A method for preparing wear-resistant coating on extrusion die surface
By preparing composite micropowder and reinforced ceramic micropowder, combined with laser cladding technology, a high-hardness dense coating is formed, which solves the problem of wear and defects of the surface coating of the extrusion mold under high temperature conditions and improves the wear resistance and service life of the mold. , enhancing work stability.
Patent Information
- Application Number
- CN202410954558.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-17
AI Technical Summary
The surface coating of existing extrusion molds is prone to wear and peeling during high-temperature continuous production. The bonding performance, wear resistance and corrosion resistance are insufficient, resulting in short service life and defects such as pores, bubbling, and cracks, which reduces production. efficiency.
The method of preparing composite micropowder, loaded metal clusters, reinforced ceramic micropowder and coating agent is used, and through ultrasonic dispersion, ball milling, ball firing and laser cladding technology, a high-hardness, dense wear-resistant coating is formed to improve the relationship between the coating and the mold matrix. Bonding strength and wear resistance.
Significantly improves the wear resistance, hardness and corrosion resistance of the extrusion die surface, extends the service life, avoids coating defects, enhances working stability under high temperature conditions, and reduces the friction and friction between the aluminum alloy billet and the die. Risk of sticking.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of extrusion die coatings, in particular to a method for preparing a wear-resistant coating on the surface of an extrusion die. Background Art
[0002] In the production process of aluminum alloy products, extrusion process is an important processing method. Generally, the heated aluminum alloy billet is placed into the extrusion die on the extruder. The shape and size of the aluminum alloy profile after extrusion are determined by the predetermined shape and size of the extrusion die. The extruder applies pressure to extrude the aluminum alloy billet out of the die to form the required aluminum alloy profile. The extrusion die plays a key role in the production process of aluminum alloy products.
[0003] Specifically, in the extrusion process of aluminum alloy, the aluminum alloy billet is generally heated to 350℃, and then the aluminum alloy billet is extruded using an aluminum alloy mold to finally obtain an aluminum alloy profile of the desired shape. In order to ensure that the temperature of the alloy does not drop during the extrusion process of the aluminum alloy, it is generally necessary to place the aluminum alloy extrusion mold in a heating furnace in advance for heating and insulation to ensure that the temperature of the extrusion mold is not lower than 380℃ after the extrusion mold is installed on the extruder, thereby ensuring that the temperature of the aluminum alloy does not drop when it enters the extrusion mold, thereby ensuring a good extrusion molding effect on the aluminum alloy billet. In the extrusion process of the profile, due to the great friction between the profile and the mold and the great compressive stress generated on the mold during the extrusion process, in order to ensure the long-term performance of the aluminum alloy extrusion mold, the performance requirements for the aluminum alloy extrusion mold are: at the maximum extrusion working temperature of 400℃, it can still maintain good hardness, wear resistance, and stress deformation resistance. At the same time, during the extrusion process, the outer surface of the aluminum alloy billet and the inner wall of the extrusion die will come into close contact under the action of the extrusion force, so it is also necessary to avoid scratching, adhesion and mutual diffusion between the aluminum alloy billet and the die.
[0004] In order to solve the above technical problems, the prior art provides a coating on the inner wall surface of the extrusion die to reduce the friction between the aluminum alloy billet and the extrusion die, and to avoid mutual scratching, adhesion and mutual diffusion between the aluminum alloy billet and the die. However, in the actual high-temperature continuous production process, the coating on the surface of the existing extrusion die is easy to wear or peel off, the coating cannot effectively protect the die substrate, the effective service life is short, and the bonding performance of the coating with the extrusion die substrate, and the wear resistance, hardness and corrosion resistance of the coating need to be further improved.
[0005] At the same time, the coating is prone to defects such as pores, bubbles, cracks, and uneven thickness during the preparation process of the extrusion die, which will further reduce the long-term working stability of the coating, shorten the service life of the extrusion die, and reduce the extrusion production efficiency.
