A method for producing high-strength and toughness steel plates for high-rise building structures

By combining low-carbon equivalent design and LF+VD refining with normalizing and tempering heat treatment processes, the problem of high strength and low yield strength ratio of steel plates for high-rise buildings has been solved, and the high strength, toughness and resistance to lamellar tearing performance have been improved, thus meeting the structural requirements of high-rise buildings.

CN118497591BActive Publication Date: 2024-11-05HUNAN VALIN XIANGTAN IRON & STEEL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410984279.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-05
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

Existing steel plates for high-rise buildings cannot simultaneously meet the performance requirements of high strength, low yield strength ratio, resistance to lamellar tearing and easy welding. In particular, steel plates with a tensile strength of 690MPa have deficiencies in terms of composition design and production process.

Method used

The design adopts a low carbon equivalent, controlling low P, low S, low Si, and low B, and adding Nb, V, and Ti microalloying elements. Through LF+VD refining and two-stage controlled rolling combined with normalizing and tempering heat treatment processes, the microstructure type and precipitate morphology are controlled to improve the matrix strength and toughness.

Benefits of technology

The produced steel plates have high strength and toughness, low yield strength ratio and resistance to lamellar tearing, with a yield strength ≥550MPa, tensile strength ≥690MPa, elongation ≥18%, yield strength ratio ≤0.85, impact absorption energy at -20℃ ≥47J, and Z-direction tensile reduction of area ≥35%, making them suitable for high-rise building structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118497591B_ABST
    Figure CN118497591B_ABST
Patent Text Reader

Abstract

A method for producing high-strength and tough steel plates for high-rise building structures belongs to the technical field of low-alloy high-strength steel production. The weight percentage of the steel is C=0.11%~0.13%, Si≤0.15%, Mn=1.20%~1.50%, P≤0.010%, S≤0.002%, Al=0.02%~0.05%, Ni=0.80%~1.0%, Mo=0.20%~0.40%, Ti≤0.005%, Nb=0.02%~0.03%, V=0.12%~0.15%, N=0.01 0%~0.015%, B≤0.0005%, the balance is Fe and inevitable impurity elements; through smelting, refining, continuous casting, controlled rolling and controlled cooling and heat treatment processes, the steel plate produced has high toughness, low yield ratio and good lamellar tear resistance: yield strength ≥550MPa, tensile strength ≥690MPa, elongation ≥18%, yield ratio ≤0.85, -20℃ impact absorption energy ≥47J, Z-direction tensile section shrinkage ≥35%. The method of the present invention can produce extra-thick plates above 150mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of low-alloy high-strength steel production, and in particular relates to a method for producing a high-strength and toughness steel plate for a high-rise building structure. Background Art

[0002] In recent years, with the rapid development of the national economy and the rapid development of urbanization, high-rise buildings have shown a trend of continuous breakthroughs in maximum height, continuous reduction in material and engineering costs, and higher requirements for safety and seismic performance. With the high-rise and large-scale buildings, ordinary tensile strength of 490MPa and 590MPa high-rise building steel can no longer meet the requirements, and tensile strength of 690MPa has become a new trend for high-strength building steel. Usually, for steel plates above 600MPa, quenching and tempering processes are mostly used, and the organization is bainite and martensite, and the yield ratio is generally higher than 0.85. However, for structural steel for high-rise buildings, low yield ratio, resistance to lamellar tearing, and easy welding are very important for the overall safety of the structure. Therefore, in order to achieve a tensile strength of 690MPa and other properties to meet the requirements of building structure steel, innovation and development are needed in terms of component design and production process. Summary of the invention

[0003] The present invention provides a method for producing high-strength and toughness steel plates for high-rise building structures. The produced steel plates have high strength and toughness, low yield strength ratio and resistance to lamellar tearing. At the same time, the steel plates have good weldability: the yield strength of the steel is ≥550MPa, the tensile strength is ≥690MPa, the elongation is ≥18%, the yield strength ratio is ≤0.85, the impact absorption energy at -20°C is ≥47J, and the Z-direction tensile section shrinkage rate is ≥35%.

