and AA5059-H131 plates. Patent document CN104152759A discloses a high-strength, corrosion-resistant Al-Mg alloy and its preparation process, wherein the basic composition ranges from Mg: 5.0 to 6.5 wt%, Zn: 1.2 to 2.5 wt%, Mn: 0.4 to 1.2 wt%, Zr: 0.05 to 0.25 wt%, Cu≤0.4 wt%, Cr≤0.1wt%, Ti≤0.15 wt%, Fe≤0.4wt%, Li≤0.4 wt%, and the remainder is Al and unavoidable impurities. Compared with traditional aluminum alloys for ships such as AA5083 and AA5059, the alloy significantly improves the intergranular corrosion resistance of the alloy while maintaining certain mechanical properties and exfoliation corrosion properties. Patent document CN104694800A discloses a high-strength, lightweight Al-Mg-Zn alloy, whose basic composition range is: Mg: 6.0~10.0wt%, Zn: 3.0~5.0wt%, Cu<2.0wt%, Mn<1.2wt%, Fe<0.3wt%, Li<0.3wt%, at least one element of Cr, Ti, Zr, Sc, Hf, La, Ce, Pr, Nd is added, and the amount of a single element added is less than 0.5wt%. The tensile strength of the alloy in the T6 state exceeds 530MPa. Other studies have found that the simultaneous addition of Li elements to the alloy is conducive to significantly reducing the density, and combined with the addition of more Cu elements, the alloy has a higher strength.Patent document CN104711463A discloses a method for preparing an Al-Mg-Zn-Li aluminum alloy and a plate thereof, wherein the basic composition ranges from Mg: 3.0 to 8.0 wt%, Zn: 2.1 to 5.0 wt%, Li <2.0 wt%, Cu <2.0 wt%, Mn <1.2 wt%, Fe <0.3 wt%, Si <0.3 wt%, and one or more elements selected from Cr, Ti, Zr, Sc, Hf, La, Ce, Pr, Nd, and Ag are added, and the amount of a single element added is less than 0.5 wt%; other impurity elements are inevitably present, and the amount of a single impurity element does not exceed 0.05 wt%, the total amount of impurities does not exceed 0.2 wt%, and the balance is Al. The prepared alloy plate has high strength and low density. Patent document CN104862551A discloses an Al-Mg-Cu-Zn aluminum alloy and a method for preparing an aluminum alloy sheet, wherein the basic composition ranges from Mg: 4.0 to 6.0 wt%, Cu: 0.30 to 1.0 wt%, Zn: 1.0 to 3.5 wt%, Mn≤0.4 wt%, Fe≤0.4 wt%, Li≤0.4 wt%, Cr≤0.2 wt%, Ti≤0.1 wt%, and the remainder is Al and unavoidable impurities. The alloy increases the Cu content in the alloy on the basis of AA5182 and AA5023 alloys, and Zn is added at the same time, making full use of the precipitation strengthening of the transition phase of the S phase in the Al-Mg-Cu system and the transition phase of the T phase in the Al-Mg-Zn system, and can be used for significantly improving the strength of automotive inner panels during the 180°C / 30min paint treatment process. Patent document CN110541096A discloses a high-strength, easy-to-weld Al-Mg-Zn-Cu alloy and its preparation method, the basic composition range of which is: Mg: 4.3~7.0wt%, Zn: 2.5~5.0 wt%, Cu: 0.4~1.2 wt%, Mn≤0.3 wt%, Cr≤0.1 wt%, Ti≤0.2 wt%, Zr≤0.3wt%, the rest is Al and unavoidable impurities, wherein the Zn / Mg mass ratio is ≤1.0, and the strength of the alloy is basically equivalent to that of the traditional 7xxx series aluminum alloy. Another study further improved the performance of the alloy by adding Si element to the Al-Mg-Zn alloy. Patent document CN116065066A discloses a lightweight, high-strength, corrosion-resistant aluminum alloy, whose basic components range from Mg: 6.0~10.0wt%, Zn: 1.0~3.5wt%, Si: 0.1~1.3wt%, and at least one of Mn, Cu, Zr, Sc, and Ti elements with a total content not exceeding 0.8wt%, and the rest being Al and unavoidable impurities. The alloy exhibits excellent low density, high strength, corrosion resistance, and damage resistance.

[0005] Although the research and development of Al-Mg-Zn series alloys has achieved certain results in recent years, there is still a lot of room for improvement in the excellent matching of key properties such as low density, high strength, corrosion resistance and damage resistance of the alloy. For example, adding Zn and Cu elements to Al-Mg series aluminum alloys improves the strength of the alloy, but since most of these elements are heavy elements, Al-Mg series aluminum alloys lose their inherent low density advantage, and their specific strength is not as competitive as that of traditional 2xxx and 7xxx series aluminum alloys; Al-Mg-Zn-Si alloys can obtain low density, high strength and toughness and corrosion resistance, but cannot simultaneously obtain an increase in elastic modulus; adding light element Li to Al-Mg-Zn-Cu alloys is beneficial to reducing the density of the alloy, but it is easy to form coarse second phases such as AlZnLi, AlCuLi and AlCuMg, which deteriorates the corrosion resistance and damage resistance of the alloy. Therefore, it is necessary to further study and develop new Al-Mg-Zn-Li aluminum alloy materials with excellent matching of key properties such as low density, high modulus, high strength, damage resistance and corrosion resistance. Summary of the invention