[0006] Therefore, a method for preparing a wear-resistant coating on the surface of an extrusion die is provided, which reduces the friction between the aluminum alloy billet and the extrusion die, improves the bonding performance between the coating and the extrusion die substrate while avoiding mutual abrasion, adhesion and mutual diffusion between the aluminum alloy billet and the die, and simultaneously improves the wear resistance, hardness and corrosion resistance of the coating, improves the working stability of the extrusion die in the high-temperature continuous production process, and improves its effective service life; and avoids pores, bubbles, cracks, and uneven thickness defects of the coating in the preparation process of the extrusion die, further improving the long-term working stability of the coating, which has important technical significance. Summary of the invention
[0007] In order to solve the technical problems existing in the prior art, the present invention provides a method for preparing a wear-resistant coating on the surface of an extrusion die, which reduces the friction between an aluminum alloy billet and the extrusion die, improves the bonding performance between the coating and the extrusion die substrate while avoiding mutual abrasion, adhesion and mutual diffusion between the aluminum alloy billet and the die, and simultaneously improves the wear resistance, hardness and corrosion resistance of the coating, improves the working stability of the extrusion die in a high-temperature continuous production process, and increases its effective service life; and avoids defects such as pores, bubbles, cracks and uneven thickness of the coating during the preparation process of the extrusion die, and further improves the long-term working stability of the coating.
[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0009] A method for preparing a wear-resistant coating on the surface of an extrusion die comprises the following steps: preparing composite micropowder, loading metal clusters, preparing reinforced ceramic micropowder, preparing a coating agent, and cladding treatment.
[0010] The method for preparing the composite micropowder comprises the following steps: adding nano isostatic graphite micropowder and hexadecyltrimethylammonium bromide into ammonia water with a mass concentration of 1.2-1.5wt%, performing ultrasonic dispersion for 10-20 minutes, stirring and heating to 40-45°C, and maintaining the temperature and stirring for 40-60 minutes to obtain a premixed liquid; adding a first liquid into the premixed liquid under stirring conditions, and controlling the adding time of the first liquid to be 20-35 seconds; after the first liquid is added, stirring and reacting in a closed environment for 4-5 hours, and then stirring Add a second liquid dropwise, and control the drop rate of the second liquid to be 2-2.5 mL / min; after the second liquid is added dropwise, continue stirring for 40-60 min, then stand and age for 22-24 h at 45-50 ° C, centrifuge to obtain a solid, wash the solid with deionized water until it is neutral, transfer it to a drying oven, dry it at 90-100 ° C for 7-9 h, transfer it to a calcining furnace, calcine it at 500-550 ° C for 9-10 h, naturally cool it to room temperature, and grind it to obtain a composite micropowder.
[0011] In the preparation of the composite micropowder, the first liquid is an ethanol solution of tetraethoxysilane; the molar concentration of tetraethoxysilane in the first liquid is 0.2-0.25 mol / L;
[0012] The second liquid is a mixed ethanol solution of tetraethoxysilane and zirconium n-propoxide; the molar concentration of tetraethoxysilane in the second liquid is 1-1.1 mol / L, and the molar concentration of zirconium n-propoxide is 0.15-0.2 mol / L;
[0013] The weight ratio of nano isostatic graphite powder, hexadecyltrimethylammonium bromide, ammonia water, the first liquid and the second liquid is 6-7:1.2-1.4:550-600:10-11:10-11;
[0014] The particle size of nano-isostatic graphite powder is 400-500nm, the anisotropy is 1.03-1.05, and the ash content is 60-70ppm.
[0015] The method for loading metal clusters comprises the following steps: adding nickel nitrate hexahydrate and zirconium oxychloride octahydrate into deionized water, stirring and dissolving, and obtaining a loading liquid; adding composite micropowder into 4-5 times the weight of the loading liquid, ultrasonically dispersing for 10-20 minutes, stirring for 7-8 hours, and standing for 10-12 hours; centrifuging to obtain a solid, transferring the solid into a drying oven, drying at 105-115° C. to constant weight, transferring the solid into a tubular furnace, heat-treating at 420-450° C. for 3-4 hours in a hydrogen atmosphere, and naturally cooling to room temperature to obtain metal cluster loaded micropowder.