[0004] The technical solution of the present invention is:

[0005] A method for producing a high-strength and tough steel plate for a high-rise building structure, wherein the weight percentage of the steel is C=0.11%~0.13%, Si≤0.15%, Mn=1.20%~1.50%, P≤0.010%, S≤0.002%, Al=0.02%~0.05%, Ni=0.80%~1.0%, Mo=0.20%~0.40%, Ti≤0.005%, Nb=0.02%~0.03%, V=0.12%~0.15%, N=0.010%~0.015%, B≤0.0005%, the remainder is Fe and unavoidable impurity elements, wherein the carbon equivalent CEV=C+Mn / 6+(Cr+Mo+V) / 5+ (Ni+Cu) / 5≤0.54%; steel yield strength ≥550MPa, tensile strength ≥690MPa, elongation ≥18%, yield strength ratio ≤0.85, -20℃ impact absorption energy ≥47J, Z-direction tensile section shrinkage ≥35%; key process steps include:

[0006] (1) Smelting: Use converter smelting, control the end point P≤0.008%;

[0007] (2) Refining: LF+VD refining is adopted. After LF is heated to 1600℃, ferroniobium and ferrovanadium are added and the temperature of the molten steel is kept above 1600℃ for ≥20min after addition. 1.2~1.6m / t pure Ca wire is fed when LF leaves the station. After VD breaks vacuum, pure Ca wire is fed twice, 0.5~1.0m / t each time, with a time interval of ≥1min. After that, nitrogen wire is fed depending on the nitrogen content in the molten steel.

[0008] (3) Continuous casting: control the superheat to 10~20℃ and the casting speed to 1.8~3 m / min. h ,in h is the thickness of the ingot in m; then the ingot is cooled to room temperature;

[0009] (4) Controlled rolling and controlled cooling: Control the heating temperature to 1230~1250℃; adopt two-stage controlled rolling, the first stage rolling reduction ratio is ≥2.5, the rolling end temperature is ≥1000℃ and the pass reduction rate is ≥15%, the second stage rolling start temperature is ≤920℃, and the end temperature is 820~850℃; after rolling, air cool or cool to room temperature at a cooling rate lower than air cooling;

[0010] (5) Heat treatment: Normalizing temperature is 950~980℃, holding time is (2.5~3.5)min t ; The first tempering temperature is 660~690℃, and the holding time is (0.8~1.2) minutes. t +30; the second tempering temperature is 580~620℃, and the holding time is 2~10h; t The thickness of the steel plate is measured in mm.

[0011] Preferably, step (1) smelting: controlling the amount of slag to be 7% to 9% of the amount of molten iron charged.

[0012] Preferably, in step (2) refining: the molten steel is stirred with bottom blowing nitrogen throughout the LF+VD refining process.

[0013] Preferably, in step (3) continuous casting: the surface of the ingot is cleaned by flame, and the cleaning range includes at least the center of the ingot width and more than 300 mm on both sides.

[0014] Preferably, step (4) controlled rolling and controlled cooling: after rolling, the stack is slowly cooled to room temperature.

[0015] Preferably, in the heat treatment of step (5): air cooling to room temperature after normalizing; and slowly cooling to room temperature after tempering.

[0016] Principle of the invention:

[0017] In terms of composition design, low carbon equivalent control is adopted. At the same time, in order to obtain good comprehensive mechanical properties, low P, low S, low Si, low B, Nb, V, Ti micro-alloying elements and high N content are controlled to finely control the type, quantity, size and distribution of carbonitride precipitation, and more Ni and Mo are added to delay the diffusion phase transformation of supercooled austenite, thereby improving the matrix strength. Higher Ni can also improve α -The toughness of the Fe matrix, the added Mo also contributes to the improvement of strength through precipitation.

[0018] In terms of technology, in order to obtain high-purity, high-homogeneity defect-free ingots and control the appropriate organization type and precipitate morphology, LF+VD and heavy Ca treatment are used in refining, which has obvious effects on obtaining ultra-low S and controlling banded MnS inclusions. Adding ferroniobium and ferrovanadium at a high temperature of the molten steel and allowing enough time for melting after addition can avoid large particles of carbonitrides being retained in the steel. Banded MnS inclusions and large particles of carbonitrides affect the strength and toughness of the steel and seriously deteriorate the lamellar tearing resistance. Continuous casting adopts appropriate superheat and relatively low pulling speed to avoid serious dendrite segregation and surface quality problems in steel billets with high nitrogen content. High-temperature heating is used for rolling, which is conducive to reducing the segregation of the ingot and promoting the full solid solution of carbonitrides. Two-stage controlled rolling is adopted, and large deformation rolling is adopted in the first stage recrystallization zone, in order to prevent the occurrence of mixed crystals and obtain fine and uniform recrystallized grains. Slow cooling after rolling is helpful for sufficient interphase precipitation, which is important for controlling the austenite grain size during subsequent high-temperature and long-time normalizing heat treatment. The heat treatment uses high normalizing temperature and long time, which makes the austenitization sufficient and the C curve of supercooled austenite transformation shifts to the right, thereby obtaining more granular bainite, which has a significant effect on improving the strength of the matrix. Then, two temperings are used, which, on the one hand, make the MA component and cementite transform fully and improve the toughness, and on the other hand, make the precipitation of Mo, Nb, and V sufficient and improve the strength.