[0006] The present invention has found through a lot of research and industrial practice that the existing Al-Mg-Zn series aluminum alloy mainly uses Mg and Zn as the main strengthening components, and Mg 32 (Al, Zn) 49 Phase is the main strengthening phase, and its precipitation sequence and main strengthening phase type are relatively single, making it difficult to obtain the ideal comprehensive performance matching of light weight, high strength, high modulus, corrosion resistance and damage resistance. If in the existing Al-Mg-Zn series aluminum alloys, the Mg and Zn contents are controlled in a higher range, and a higher content of Li is added as the main alloying element without adding Cu, the alloy will be further lightweight. At the same time, the newly added Al3Li aging precipitation sequence can significantly enhance the aging strengthening response ability of the alloy, improve the elastic modulus of the alloy, and inhibit the formation of grain boundary β-Al3Mg2 phase, effectively avoiding the deterioration of the corrosion performance of the alloy; further assist in the use of low content Zr, Mn, Sc, Er and other elements for microalloying to refine the alloy structure; especially strictly control the content of Cu, Fe, and Si impurities, minimize the formation of coarse second phases, thereby ensuring the improvement of material performance. Fine optimization design of the composition range and the ratio of each element of the alloy is an important guarantee to ensure its excellent performance matching. Through reasonable design, the alloy can be made to precipitate T-Mg in the aging process while ensuring light weight. 32 (Al, Zn) 49 and the precipitation strengthening phase of the δ′-Al3Li structure, so that the Al-Mg-Zn-Li series alloy of the present invention obtains high modulus and high strength and toughness while maintaining good corrosion resistance.

[0007] The purpose of the present invention is to overcome the shortcomings of the comprehensive performance matching of the existing Al-Mg-Zn series aluminum alloy materials, and on the basis of the existing alloys, further improve their comprehensive performance matching through the optimization design of composition and preparation and processing technology, so as to provide an ideal material for the high-end manufacturing industry, which is a lightweight Al-Mg-Zn-Li series aluminum alloy with both strength, toughness and corrosion resistance.

[0008] The primary technical problem to be solved by the present invention is to propose a lightweight, high-strength, corrosion-resistant and damage-resistant aluminum alloy material. The second technical problem to be solved by the present invention is to propose a method for preparing the aluminum alloy material. The third technical problem to be solved by the present invention is to propose that the aluminum alloy material is welded with itself or other alloys to form a new product. The fourth technical problem to be solved by the present invention is to propose that the aluminum alloy material is processed into a final component through various surface treatments, stamping and machining methods. The fifth technical problem to be solved by the present invention is to propose the application of the final component.

[0009] The invention relates to a lightweight, high-modulus, high-toughness and corrosion-resistant aluminum alloy material. The aluminum alloy contains: Mg 5.0-7.9wt%, Zn 2.2-4.6wt%, Li 0.5-1.9wt%, and at least one of Mn, Ti, Zr, Sc and Er elements with a total content not exceeding 0.7wt%, and the rest are Al and inevitable impurities, wherein each impurity element is ≤0.25wt% and the total is ≤0.50wt%.

[0010] A first preferred embodiment of the present invention is that the aluminum alloy contains: Mg 5.3~7.8wt%, Zn 2.2~4.5wt%, Li 0.6~1.8wt%, and at least one of Mn, Ti, Zr, Sc, and Er elements with a total content not exceeding 0.6wt%, and the rest is Al and unavoidable impurities, wherein each impurity element is ≤0.20wt% and the total is ≤0.40wt%.

[0011] As a second preferred embodiment of the present invention, the aluminum alloy contains: the aluminum alloy contains: Mg 5.5~7.7wt%, Zn 2.3~4.4wt%, Li 0.6~1.7wt%, and at least one of the elements Mn, Ti, Zr, Sc, and Er with a total content not exceeding 0.5wt%, and the rest are Al and unavoidable impurities.

[0012] As a third preferred embodiment of the present invention, the aluminum alloy contains: Mg 5.8-7.6wt%, Zn 2.5-4.3wt%, and Li 0.7-1.7wt%.

[0013] As a fourth preferred embodiment of the present invention, the aluminum alloy contains: 6.0-7.5wt% Mg, 2.7-4.1wt% Zn, and 0.8-1.7wt% Li.

[0014] As a fifth preferred embodiment of the present invention, the aluminum alloy contains: Li 0.9-1.6 wt %.

[0015] As a sixth preferred embodiment of the present invention, in the aluminum alloy, the contents of Mg, Zn and Li satisfy the relationship: 9.5≤Mg+Zn+Li≤12.6, 1.3≤Mg / Zn≤3.4.

[0016] As a seventh preferred embodiment of the present invention, in the aluminum alloy, the contents of Mg, Zn and Li satisfy the relationship: 10.0≤Mg+Zn+Li≤12.0, 1.4≤Mg / Zn≤2.8.

[0017] As an eighth preferred embodiment of the present invention, in the aluminum alloy, the contents of Mg, Zn and Li satisfy the relationship: 10.2≤Mg+Zn+Li≤11.8, 1.5≤Mg / Zn≤2.6.

[0018] As a ninth preferred embodiment of the present invention, the aluminum alloy contains: Mn 0.15-0.30wt%.

[0019] As a tenth preferred embodiment of the present invention, the aluminum alloy contains: Ti 0.01-0.12wt%.

[0020] As an eleventh preferred embodiment of the present invention, the aluminum alloy contains: Zr 0.06-0.24wt%.

[0021] As a twelfth preferred embodiment of the present invention, the aluminum alloy contains: Sc 0.06-0.24wt%.

[0022] As a thirteenth preferred embodiment of the present invention, the aluminum alloy contains: Er 0.06-0.36wt%.

[0023] As a fourteenth preferred embodiment of the present invention, Sc and Zr elements are added simultaneously to the aluminum alloy, and the sum of the contents of Sc and Zr satisfies: 0.15 wt%≤(Sc+Zr) wt%≤0.30 wt%.

[0024] As a fifteenth preferred embodiment of the present invention, Er and Zr elements are added simultaneously to the aluminum alloy, and the sum of the contents of Er and Zr satisfies: 0.15 wt%≤(Er+Zr) wt%≤0.40 wt%.