[0016] In the loaded metal cluster, the weight ratio of nickel nitrate hexahydrate, zirconium oxychloride octahydrate, and deionized water in the loaded liquid is 22-23:7-7.5:180-190;
[0017] The hydrogen pressure in the tubular furnace is controlled at 0.06-0.08MPa.
[0018] The method for preparing the reinforced ceramic micropowder comprises the following steps: putting composite micropowder, titanium powder, titanium carbide powder, aluminum-vanadium alloy powder and anhydrous ethanol into a ball mill, controlling the ball-to-material ratio to be 8-8.5:1, and the ball milling speed to be 150-200 rpm, and performing ball milling for 10-12 hours, and then transferring the mixture into a vacuum drying oven, and drying the mixture at 110-120° C. for 6-7 hours in a vacuum environment of 0.07-0.08 MPa, and then transferring the mixture into a sintering furnace, and in an argon atmosphere environment, controlling the sintering pressure to be 19-20.5 MPa, and heating the mixture to 1200-1300° C. at a heating rate of 12-15° C. / min, and sintering the mixture for 2.5-3.5 hours at the heating rate, and then naturally cooling the mixture to room temperature, and crushing the mixture to 10-15 μm to obtain the reinforced ceramic micropowder.
[0019] In the preparation of the reinforced ceramic micropowder, the weight ratio of the composite micropowder, titanium powder, titanium carbide powder, aluminum-vanadium alloy powder and anhydrous ethanol is 6.8-7.2:13-13.5:16.5-17.5:11-11.5:24-26.
[0020] The method for preparing the coating agent is to put metal cluster loaded micropowder, reinforced ceramic micropowder, yttrium oxide powder and aluminum silicon alloy powder into a mixer, mix them evenly at 500-600rpm to obtain a premixed powder; and mix the premixed powder evenly with neutral water glass to obtain a coating agent.
[0021] In the coating agent, the weight ratio of metal cluster loaded micropowder, reinforced ceramic micropowder, yttrium oxide powder and aluminum silicon alloy powder is 10-12:25-28:2.5-3:15-17;
[0022] The weight ratio of premixed powder to neutral water glass is 1:4.2-4.6;
[0023] The silicon content of aluminum silicon alloy powder is 11-12wt%;
[0024] The modulus of neutral water glass is 3.1-3.3 and the Baume degree is 44-45°Bé.
[0025] The cladding treatment method is to clean the surface of the extrusion die, then apply the coating agent to the surface of the extrusion die, control the coating thickness of the coating agent to be 0.7-0.8mm, and after the coating is completed, dry it at 100-110°C for 60-90min in an argon atmosphere environment; then, in the argon atmosphere environment, use a transverse flow CO2 laser with a laser wavelength of 10.6μm to perform laser cladding treatment, control the laser output power to be 2500-3000W, the scanning speed to be 4-5mm / s, the spot diameter to be 2-4mm, and the argon gas introduction rate to be 22-25L / min; after the laser cladding treatment is completed, cool it naturally to complete the preparation of the wear-resistant coating on the surface of the extrusion die.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] (1) The method for preparing the wear-resistant coating on the surface of the extrusion die of the present invention comprises the following steps: in the step of preparing the composite micropowder, nano-isostatically pressed graphite micropowder and zirconium silicon nano-micropowder are composited in an in-situ manner to prepare the composite micropowder; the composite micropowder is used as a matrix to load Ni / Zr composite metal clusters in a manner of first loading and then in-situ reduction to prepare metal cluster loaded micropowder; and the composite micropowder is combined with titanium powder, titanium carbide powder, and aluminum-vanadium alloy powder to prepare a mixed powder of titanium-vanadium-aluminum-carbon ceramic and the composite micropowder (i.e., reinforced ceramic micropowder); and then in the step of preparing the composite micropowder, the composite micropowder is composited with the zirconium silicon nano-micropowder to prepare the composite micropowder; .... In the coating agent, metal cluster loaded micropowder, reinforced ceramic micropowder, silicon aluminum alloy and yttrium oxide powder are combined to obtain a premixed powder, and the viscosity is adjusted by water glass to obtain a coating agent; after the coating agent is applied to the surface of the extrusion die, a wear-resistant coating on the surface of the extrusion die is obtained by laser cladding, thereby completing the preparation of the wear-resistant coating on the surface of the extrusion die; wherein, through the high hardness, isotropy and lubrication properties of nano-isostatic graphite micropowder, it is combined with zirconium silicon nano-powder and loaded with Ni / Zr composite metal clusters to obtain metal cluster loaded micropowder, which can During the laser cladding process, it is evenly dispersed in the wear-resistant coating, reacts with the silicon-aluminum alloy