[0019] The beneficial effects of the present invention are as follows: 1) The steel plate produced by the method of the present invention has good comprehensive mechanical properties, yield strength ≥550MPa, tensile strength ≥690MPa, elongation ≥18%, yield strength ratio ≤0.85, -20℃ impact absorption energy ≥47J, Z-direction tensile section shrinkage ≥35%, and can meet the stringent requirements of high-rise building structure steel for high strength and toughness, low yield strength ratio, resistance to lamellar tearing and easy welding; 2) The present invention adopts normalizing + tempering + tempering heat treatment process, the steel plate has uniform microstructure and performance, and small thickness effect. Even if extra-thick plates above 150mm are produced, the performance degradation is minimal; 3) The steel plate of the present invention has low residual stress, easy to control plate shape, and can be mass-produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 , Figure 2 , Figure 3 They are metallographic organization diagrams of the steel plate surface, 1 / 4 thickness and 1 / 2 thickness in Example 1 of the present invention respectively. DETAILED DESCRIPTION

[0021] The present invention is further described below with reference to the embodiments and drawings. Example 1

[0022] A method for producing a high-strength and tough steel plate for a high-rise building structure, wherein the steel plate has a thickness of 150 mm, and the weight percentage of the steel is C=0.13%, Si=0.12%, Mn=1.47%, P=0.007%, S=0.001%, Al=0.042%, Ni=0.95%, Mo=0.33%, Ti=0.003%, Nb=0.025%, V=0.146%, N=0.0139%, B=0.0004%, and the remainder is Fe and unavoidable impurity elements, wherein the carbon equivalent CEV=C+Mn / 6+(Cr+Mo+V) / 5+(Ni+Cu) / 5=0.54%; the key process steps include:

[0023] (1) Smelting: Using converter smelting, the amount of slag added is about 8% of the molten iron charge, and the end point P = 0.005%;

[0024] (2) Refining: LF+VD refining is adopted. Nitrogen is blown from the bottom to stir the molten steel during the whole refining process. When the LF temperature rises to 1610℃, ferroniobium and ferrovanadium are added, and then the temperature is continued to rise, and the molten steel temperature is kept above 1600℃ until it leaves the station, and the holding time is ≥20min. When the LF leaves the station, about 1.4m / t pure Ca wire is fed; after the VD vacuum is broken, pure Ca wire is fed twice, 0.8m / t is fed for the first time, and 0.8m / t is fed for the second time, with a time interval of 1min; then 300m nitrogen wire is fed;

[0025] (3) Continuous casting: The superheat during the casting process is 15°C, the pulling speed is 0.45m / min, and the casting is 450mm thick. The casting is then cooled to room temperature and the surface quality is inspected. The surface of the casting is cleaned by flame.

[0026] (4) Controlled rolling and controlled cooling: The heating temperature is 1240°C; two-stage controlled rolling is adopted, the first stage rolling reduction ratio is 2.5, the rolling end temperature is 1132°C and the reduction rate of this pass is 15.6%, the second stage rolling start temperature is 855°C, and the end temperature is 835°C; after rolling, air cooling to room temperature;

[0027] (5) Heat treatment: normalizing temperature is 975℃, holding time is 450min, and air cooling is performed to room temperature after normalizing; the first tempering temperature is 670℃, holding time is 180min, and stacking is slowly cooled to room temperature after tempering; the second tempering temperature is 615℃, holding time is 8h, and stacking is slowly cooled to room temperature after tempering.