[0025] As the sixteenth preferred embodiment of the present invention, the unavoidable impurities contained in the above aluminum alloy include elements unintentionally introduced as impurities in the process of manufacturing the alloy ingot, which need to meet the following requirements: Cu≤0.18wt%, Fe≤0.18wt%, Si≤0.16wt%, other impurity elements each ≤0.15wt%, and the total ≤0.35wt%. Preferably, Cu≤0.15wt%, Fe≤0.15wt%, Si≤0.12wt%, other impurity elements each ≤0.10wt%, and the total ≤0.30wt%. Further preferably, Cu≤0.12wt%, Fe≤0.10wt%, Si≤0.08wt%, other impurity elements each ≤0.05wt%, and the total ≤0.25wt%. Further preferably, Cu≤0.10wt%, Fe≤0.08wt%, Si≤0.06wt%.

[0026] The present invention also relates to a preparation method for producing the above-mentioned aluminum alloy material. The basic preparation process of the aluminum alloy deformation material can be described as "alloy preparation and smelting - semi-continuous casting or spray forming to prepare ingots - homogenization heat treatment of ingots - hot deformation processing - (intermediate annealing) - (cold deformation processing) - solution treatment - (pre-deformation or straightening) - aging treatment - supply of products"; the basic preparation process of the aluminum alloy casting can be described as "alloy preparation and smelting - casting molding of castings - solution treatment - aging treatment - supply of products".

[0027] The method for producing the aluminum alloy deformed material comprises the following steps:

[0028] (1) Manufacturing an ingot of the aluminum alloy material of the present invention;

[0029] (2) performing homogenization heat treatment and / or preheating on the obtained ingot;

[0030] (3) hot deforming the ingot into a desired processed material form, or hot deforming the ingot into a pre-processed material, by one or more hot deformation processing methods selected from extrusion, rolling and forging;

[0031] (4) Reheating the pre-processed material and cold-forming it into the required processed material form;

[0032] (5) performing solution heat treatment on the processed material;

[0033] (6) Rapidly cooling the solution heat treated material to room temperature; and

[0034] (7) The cooled processed material is subjected to natural aging or artificial aging treatment to obtain alloy-aged processed material.

[0035] Wherein, in step (1), the ingot is manufactured by smelting, degassing, removing inclusions and semi-continuous casting or injection molding; during the smelting process, nitrogen or inert gas is used to protect the melt, and the element content is accurately controlled with Mg and Li as the core. Through online component detection and analysis, the ratio between the alloy elements is quickly supplemented and adjusted, and the entire ingot manufacturing process is completed. In a preferred aspect, 0.0002~0.005wt% Be is added in the form of Al-Be intermediate during smelting to change the properties of the oxide film, reduce oxidation burning and inclusions. In another preferred aspect, wherein in step (1), it also includes applying an electromagnetic field, an ultrasonic field or mechanical stirring at or near the crystallizer.

[0036] In step (2), the homogenization heat treatment is performed by a method selected from the following groups: (1) a single-stage homogenization heat treatment in the range of 380-492°C for a total time of 12-54 h; and (2) a double-stage or multi-stage homogenization heat treatment in the range of 395-498°C for a total time of 12-50 h.

[0037] In steps (3) and (4), the preheating temperature and reheating temperature before each hot deformation process are 380-440°C, and the treatment time is 0.1-8 h. In a preferred aspect, the cold deformation process also includes an intermediate annealing treatment of 355-445°C / 0.5-5.5 h.

[0038] In step (5), the solution heat treatment needs to further control the subgrain size and recrystallization structure ratio in the material according to the performance requirements, and is carried out by a method selected from the following group: (1) single-stage, double-stage or multi-stage solution heat treatment in the range of 450-502°C for a total time of 0.5-7.5 h; and (2) continuous temperature rise solution heat treatment in the range of 450-502°C for a total time of 0.5-4.5 h. In a preferred aspect, the continuous temperature rise solution heat treatment is adopted, and the heating rate is ≤60°C / min.

[0039] In step (6), the processed material is rapidly cooled to room temperature using one or a combination of cooling medium spray quenching, immersion quenching and strong wind cooling.

[0040] In step (7), the artificial aging heat treatment is performed by a method selected from the following group: (1) natural aging is performed at room temperature after quenching and cooling, and the time is ≥ 72 h; (2) after quenching and cooling, artificial aging is performed at a temperature in the range of 75-200°C, and the total time is 6-72 h; and (3) after quenching and cooling, a combination of natural aging and artificial aging is performed, and the artificial aging temperature is 75-200°C and the time is 6-72 h.

[0041] Between steps (6) and (7), the following steps may also be included: straightening and / or pre-deforming the cooled processed material, using roller straightening, stretching straightening, stretching bending straightening and a combination thereof to perform straightening to improve the straightness of the processed material, and using stretching, compression and a combination thereof to perform pre-deformation to reduce residual stress formed by quenching and cooling, so as to facilitate subsequent processing and application.

[0042] Through the preparation method of the present invention, the processed material is a profile, wire, rod, pipe, thin plate, thick plate, or forging product.

[0043] The density of the lightweight, high modulus, high toughness and corrosion-resistant aluminum alloy material of the present invention is ≤2.63 g / cm 3 , elastic modulus ≥ 72.0GPa, tensile strength ≥ 450MPa, exfoliation corrosion performance not less than EA grade. The density of the aluminum alloy material is preferably ≤ 2.61g / cm 3 , elastic modulus ≥ 72.5 GPa, tensile strength ≥ 470 MPa, exfoliation corrosion performance not less than EA grade. It is further preferred that the density of the aluminum alloy material is ≤ 2.60 g / cm 3 , elastic modulus ≥73.0GPa, tensile strength ≥500MPa, exfoliation corrosion performance is not lower than PC grade.