at the interface, effectively combines to form hard points, and refines the coating structure. Combined with the promotion effect of the laser cladding process on the density of the coating, while improving the coating hardness, the bonding strength between the coating and the mold substrate, and the wear resistance of the coating, the coating defects are eliminated, the uniformity of the coating thickness is improved, and the friction between the aluminum alloy billet and the extrusion die during the extrusion process is reduced. The mutual scratches, adhesion and mutual diffusion between the aluminum alloy billet and the extrusion die are effectively avoided, the working stability of the extrusion die is improved, and the working stability of the wear-resistant coating in the high-temperature continuous production process is improved; further, the reinforced ceramic micropowder prepared by combining the composite micropowder with the di-titanium vanadium aluminum carbon ceramic is used as the hard phase, and the synergistic effect with other raw materials is used. In the process of laser cladding to form the grain structure, the fine grain strengthening effect is used to further improve the coating hardness, the bonding strength between the coating and the mold substrate, the coating wear resistance and the coating stability, improve the corrosion resistance of the coating, and improve the long-term working stability of the coating.
[0028] (2) The method for preparing the wear-resistant coating on the surface of the extrusion die of the present invention has no defects such as pores, bubbles and cracks, and the hardness of the coating is 1132-1143HV, the porosity of the coating is 0.22-0.25%, the bonding strength between the coating and the substrate is 400-406MPa, the coefficient of variation of the coating thickness is 0.16-0.20, the friction coefficient of the coating surface is 0.309-0.318, and the corrosion potential is -0.373V to -0.363V. The wear-resistant coating can effectively reduce the friction between the aluminum alloy billet and the extrusion die, improve the bonding performance between the coating and the extrusion die substrate, and simultaneously improve the wear resistance, hardness and corrosion resistance of the coating, improve the working stability of the extrusion die in the high-temperature continuous production process, avoid the defects of pores, bubbles, cracks and uneven thickness of the coating in the preparation process of the extrusion die, increase the service life of the extrusion die, and improve the extrusion production efficiency.
[0029] (3) The method for preparing the wear-resistant coating on the surface of the extrusion die of the present invention has a wear rate of 0.063-0.068% after a friction test, which effectively improves the wear resistance of the coating and increases its effective service life.
[0030] (4) According to the method for preparing the wear-resistant coating on the surface of the extrusion die of the present invention, after the extrusion die has been working continuously for 720 hours at a working temperature of 400°C, there is no adhesion or mutual diffusion between the wear-resistant coating of the extrusion die and the aluminum alloy billet, and the wear-resistant coating has no bubbling or crack defects. The friction coefficient of the coating surface can still reach 0.311, and the bonding strength between the coating and the die substrate can still reach 403MPa, which effectively improves the long-term working stability of the extrusion die in the high-temperature continuous production process. DETAILED DESCRIPTION
[0031] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.
[0032] Example 1
[0033] A method for preparing a wear-resistant coating on the surface of an extrusion die, specifically comprising:
[0034] 1. Preparation of composite micropowder
[0035] Nano-isostatic graphite powder and hexadecyltrimethylammonium bromide were put into ammonia water with a mass concentration of 1.2wt%, and after ultrasonic dispersion for 10 minutes, the temperature was raised to 40°C with stirring, and the temperature was kept stirring for 40 minutes to obtain a premixed solution; under stirring, the first liquid was added to the premixed solution, and the addition time of the first liquid was controlled to be 20s; after the first liquid was added, the reaction was stirred for 4 hours in a closed environment, and the second liquid was added dropwise with stirring, and the drop rate of the second liquid was controlled to be 2mL / min; after the second liquid was added dropwise, stirring was continued for 40 minutes, and then the mixture was allowed to stand for aging at 45°C for 22 hours, and a solid was obtained by centrifugation, and the solid was washed with deionized water until it was neutral, transferred to a drying oven, dried at 90°C for 7 hours, transferred to a roasting furnace, roasted at 500°C for 9 hours, naturally cooled to room temperature, and crushed to obtain a composite powder.