[0028] The microstructure of the steel plate of Example 1 was observed. Figure 1 , Figure 2 and Figure 3 They are the metallographic structures on the surface, 1 / 4 thickness and 1 / 2 thickness of the steel plate of Example 1 of the present invention respectively. It can be seen that the structure of the steel plate of Example 1 in the thickness direction is very fine and uniform, mainly granular bainite, and a large number of fine precipitates are dispersed. Example 2

[0029] A method for producing a high-strength and tough steel plate for a high-rise building structure, wherein the steel plate has a thickness of 100 mm, and the weight percentage of the steel is C=0.12%, Si=0.08%, Mn=1.40%, P=0.008%, S=0.001%, Al=0.035%, Ni=0.87%, Mo=0.28%, Ti=0.004%, Nb=0.026%, V=0.13%, N=0.0133%, B=0.0003%, and the remainder is Fe and unavoidable impurity elements, wherein the carbon equivalent CEV=C+Mn / 6+(Cr+Mo+V) / 5+(Ni+Cu) / 5=0.50%; the key process steps include:

[0030] (1) Smelting: Using converter smelting, the amount of slag added is about 7.5% of the molten iron charge, and the end point P = 0.006%;

[0031] (2) Refining: LF+VD refining is adopted. Nitrogen is blown from the bottom to stir the molten steel during the whole refining process. When the LF temperature rises to 1600℃, ferroniobium and ferrovanadium are added, and then the temperature is continued to rise, and the molten steel temperature is kept above 1600℃ until it leaves the station, and the holding time is ≥20min. When the LF leaves the station, about 1.5m / t pure Ca wire is fed; after the VD vacuum is broken, pure Ca wire is fed twice, 0.7m / t is fed for the first time, and 0.7m / t is fed for the second time, with a time interval of 1.2min; then 250m nitrogen wire is fed;

[0032] (3) Continuous casting: The superheat during the casting process is 16-17°C, the pulling speed is 0.7 m / min, and the casting is made into a 350 mm thick billet; then the billet is piled and cooled to room temperature for surface quality inspection, and the center position of the billet width and both sides are cleaned by flame for more than 300 mm;

[0033] (4) Controlled rolling and controlled cooling: The heating temperature is 1245°C; two-stage controlled rolling is adopted, the first stage rolling reduction ratio is 2.5, the rolling end temperature is 1125°C and the pass reduction rate is 18.2%, the second stage rolling start temperature is 860°C, and the end temperature is 842°C; after rolling, air cooling to room temperature;

[0034] (5) Heat treatment: normalizing temperature is 970℃, holding time is 300min, and air cooling is performed to room temperature after normalizing; the first tempering temperature is 675℃, holding time is 120min, and stacking is slowly cooled to room temperature after tempering; the second tempering temperature is 600℃, holding time is 5h, and stacking is slowly cooled to room temperature after tempering. Example 3

[0035] A method for producing a high-strength and tough steel plate for a high-rise building structure, wherein the steel plate has a thickness of 50 mm, and the weight percentage of the steel is C=0.12%, Si=0.10%, Mn=1.25%, P=0.008%, S=0.002%, Al=0.036%, Ni=0.81%, Mo=0.22%, Ti=0.003%, Nb=0.023%, V=0.128%, N=0.0125%, B=0.0003%, and the remainder is Fe and unavoidable impurity elements, wherein the carbon equivalent CEV=C+Mn / 6+(Cr+Mo+V) / 5+ (Ni+Cu) / 5=0.46%; the key process steps include:

[0036] (1) Smelting: converter smelting is adopted, the amount of slag added is about 8.6% of the amount of molten iron charged, and the end point P = 0.006%;

[0037] (2) Refining: LF+VD refining is adopted. Nitrogen is blown from the bottom to stir the molten steel during the whole refining process. When the LF temperature rises to 1600℃, ferroniobium and ferrovanadium are added, and then the temperature is continued to rise, and the molten steel temperature is kept above 1600℃ until it leaves the station, and the holding time is ≥20min. When the LF leaves the station, about 1.5m / t pure Ca wire is fed; after the VD vacuum is broken, pure Ca wire is fed twice, 0.6m / t for the first time and 0.8m / t for the second time, with a time interval of 1min; then 350m nitrogen wire is fed;

[0038] (3) Continuous casting: The superheat during the pouring process is 12~13℃, the pulling speed is 0.8m / min, and the ingot is cast into a 300mm thick ingot; then the ingot is piled and cooled to room temperature for surface quality inspection, and the center position of the ingot width and both sides are cleaned by flame for more than 300mm;

[0039] (4) Controlled rolling and controlled cooling: The heating temperature is 1235°C; two-stage controlled rolling is adopted, the first stage rolling reduction ratio is 2.5, the rolling end temperature is 1080°C and the pass reduction rate is 20.8%, the second stage rolling start temperature is 890°C, and the end temperature is 830°C; after rolling, air cooling to room temperature;

[0040] (5) Heat treatment: normalizing temperature is 960℃, holding time is 150min, and air cooling is performed to room temperature after normalizing; the first tempering temperature is 680℃, holding time is 80min, and stacking is slowly cooled to room temperature after tempering; the second tempering temperature is 590℃, holding time is 3h, and stacking is slowly cooled to room temperature after tempering.