[0044] The present invention also relates to a preparation method for producing the aluminum alloy casting, comprising the following steps:

[0045] (1) preparing aluminum alloy castings of the aluminum alloy material by smelting, degassing, removing inclusions, sand mold casting, metal mold casting, or die casting; in the smelting process, nitrogen or inert gas is used to protect the melt, and the element content is accurately controlled with Mg and Li as the core. Through online component detection and analysis, the ratio between the alloy elements is quickly supplemented and adjusted, and the entire casting preparation process is completed;

[0046] (2) subjecting the obtained aluminum alloy casting to a solution heat treatment: including subjecting the aluminum alloy casting to a single-stage, double-stage or multi-stage solution heat treatment at a temperature in the range of 450-502°C for a total time of 0.5-7.5 h, or subjecting the aluminum alloy casting to a continuous temperature rise solution heat treatment at a temperature in the range of 450-502°C for a total time of 0.5-4.5 h;

[0047] (3) The aluminum alloy castings are subjected to natural aging or artificial aging heat treatment; natural aging is carried out at room temperature for ≥ 72 h; artificial aging treatment is carried out in the range of 75~200℃ for a total time of 6~72 h; or a combination of natural aging and artificial aging is used, with the artificial aging temperature being 75~200℃ and the time being 6~72 h.

[0048] The aluminum alloy material of the present invention can be welded with itself or other alloys to form a new product; the welding methods include stir friction welding, fusion welding, brazing, electron beam welding, and laser welding. It can also be processed into a final component through various surface treatments, stamping, and machining; the final component is a load-bearing structural part.

[0049] The beneficial effects of the present invention are:

[0050] (1) By optimizing the composition of Al-Mg-Zn-Li aluminum alloys and using matching preparation methods, high Mg content and Li addition, as well as T-Mg 32 (Al, Zn) 49 The synergistic strengthening of the double aging precipitation sequence of the δ′-Al3Li structural phase significantly improves the alloy's strengthening response ability and effectively avoids the existence of coarse residual phases, so that the material can obtain high strength and toughness while ensuring light weight, and also has good corrosion resistance. The material exhibits excellent comprehensive performance and is an ideal material for various load-bearing structural parts, which can meet the stringent requirements of various high-end manufacturing for lightweight and high-performance aluminum alloy materials.

[0051] (2) The present invention, through the addition of the light element Li, not only introduces a new aging sequence of the δ′-Al3Li structural phase to improve the strength of the Al-Mg-Zn alloy, but also increases the elastic modulus of the alloy and further reduces the density of the alloy, thereby achieving a significant simultaneous improvement in the specific strength and specific stiffness of the alloy, which is beneficial to promoting the development of lightweighting in the fields of aerospace, transportation, automobiles and ships, and has important social and economic benefits.

[0052] (3) The material of the present invention has excellent performance, a simple and practical preparation method, strong operability, is easy to industrialize and promote, and has a promising market prospect. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 This is a TEM morphology photograph of the precipitated phase in the aged state of the 28# alloy in Example 2 of the present invention.

[0054] Figure 2 This is the electron diffraction pattern corresponding to the intracrystalline precipitation of the 28# alloy in the aged state in Example 2 of the present invention.

[0055] Figure 3 The figure shows the comparison of specific strength and fracture toughness between the alloy of the present invention and existing typical alloys.

[0056] Figure 4 The figure is a comparison of the specific strength and corrosion resistance of the alloy of the present invention and existing typical alloys. DETAILED DESCRIPTION

[0057] The technical solution of the present invention is further described in detail below in conjunction with embodiments.

[0058] Example 1

[0059] Alloy extruded plates and strips were prepared on a laboratory scale to demonstrate the principle of the present invention. The composition of the experimental alloy is shown in Table 1. φ230mm round ingots were prepared by alloy smelting, degassing, inclusion removal, and simulating semi-continuous casting conditions known in the industry. During the melting and casting process, a covering agent and argon gas were used to protect the melt. The homogenization heat treatment system of the ingot was selected as (460±5℃ / 24h)+(485±5℃ / 24h), and air-cooled. After peeling, milling, and sawing, an extruded billet with a specification of φ190mm was obtained. The billet was preheated at 400±10℃ for 4h, and a 26×102mm plate and strip was obtained by extrusion deformation. The extrusion temperature was controlled at about 390℃. The extruded strip is loaded into an air furnace at 455℃ and subjected to continuous solution heat treatment at a temperature of 460~490℃ for a total time of 120min. After water quenching, it is immediately subjected to 2.0~2.5% tensile straightening / pre-deformation treatment, and then a double-stage aging treatment of 90±5℃ / 24h+140±5℃ / 22~28h is carried out according to the characteristics of the alloy.

[0060] Samples were cut according to relevant methods, and the density (GB / T 1423), tensile properties (GB / T 16865), elastic modulus (GB / T 3354), fracture toughness (GB / T4161), fatigue properties (GB / T 3075), exfoliation corrosion (GB / T 22639) and intergranular corrosion (GB / T 7998) tests were carried out on the alloy according to relevant test standards, which were used as common performance indicators of the alloy for evaluation. The results are shown in Table 2.

[0061] Table 1 Experimental alloy composition

[0062]

[0063] Note: The elements Li, Cu and Mn with specific values ​​in the table are added elements; those not marked are not added and their contents are controlled as impurity elements.

[0064] Table 2 Performance test results of experimental alloys

[0065]

[0066] It can be seen from Table 2 that alloys 1#, 2#, 3#, 4#, 5#, 6#, 7#, 8#, 9#, 10#, 11#, 12#, 13#, 14#, 15#, 16#, 17#, 18#, 19# and 20# all have a good match of density-strength-plasticity-elastic modulus-fracture toughness-fatigue performance-corrosion resistance: the density does not exceed 2.62 g / cm 3The tensile strength is maintained above 500MPa, the elongation after fracture is higher than 10.0%, the elastic modulus is higher than 73.0GPa, and the fracture toughness is higher than 30.0MPa‧m 1 / 2 level; under the condition of constant stress of 241MPa and strain ratio of 0.1, the fatigue test of 120,000 cycles was passed; the alloy exfoliation corrosion level was not lower than PB level, and the intergranular corrosion level was not lower than level 1. However, the performance of 20#, 21#, 22#, 23#, 24#, 25#, and 26# alloys do not meet the good match of density-strength-plasticity-elastic modulus-fracture toughness-fatigue performance-corrosion resistance. Among them, 21# alloy has a low Zn content and no Li element is added, so its strength and elastic modulus are relatively low, and its density is increased; 22# alloy adds a small amount of Cu and no Li element is added, so its elastic modulus is relatively low, its corrosion resistance is reduced, and its density is increased; 23# alloy adds a higher content of Cu element, so its plasticity, fracture toughness, fatigue performance and corrosion resistance are relatively low, and its density is increased; 24# alloy adds a high content of Li element, so its plasticity, fracture toughness and corrosion resistance are seriously deteriorated; 25# alloy has a low Zn content, so its strength and fracture toughness are relatively low, and its corrosion resistance is reduced; 26# alloy has a low Zn and high Li content, so its strength and fatigue performance are relatively low.