[0036] The first liquid is an ethanol solution of tetraethoxysilane; the molar concentration of tetraethoxysilane in the first liquid is 0.2 mol / L.
[0037] The second liquid is a mixed ethanol solution of tetraethoxysilane and zirconium n-propoxide; the molar concentration of tetraethoxysilane in the second liquid is 1 mol / L, and the molar concentration of zirconium n-propoxide is 0.15 mol / L.
[0038] The weight ratio of nano-isostatic graphite powder, hexadecyltrimethylammonium bromide, ammonia water, the first liquid and the second liquid is 6:1.2:550:10:10.
[0039] The particle size of the nano-isostatic graphite powder is 400nm, the anisotropy is 1.03, and the ash content is 60ppm.
[0040] 2. Loading metal clusters
[0041] Nickel nitrate hexahydrate and zirconium oxychloride octahydrate are put into deionized water, stirred to dissolve, and a loading liquid is obtained; the composite micropowder is put into 4 times the weight of the loading liquid, ultrasonically dispersed for 10 minutes, stirred for 7 hours, and allowed to stand for 10 hours; a solid is obtained by centrifugation, and the solid is transferred to a drying oven, dried at 105°C to constant weight, and then transferred to a tubular furnace, heat treated at 420°C for 3 hours in a hydrogen atmosphere, and naturally cooled to room temperature to obtain a metal cluster loaded micropowder.
[0042] The weight ratio of nickel nitrate hexahydrate, zirconium oxychloride octahydrate and deionized water in the loading liquid is 22:7:180.
[0043] The hydrogen pressure in the tubular furnace is controlled at 0.06MPa.
[0044] 3. Preparation of reinforced ceramic powder
[0045] The composite micropowder, titanium powder, titanium carbide powder, aluminum-vanadium alloy powder and anhydrous ethanol are put into a ball mill, the ball-to-material ratio is controlled to be 8:1, the ball mill speed is 150rpm, and after ball milling for 10 hours, the ball is transferred to a vacuum drying oven, and dried at 110°C for 6 hours in a vacuum environment of 0.07MPa. The powder is then transferred to a sintering furnace, and the sintering pressure is controlled to be 19MPa in an argon atmosphere. The temperature is raised to 1200°C at a heating rate of 12°C / min, and the powder is sintered for 2.5 hours at this temperature. The powder is naturally cooled to room temperature and crushed to 10μm to obtain reinforced ceramic micropowder.
[0046] Among them, the weight ratio of composite micropowder, titanium powder, titanium carbide powder, aluminum-vanadium alloy powder and anhydrous ethanol is 6.8:13:16.5:11:24.
[0047] 4. Preparation of coating agent
[0048] Put metal cluster loaded micropowder, reinforced ceramic micropowder, yttrium oxide powder and aluminum silicon alloy powder into a mixer, mix them evenly at 500 rpm to obtain a premixed powder; mix the premixed powder evenly with neutral water glass to obtain a coating agent.
[0049] Among them, the weight ratio of metal cluster loaded micropowder, reinforced ceramic micropowder, yttrium oxide powder and aluminum silicon alloy powder is 10:25:2.5:15.
[0050] The weight ratio of the premixed powder to the neutral water glass is 1:4.2.
[0051] The silicon content of the aluminum silicon alloy powder is 11wt%.
[0052] The modulus of neutral water glass is 3.1 and the Baume degree is 44°Bé.
[0053] 5. Cladding treatment
[0054] Clean the surface of the extrusion die, and then apply the coating agent to the surface of the extrusion die, and control the coating thickness of the coating agent to be 0.7mm. After coating, dry it at 100℃ for 60min in an argon atmosphere. Then, in an argon atmosphere, use a transverse flow CO2 laser with a laser wavelength of 10.6μm for laser cladding treatment. Control the laser output power to 2500W, the scanning speed to 4mm / s, the spot diameter to 2mm, and the argon gas introduction rate to 22L / min. After the laser cladding treatment is completed, cool it naturally to complete the preparation of the wear-resistant coating on the surface of the extrusion die.