[0041] The mechanical properties of the steel plate of the embodiment are tested, and the results are shown in Table 1. It can be seen that the steel plate of the embodiment has good strength and toughness, low yield strength ratio, and excellent lamellar tear resistance.

[0042] Table 1 Mechanical properties test results of steel plates in the examples

[0043] .

Claims

1. A method for producing high-strength and toughness steel plates for high-rise building structures, characterized in that: The weight percentage of steel is C=0.11%~0.13%, Si≤0.15%, Mn=1.20%~1.50%, P≤0.010%, S≤0.002%, Al=0.02%~0.05%, Ni=0.80%~1.0%, Mo=0.20%~0.40%, Ti≤0.005%, Nb=0.02%~0.03%, V=0.12%~0.15%, N=0.010%~0.015%, B≤0.0005%, the remainder is Fe and unavoidable impurity elements, among which carbon equivalent CEV=C+Mn / 6+(Cr+Mo+V) / 5+ (Ni+Cu) / 5≤0.54%; steel yield strength ≥550MPa, tensile strength ≥690MPa, elongation ≥18%, yield strength ratio ≤0.85, -20℃ impact absorption energy ≥47J, Z-direction tensile section shrinkage ≥35%; The key process steps include: (1) Smelting: Use converter smelting, control the end point P≤0.008%; (2) Refining: LF+VD refining is adopted. After LF is heated to 1600℃, ferroniobium and ferrovanadium are added and the temperature of the molten steel is kept above 1600℃ for ≥20min after addition. 1.2~1.6m / t pure Ca wire is fed when LF leaves the station. After VD breaks vacuum, pure Ca wire is fed twice, 0.5~1.0m / t each time, with a time interval of ≥1min. After that, nitrogen wire is fed depending on the nitrogen content in the molten steel. (3) Continuous casting: control the superheat to 10~20℃ and the casting speed to 1.8~3 m / min. h ,in h is the thickness of the ingot in m; then the ingot is cooled to room temperature; (4) Controlled rolling and controlled cooling: Control the heating temperature to 1230~1250℃; adopt two-stage controlled rolling, the first stage rolling reduction ratio is ≥2.5, the rolling end temperature is ≥1000℃ and the pass reduction rate is ≥15%, the second stage rolling start temperature is ≤920℃, and the end temperature is 820~850℃; after rolling, air cool or cool to room temperature at a cooling rate lower than air cooling; (5) Heat treatment: Normalizing temperature is 950~980℃, holding time is (2.5~3.5)min t ; The first tempering temperature is 660~690℃, and the holding time is (0.8~1.2) minutes. t +30; the second tempering temperature is 580~620℃, and the holding time is 2~10h; t The thickness of the steel plate is measured in mm.

2. The method for producing a high-strength and tough steel plate for high-rise building structure according to claim 1, characterized in that Step (1) Smelting: Control the slag volume to 7% to 9% of the molten iron charge.

3. The method for producing a high-strength and toughness steel plate for high-rise building structure according to claim 1, characterized in that: Step (2) Refining: During the LF+VD refining process, nitrogen is blown from the bottom to stir the molten steel.

4. The method for producing a high-strength and toughness steel plate for high-rise building structure according to claim 1, characterized in that: Step (3) Continuous casting: The surface of the ingot is cleaned by flame, and the cleaning range includes at least the center of the ingot width and more than 300 mm on both sides.

5. The method for producing a high-strength and toughness steel plate for high-rise building structure according to claim 1, characterized in that: Step (4) Controlled rolling and controlled cooling: After rolling, the stack is slowly cooled to room temperature.

6. The method for producing a high-strength and toughness steel plate for high-rise building structure according to claim 1, characterized in that: Step (5) heat treatment: air cooling to room temperature after normalizing; slowly cooling to room temperature after tempering.