[0067] Example 2

[0068] At the same time, aluminum alloy rolled plates were prepared. The experimental alloy composition is shown in Table 3. Under the conditions of using covering agent and argon gas to protect the melt, 132mm thick ingots were prepared by alloy smelting, degassing, inclusion removal, and simulated semi-continuous casting conditions known in the industry. The ingots were subjected to three-level (400±5℃ / 10h)+(470±5℃ / 12h)+(488±5℃ / 24h) homogenization heat treatment and air cooling. After peeling, milling and sawing, 105mm thick rolled billets were obtained. The billets were preheated at 405±10℃ for 3h, the initial rolling temperature was 400℃, and they were first rolled 4 times along the width direction of the ingot to 65mm, and then intermediate annealing treatment was performed at 405±5℃ / 2h, and then reversed rolling was performed and rolled along the length direction of the ingot to a thickness of about 25mm. The plate was placed in an air furnace at 465°C for solution heat treatment at 465°C / 30min+490°C / 90min. After water quenching, a pre-stretching deformation treatment of 2.1~2.6% was immediately carried out. Subsequently, a double-stage aging treatment of 90±5°C / 24h+140±5°C / 24h was carried out according to the characteristics of the alloy.

[0069] Samples were cut according to relevant methods, and the density (GB / T 1423), tensile properties (GB / T 16865), elastic modulus (GB / T 3354), fracture toughness (GB / T4161), fatigue properties (GB / T 3075), exfoliation corrosion (GB / T 22639) and intergranular corrosion (GB / T 7998) tests were carried out on the alloy according to relevant test standards, which were used as common performance indicators of the alloy for evaluation. The results are shown in Table 4.

[0070] Table 3 Experimental alloy composition

[0071]

[0072] Table 4 Performance test results of experimental alloys

[0073]

[0074] It can be seen from Table 4 that the 27# and 28# alloys of the present invention both exhibit good matching of strength, toughness and corrosion resistance, and are significantly better than the 29# alloy with Cu added. Figure 1 The TEM morphology of the precipitated phase in the 28# alloy is given. Figure 2 Given Figure 1 The corresponding electron diffraction patterns precipitated in the mesocrystal clearly show that T-Mg 32 (Al, Zn) 49 Phase and δ′-Al3Li phase are beneficial for the alloy to obtain high strength, toughness, high elastic modulus and other properties.

[0075] Example 3

[0076] Small-sized aluminum alloy forgings were prepared on the pilot platform, and the alloy composition is shown in Table 5. Under the condition of using covering agent and argon gas to protect the melt, the alloy was smelted, degassed and removed, and the φ425mm round ingot was prepared by injection molding. The homogenization heat treatment system of the ingot was selected as (400±5℃ / 10h)+(470±5℃ / 8h)+(490±5℃ / 24h), and air-cooled. After peeling, milling and sawing, the φ405mm extruded billet was obtained. The billet was preheated at 400±10℃ for 8h, and the φ220mm extruded rod billet was obtained by extrusion deformation, and then a small-sized forging of 50×550×910mm was obtained by multi-sided forging. The extrusion and forging deformation temperature was controlled at 390~405℃. The forgings were placed in an air furnace at 460°C for solution heat treatment at 460°C / 30min+490°C / 120min. After water quenching, a pre-compression deformation treatment of 1.7~2.5% was immediately carried out, followed by a two-stage aging treatment of 90±5°C / 24h+140±5°C / 25h.

[0077] Samples were cut according to relevant methods, and the density (GB / T 1423), tensile properties (GB / T 16865), elastic modulus (GB / T 3354), fracture toughness (GB / T4161), fatigue properties (GB / T 3075), exfoliation corrosion (GB / T 22639) and intergranular corrosion (GB / T 7998) tests were carried out on the alloy according to relevant test standards, which were used as common performance indicators of the alloy for evaluation. The results are shown in Table 6.

[0078] Table 5 Experimental alloy composition

[0079]

[0080] Table 6 Performance test results of experimental alloys

[0081]

[0082] It can be seen from Table 6 that the 30# alloy of the present invention exhibits a good comprehensive performance match of low density, high modulus, high strength and toughness, and corrosion resistance.

[0083] Example 4

[0084] Aluminum alloy castings were prepared in the laboratory, and the alloy composition is shown in Table 7. Through raw material preparation (high-purity aluminum, pure magnesium, pure zinc, pure lithium, Al-Zr master alloy, Al-Ti-B master alloy refiner), mold baking, high-purity aluminum was melted at 740°C, and pure zinc and Al-Zr master alloy were added in the usual order, stirred to make them completely melted; the temperature was lowered to 725°C and Al-Ti-B master alloy was added, stirred and allowed to stand for 4-6 minutes; nitrogen was introduced for melt protection, and when the temperature continued to drop to 715°C, pure magnesium and pure lithium wrapped in aluminum foil were pressed into the aluminum alloy liquid in turn with a bell jar, and stirred to make It is fully melted; then it is degassed and refined, and a furnace inspection is carried out; after standing at a casting temperature of 690°C for 25 minutes, the aluminum alloy melt is poured into a baked metal mold, and the mold temperature is about 175~200°C; the prepared aluminum alloy casting is loaded into a 475°C air furnace, and a solid solution heat treatment of 475±5°C / 12h+495±5°C / 12h is carried out, and after water cooling, it is placed for natural aging for 48h, and then a double-stage aging treatment of 95±5°C / 16h+152±5°C / 20h is carried out.