[0055] Example 2
[0056] A method for preparing a wear-resistant coating on the surface of an extrusion die, specifically comprising:
[0057] 1. Preparation of composite micropowder
[0058] Nano-isostatic graphite powder and hexadecyltrimethylammonium bromide were put into ammonia water with a mass concentration of 1.3wt%, and after ultrasonic dispersion for 15 minutes, the mixture was stirred and heated to 42°C, and kept stirred for 50 minutes to obtain a premixed solution; under stirring, the first liquid was added to the premixed solution, and the addition time of the first liquid was controlled to be 25s; after the first liquid was added, the mixture was stirred and reacted in a closed environment for 4.5 hours, and then the second liquid was stirred and dripped, and the dripping rate of the second liquid was controlled to be 2.2mL / min; after the second liquid was added, the mixture was stirred for 50 minutes, and then aged at 48°C for 23 hours, and solid matter was obtained by centrifugation, and the solid matter was washed with deionized water until neutral, transferred to a drying oven, dried at 95°C for 8 hours, transferred to a roasting furnace, roasted at 530°C for 9.5 hours, naturally cooled to room temperature, and crushed to obtain a composite powder.
[0059] The first liquid is an ethanol solution of tetraethoxysilane; the molar concentration of tetraethoxysilane in the first liquid is 0.23 mol / L.
[0060] The second liquid is a mixed ethanol solution of tetraethoxysilane and zirconium n-propoxide; the molar concentration of tetraethoxysilane in the second liquid is 1.03 mol / L, and the molar concentration of zirconium n-propoxide is 0.18 mol / L.
[0061] The weight ratio of nano-isostatic graphite powder, hexadecyltrimethylammonium bromide, ammonia water, the first liquid and the second liquid is 6.5:1.3:570:10.6:10.6.
[0062] The particle size of the nano-isostatic graphite powder is 450nm, the anisotropy is 1.04, and the ash content is 65ppm.
[0063] 2. Loading metal clusters
[0064] Nickel nitrate hexahydrate and zirconium oxychloride octahydrate are put into deionized water, stirred to dissolve, and a loading liquid is obtained; the composite micropowder is put into 4.5 times the weight of the loading liquid, ultrasonically dispersed for 15 minutes, stirred for 7.5 hours, and allowed to stand for 11 hours; a solid is obtained by centrifugation, and the solid is transferred to a drying oven, dried at 100°C to constant weight, and then transferred to a tubular furnace, heat treated at 430°C for 3.5 hours in a hydrogen atmosphere, and naturally cooled to room temperature to obtain a metal cluster loaded micropowder.
[0065] The weight ratio of nickel nitrate hexahydrate, zirconium oxychloride octahydrate and deionized water in the loading liquid is 22.5:7.3:185.
[0066] The hydrogen pressure in the tubular furnace is controlled at 0.07MPa.
[0067] 3. Preparation of reinforced ceramic powder
[0068] The composite micropowder, titanium powder, titanium carbide powder, aluminum-vanadium alloy powder and anhydrous ethanol are put into a ball mill, the ball-to-material ratio is controlled to be 8.2:1, the ball mill speed is 180 rpm, and after ball milling for 11 hours, the ball is transferred to a vacuum drying oven, and dried at 115°C for 6.5 hours in a vacuum environment of 0.075 MPa. The powder is then transferred to a sintering furnace, and the sintering pressure is controlled to be 20 MPa in an argon atmosphere environment. The temperature is raised to 1250°C at a heating rate of 14°C / min, and the powder is sintered for 3 hours at this temperature. The powder is naturally cooled to room temperature and crushed to 12 μm to obtain reinforced ceramic micropowder.
[0069] Among them, the weight ratio of composite micropowder, titanium powder, titanium carbide powder, aluminum-vanadium alloy powder and anhydrous ethanol is 7.1:13.2:17:11.3:25.
[0070] 4. Preparation of coating agent
[0071] Put metal cluster loaded micropowder, reinforced ceramic micropowder, yttrium oxide powder and aluminum silicon alloy powder into a mixer, mix them evenly at 550 rpm to obtain a premixed powder; mix the premixed powder evenly with neutral water glass to obtain a coating agent.
[0072] Among them, the weight ratio of metal cluster loaded micropowder, reinforced ceramic micropowder, yttrium oxide powder and aluminum silicon alloy powder is 11:26.5:2.8:16.
[0073] The weight ratio of the premixed powder to the neutral water glass is 1:4.4.
[0074] The silicon content of the aluminum silicon alloy powder is 11.5wt%.
[0075] The modulus of neutral water glass is 3.2 and the Baume degree is 44°Bé.
[0076] 5. Cladding treatment
[0077] Clean the surface of the extrusion die, and then apply the coating agent to the surface of the extrusion die, and control the coating thickness of the coating agent to be 0.75mm. After coating, dry it at 105℃ for 75min in an argon atmosphere. Then, in an argon atmosphere, use a transverse flow CO2 laser with a laser wavelength of 10.6μm for laser cladding treatment. Control the laser output power to 2800W, the scanning speed to 4.5mm / s, the spot diameter to 3mm, and the argon gas introduction rate to 24L / min. After the laser cladding treatment is completed, cool it naturally to complete the preparation of the wear-resistant coating on the surface of the extrusion die.
[0078] Example 3
[0079] A method for preparing a wear-resistant coating on the surface of an extrusion die, specifically comprising:
[0080] 1. Preparation of composite micropowder
[0081] Nano-isostatic graphite powder and hexadecyltrimethylammonium bromide were put into ammonia water with a mass concentration of 1.5wt%, and after ultrasonic dispersion for 20 minutes, the temperature was raised to 45°C with stirring, and the temperature was kept stirring for 60 minutes to obtain a premixed solution; under stirring, the first liquid was added to the premixed solution, and the addition time of the first liquid was controlled to be 35s; after the first liquid was added, the reaction was stirred for 5 hours in a closed environment, and the second liquid was added dropwise with stirring, and the drop rate of the second liquid was controlled to be 2.5mL / min; after the second liquid was added dropwise, stirring was continued for 60 minutes, and then the mixture was allowed to stand for aging at 50°C for 24 hours, and a solid was obtained by centrifugation, and the solid was washed with deionized water until it was neutral, transferred to a drying oven, dried at 100°C for 9 hours, transferred to a roasting furnace, roasted at 550°C for 10 hours, naturally cooled to room temperature, and crushed to obtain a composite powder.
[0082] The first liquid is an ethanol solution of tetraethoxysilane; the molar concentration of tetraethoxysilane in the first liquid is 0.25 mol / L.
[0083] The second liquid is a mixed ethanol solution of tetraethoxysilane and zirconium n-propoxide; the molar concentration of tetraethoxysilane in the second liquid is 1.1 mol / L, and the molar concentration of zirconium n-propoxide is 0.2 mol / L.
[0084] The weight ratio of nano-isostatic graphite powder, hexadecyltrimethylammonium bromide, ammonia water, the first liquid and the second liquid is 7:1.4:600:11:11.
[0085] The particle size of the nano-isostatic graphite powder is 500nm, the anisotropy is 1.05, and the ash content is 70ppm.
[0086] 2. Loading metal clusters
[0087] Nickel nitrate hexahydrate and zirconium oxychloride octahydrate are put into deionized water, stirred to dissolve, and a loading liquid is obtained; the composite micropowder is put into 5 times the weight of the loading liquid, ultrasonically dispersed for 20 minutes, stirred for 8 hours, and allowed to stand for 12 hours; a solid is obtained by centrifugation, and the solid is transferred to a drying oven, dried at 115°C to constant weight, and then transferred to a tubular furnace, heat treated at 450°C for 4 hours in a hydrogen atmosphere, and naturally cooled to room temperature to obtain a metal cluster loaded micropowder.