[0085] Samples were cut according to relevant methods, and the density (GB / T 1423), tensile properties (GB / T 16865), elastic modulus (GB / T 3354), exfoliation corrosion (GB / T22639) and intergranular corrosion (GB / T 7998) tests were carried out on the alloy according to relevant test standards to evaluate the alloy as common performance indicators. The results are shown in Table 8.

[0086] Table 7 Experimental alloy composition

[0087]

[0088] Table 8 Performance test results of experimental alloys

[0089]

[0090] It can be seen from Table 8 that 31# alloy has low density, high strength level, elastic modulus, and good matching of strength, plasticity and corrosion resistance.

[0091] Example 5

[0092] Alloy strips were prepared under industrial conditions, and the composition of the alloy is shown in Table 9. Under the conditions of using covering agent and argon gas to protect the melt, round ingots with a specification of φ482mm were prepared through alloy smelting, degassing, inclusion removal, and semi-continuous casting, which are well known in the industry. The homogenization heat treatment system of 32# and 33# alloy ingots was selected as (400±5℃ / 10h)+(470±5℃ / 12h)+(490±5℃ / 24h), and the other alloys were annealed at their conventional annealing system of 470~505℃ / 40h, air-cooled. After peeling, milling and sawing, an extruded billet with a specification of φ456mm was obtained. The billet was preheated at 430±10℃ for 4h, and a large-size extruded strip of 38×402mm was obtained by extrusion deformation, and the extrusion temperature was controlled at about 390℃±10℃. According to the characteristics of the alloy itself, appropriate process parameters are selected in the range of 450~525℃, and the alloy plates and strips are subjected to solution heat treatment. After water quenching, 1.5~2% tensile straightening treatment is immediately carried out, and then aging treatment is carried out in a typical aging state. 32# and 33# alloys are subjected to a double-stage aging treatment of 90±3℃ / 24h+140±3℃ / 26h, 34# alloy is subjected to a double-stage aging treatment of 121±3℃ / 12h+152±3℃ / 28h, 35# alloy is subjected to an aging treatment of 135±3℃ / 16h, 36# alloy is subjected to a double-stage aging treatment of 121±3℃ / 5h+163±3℃ / 20h, and 37# alloy is subjected to an aging treatment of 190±3℃ / 12h, so that the alloy materials obtain better comprehensive performance matching.

[0093] Samples were cut according to relevant methods, and the density (GB / T 1423), tensile properties (GB / T 16865), fracture toughness (GB / T 4161), fatigue properties (GB / T3075), exfoliation corrosion (GB / T 22639) and intergranular corrosion (GB / T 7998) tests were carried out on the alloy according to relevant test standards, which were used as common performance indicators of the alloy for evaluation. The results are shown in Table 10.

[0094] Table 9 Experimental alloy composition

[0095]

[0096] Note: The specific values ​​of Zn, Li, Cu and Mn in the table are added elements; those not marked are not added and the content is controlled according to the impurity elements. The composition points of 34#, 35#, 36# and 37# are taken from the midline values ​​of the composition range registered by the International Aluminum Association for 2099, 1420, 7050 and 2024 aluminum alloys respectively.

[0097] Table 10 Performance test results of experimental alloys

[0098]

[0099] It can be seen from Table 10 that the 32# and 33# alloys of the present invention have low density, high elastic modulus, good matching of strength, toughness and corrosion resistance; compared with the 2099 alloy (34# alloy) prepared under the same conditions, the alloy of the present invention has better comprehensive performance, higher fracture toughness and corrosion resistance; compared with the 1420 alloy (35# alloy), the alloy of the present invention has better comprehensive performance and higher strength performance; compared with the 7050 alloy (36# alloy) and the 2024 alloy (37# alloy), the alloy of the present invention has obvious comprehensive performance advantages, low density, high elastic modulus, excellent corrosion resistance, and maintains high strength, fracture toughness and fatigue resistance.

[0100] Figure 3 , Figure 4 The comparison of specific strength and fracture toughness, specific modulus and exfoliation corrosion grade of alloys 32#, 33#, 2099 alloy (34# alloy), 1420 alloy (35# alloy), 7050 alloy (36# alloy) and 2024 alloy (37# alloy) of the present invention is given respectively. It can be seen that the alloy products of the present invention show low density and good matching of mechanical properties and corrosion properties.

Claims

1. A lightweight, high modulus, high strength and corrosion resistant aluminum alloy material, characterized in that: The aluminum alloy contains: Mg 5.0-7.9wt%, Zn 2.2-4.6wt%, Li 0.5-1.9wt%, and at least one of Mn, Ti, Zr, Sc, and Er with a total content not exceeding 0.7wt%, and the remainder is Al and unavoidable impurities, wherein Cu is ≤0.18wt%, and other impurity elements are each ≤0.25wt% and the total is ≤0.50wt%; the density of the aluminum alloy material is ≤2.63g / cm 3 , elastic modulus ≥72.0GPa, tensile strength ≥450MPa, exfoliation corrosion performance not lower than EA grade.

2. The lightweight, high modulus, high toughness and corrosion-resistant aluminum alloy material according to claim 1 is characterized in that: The aluminum alloy contains: Mg 5.3~7.8wt%, Zn 2.2~4.5wt%, Li 0.6~1.8wt%, and at least one of Mn, Ti, Zr, Sc, and Er elements with a total content not exceeding 0.6wt%, and the rest is Al and unavoidable impurities, wherein each impurity element is ≤0.20wt% and the total is ≤0.40wt%.

3. The lightweight, high modulus, high toughness and corrosion resistant aluminum alloy material according to claim 2 is characterized in that: The aluminum alloy contains: Mg 5.5-7.7wt%, Zn 2.3-4.4wt%, Li 0.6-1.7wt%, and at least one of Mn, Ti, Zr, Sc, and Er elements with a total content not exceeding 0.5wt%, and the rest is Al and inevitable impurities.

4. The lightweight, high modulus, high strength and corrosion resistant aluminum alloy material according to claim 3 is characterized in that: The aluminum alloy contains Mg 5.8-7.6 wt %, Zn 2.5-4.3 wt %, and Li 0.7-1.7 wt %.

5. The lightweight, high modulus, high strength and toughness corrosion-resistant aluminum alloy material according to claim 4 is characterized in that: The aluminum alloy contains: 6.0-7.5 wt % of Mg, 2.7-4.1 wt % of Zn, and 0.8-1.7 wt % of Li.

6. The lightweight, high modulus, high toughness and corrosion resistant aluminum alloy material according to claim 5, characterized in that: The aluminum alloy contains: Li 0.9~1.6wt%.

7. The lightweight, high modulus, high strength and corrosion resistant aluminum alloy material according to claim 2, characterized in that: In the aluminum alloy, the contents of Mg, Zn and Li satisfy the relationship: 9.5≤Mg+Zn+Li≤12.6, 1.3≤Mg / Zn≤3.

4.

8. The lightweight, high modulus, high strength and toughness corrosion-resistant aluminum alloy material according to claim 7, characterized in that: In the aluminum alloy, the contents of Mg, Zn and Li satisfy the relationship: 10.0≤Mg+Zn+Li≤12.0, 1.4≤Mg / Zn≤2.

8.

9. The lightweight, high modulus, high strength and toughness corrosion-resistant aluminum alloy material according to claim 8, characterized in that: In the aluminum alloy, the contents of Mg, Zn and Li satisfy the relationship: 10.2≤Mg+Zn+Li≤11.8, 1.5≤Mg / Zn≤2.

6.

10. The lightweight, high modulus, high strength and toughness corrosion-resistant aluminum alloy material according to claim 2, characterized in that: The aluminum alloy contains: Mn 0.15-0.30wt%.

11. The lightweight, high modulus, high strength and corrosion resistant aluminum alloy material according to claim 2, characterized in that: The aluminum alloy contains: Ti 0.01-0.12wt%.

12. The lightweight, high modulus, high strength and corrosion resistant aluminum alloy material according to claim 2, characterized in that: The aluminum alloy contains: Zr 0.06-0.24wt%.

13. The lightweight, high modulus, high strength and corrosion resistant aluminum alloy material according to claim 3, characterized in that: The aluminum alloy contains: Sc 0.06-0.24wt%.

14. The lightweight, high modulus, high strength and corrosion resistant aluminum alloy material according to claim 3, characterized in that: The aluminum alloy contains: Er 0.06-0.36wt%.

15. The lightweight, high modulus, high strength and toughness corrosion-resistant aluminum alloy material according to claim 13, characterized in that: In the aluminum alloy, the contents of Sc and Zr satisfy: 0.15 wt%≤(Sc+Zr) wt%≤0.30 wt%.

16. The lightweight, high modulus, high strength and toughness corrosion-resistant aluminum alloy material according to claim 14, characterized in that: In the aluminum alloy, the contents of Er and Zr satisfy: 0.15 wt%≤(Er+Zr) wt%≤0.40 wt%.

17. The lightweight, high modulus, high strength and toughness corrosion-resistant aluminum alloy material according to claim 2, characterized in that: The unavoidable impurities include elements unintentionally introduced as impurities during the process of manufacturing the alloy ingot, wherein Cu≤0.15wt%, Fe≤0.18wt%, Si≤0.16wt%, and other impurity elements are each ≤0.15wt%, and the total is ≤0.35wt%.

18. The lightweight, high modulus, high strength and toughness corrosion-resistant aluminum alloy material according to claim 17, characterized in that: The unavoidable impurities include elements unintentionally introduced as impurities during the process of manufacturing the alloy ingot, wherein Cu≤0.15wt%, Fe≤0.15wt%, Si≤0.12wt%, and other impurity elements are each ≤0.10wt%, and the total is ≤0.30wt%.

19. The lightweight, high modulus, high strength and toughness corrosion-resistant aluminum alloy material according to claim 18, characterized in that: The unavoidable impurities include elements unintentionally introduced as impurities during the process of manufacturing the alloy ingot, wherein Cu≤0.12wt%, Fe≤0.10wt%, Si≤0.08wt%, and other impurity elements are each ≤0.05wt%, and the total is ≤0.25wt%.

20. The lightweight, high modulus, high strength and toughness corrosion-resistant aluminum alloy material according to claim 19, characterized in that: In the aluminum alloy, Cu≤0.10wt%, Fe≤0.08wt%, and Si≤0.06wt%.

21. A method for producing a deformed aluminum alloy material, characterized in that: The following steps are involved: (1) Manufacturing an ingot of the aluminum alloy material according to any one of claims 1 to 20; (2) performing homogenization heat treatment and / or preheating on the obtained ingot; (3) hot deforming the ingot into a desired processed material form, or hot deforming the ingot into a pre-processed material, by one or more hot deformation processing methods selected from extrusion, rolling and forging; (4) Reheating the pre-processed material and cold-forming it into the required processed material form; (5) performing solution heat treatment on the processed material; (6) Rapidly cooling the solution heat treated material to room temperature; and (7) The cooled processed material is subjected to natural aging or artificial aging treatment to obtain alloy-aged processed material.

22. The method according to claim 21, characterized in that In step (1), the ingot is manufactured by smelting, degassing, removing inclusions, and semi-continuous casting or injection molding. During the smelting process, nitrogen or inert gas is used to protect the melt, and the element content is accurately controlled with Mg and Li as the core. Through online component detection and analysis, the ratio between the alloy elements is quickly supplemented and adjusted, and the entire ingot manufacturing process is completed.

23. The method according to claim 22, characterized in that In step (1), 0.0002-0.005 wt% Be is added in the form of Al-Be intermediate during smelting to change the properties of the oxide film and reduce oxidation loss and inclusions.

24. The method according to claim 22, characterized in that In step (1), it also includes applying an electromagnetic field, an ultrasonic field or mechanical stirring at or near the crystallizer.

25. The method according to claim 21, characterized in that In step (2), the homogenization heat treatment is performed by a method selected from the following group: (1) a single-stage homogenization heat treatment at 380-492°C for a total time of 12-54 h; and (2) Double or multi-stage homogenization heat treatment is carried out in the range of 395~498℃ for a total time of 12~50 h.

26. The method according to claim 21, characterized in that In steps (3) and (4), the preheating temperature and reheating temperature before each thermal deformation process are 380-440°C, and the processing time is 0.1-8 h.

27. The method according to claim 21, characterized in that In step (4), the cold deformation passes also include an intermediate annealing treatment of 355~445℃ / 0.5~5.5h.

28. The method according to claim 21, characterized in that In step (5), the solution heat treatment needs to further adjust the subgrain size and recrystallization structure ratio in the material according to the performance requirements, and is performed by a method selected from the following group: (1) Single-stage, double-stage or multi-stage solution heat treatment at 450-502°C for a total time of 0.5-7.5 h; and (2) Carry out continuous temperature rising solution heat treatment in the range of 450~502℃ for a total time of 0.5~4.5 h.

29. The method according to claim 28, characterized in that Continuous heating solution heat treatment is adopted, and the heating rate is ≤60℃ / min.

30. The method according to claim 21, characterized in that In step (6), the processed material is rapidly cooled to room temperature using one or a combination of cooling medium spray quenching, immersion quenching and strong wind cooling.

31. The method according to claim 21, characterized in that In step (7), the artificial aging treatment is performed by a method selected from the following group: (1) After quenching and cooling, natural aging is carried out at room temperature for a time of ≥ 72 h; (2) After quenching and cooling, artificial aging treatment is performed in the range of 75~200℃, with a total time of 6~72 h; and (3) After quenching and cooling, a combination of natural aging and artificial aging is used, with the artificial aging temperature ranging from 75 to 200 °C and the time ranging from 6 to 72 h.

32. The method according to claim 21, characterized in that Between steps (6) and (7), the following steps are also included: straightening and / or pre-deforming the cooled processed material, using roller straightening, stretching straightening, stretching bending straightening and a combination thereof to straighten the material to improve the straightness of the processed material, and using stretching, compression and a combination thereof to pre-deform the material to reduce the residual stress formed by quenching and cooling, so as to facilitate subsequent processing and application.

33. The method according to claim 21, characterized in that The processed material is a profile, wire, bar, pipe, thin plate, thick plate, or forging product.

34. The lightweight, high modulus, high strength and corrosion resistant aluminum alloy material according to claim 1, characterized in that: The density of the aluminum alloy material is ≤2.61g / cm 3 , elastic modulus ≥72.5GPa, tensile strength ≥470MPa, exfoliation corrosion performance not lower than EA grade.

35. The lightweight, high modulus, high strength and toughness corrosion-resistant aluminum alloy material according to claim 34, characterized in that: The density of the aluminum alloy material is ≤2.60g / cm 3 , elastic modulus ≥73.0GPa, tensile strength ≥500MPa, exfoliation corrosion performance is not lower than PC grade.

36. A method for producing a cast aluminum alloy material, characterized in that: The following steps are involved: (1) An aluminum alloy casting of the aluminum alloy material according to any one of claims 1 to 20 is prepared by smelting, degassing, removing inclusions and sand mold casting, or metal mold casting, or die casting; during the smelting process, nitrogen or inert gas is used to protect the melt, and the element content is accurately controlled with Mg and Li as the core. Through online component detection and analysis, the ratio between the alloy elements is quickly supplemented and adjusted, and the entire casting preparation process is completed; (2) subjecting the obtained aluminum alloy casting to a solution heat treatment: including subjecting the aluminum alloy casting to a single-stage, double-stage or multi-stage solution heat treatment at a temperature in the range of 450-502°C for a total time of 0.5-7.5 h, or subjecting the aluminum alloy casting to a continuous temperature rise solution heat treatment at a temperature in the range of 450-502°C for a total time of 0.5-4.5 h; (3) The aluminum alloy castings are subjected to natural aging or artificial aging treatment; natural aging is carried out at room temperature for ≥ 72 h; artificial aging is carried out in the range of 75~200℃ for a total time of 6~72 h; or a combination of natural aging and artificial aging is used, with the artificial aging temperature being 75~200℃ for 6~72 h.

37. A welding product, characterized in that: The product is formed by welding the lightweight, high modulus, high strength and toughness corrosion-resistant aluminum alloy material according to any one of claims 1 to 20, 34 to 35 or the lightweight, high modulus, high strength and toughness corrosion-resistant aluminum alloy material manufactured by the method according to any one of claims 21 to 33, 36 with itself or other alloys; the welding methods include stir friction welding, fusion welding, brazing, electron beam welding, and laser welding.

38. A final component, characterized in that The lightweight, high modulus, high strength and toughness corrosion-resistant aluminum alloy material according to any one of claims 1 to 20, 34 to 35 or the lightweight, high modulus, high strength and toughness corrosion-resistant aluminum alloy material manufactured by the method according to any one of claims 21 to 33, 36 is processed into a final component through various surface treatments, stamping and machining.

39. The final component according to claim 38, characterized in that The final component is a load-bearing structural member.

Citation Information

Patent Citations

  • Aluminum alloy and alloy sheet thereof as well as preparation method of alloy sheet

    CN103866167A

  • High-strength and corrosion-resistant Al-Mg alloy and preparation technology thereof

    CN104152759A

  • High-strength light Al-Mg-Zn alloy

    CN104694800A

  • Al-Mg-Cu-Zn series aluminum alloy and preparation method of aluminum alloy sheet

    CN104862551A

  • High-strength easily-welded Al-Mg-Zn-Cu alloy and preparing method thereof

    CN110541096A