[0088] The weight ratio of nickel nitrate hexahydrate, zirconium oxychloride octahydrate and deionized water in the loading liquid is 23:7.5:190.
[0089] The hydrogen pressure in the tubular furnace is controlled at 0.08MPa.
[0090] 3. Preparation of reinforced ceramic powder
[0091] The composite micropowder, titanium powder, titanium carbide powder, aluminum-vanadium alloy powder and anhydrous ethanol are put into a ball mill, the ball-to-material ratio is controlled to be 8.5:1, the ball mill speed is 200 rpm, and after ball milling for 12 hours, the ball is transferred to a vacuum drying oven, and dried at 120°C for 7 hours in a vacuum environment of 0.08 MPa. The powder is then transferred to a sintering furnace, and the sintering pressure is controlled to be 20.5 MPa in an argon atmosphere. The temperature is raised to 1300°C at a heating rate of 15°C / min, and the powder is sintered for 3.5 hours at this temperature. The powder is naturally cooled to room temperature and crushed to 15 μm to obtain reinforced ceramic micropowder.
[0092] Among them, the weight ratio of composite micropowder, titanium powder, titanium carbide powder, aluminum-vanadium alloy powder and anhydrous ethanol is 7.2:13.5:17.5:11.5:26.
[0093] 4. Preparation of coating agent
[0094] Put metal cluster loaded micropowder, reinforced ceramic micropowder, yttrium oxide powder and aluminum silicon alloy powder into a mixer, mix them evenly at 600 rpm to obtain premixed powder; mix the premixed powder evenly with neutral water glass to obtain a coating agent.
[0095] Among them, the weight ratio of metal cluster loaded micropowder, reinforced ceramic micropowder, yttrium oxide powder and aluminum silicon alloy powder is 12:28:3:17.
[0096] The weight ratio of the premixed powder to the neutral water glass is 1:4.6.
[0097] The silicon content of the aluminum silicon alloy powder is 12wt%.
[0098] The modulus of neutral water glass is 3.3 and the Baume degree is 45°Bé.
[0099] 5. Cladding treatment
[0100] Clean the surface of the extrusion die, and then apply the coating agent to the surface of the extrusion die, and control the coating thickness of the coating agent to be 0.8 mm. After coating, dry it at 110°C for 90 minutes in an argon atmosphere; then, in an argon atmosphere, use a transverse flow CO2 laser with a laser wavelength of 10.6μm for laser cladding treatment, control the laser output power to 3000W, the scanning speed to 5mm / s, the spot diameter to 4mm, and the argon gas introduction rate to 25L / min; after the laser cladding treatment is completed, cool it naturally to complete the preparation of the wear-resistant coating on the surface of the extrusion die.
[0101] Comparative Example 1
[0102] The technical solution of Example 2 is adopted, but the differences are: 1) in the step of preparing composite micropowder, the addition of nano-isostatic graphite micropowder is omitted; 2) the step of loading metal clusters is omitted, and in the subsequent step of preparing coating agent, composite micropowder is used in equal amount to replace metal cluster loaded micropowder.
[0103] Comparative Example 2
[0104] The technical solution of Example 2 is adopted, but the differences are: 1) in the step of loading metal clusters, the addition of zirconium oxychloride octahydrate is omitted; 2) the step of preparing reinforced ceramic micropowder is omitted, and in the subsequent step of preparing the coating agent, the reinforced ceramic micropowder is replaced by an equal amount of composite micropowder.
[0105] The preparation method of the wear-resistant coating on the surface of the extrusion die of Examples 1-3 and Comparative Examples 1-2 was adopted. After the wear-resistant coating was prepared on the surface of the extrusion die (material 4Cr5MoSiV1), the coating was observed and recorded for pores, bubbles, and cracks. The coating hardness, coating porosity, bonding strength between the coating and the die substrate, coating thickness variation coefficient, coating surface friction coefficient, and coating corrosion resistance were tested.
[0106] Among them, coating hardness test: according to the relevant methods of GB / T7997-2014 "Test method for Vickers hardness of cemented carbide", a Vickers hardness tester is used for testing.
[0107] Coating porosity test: Test according to the relevant methods of GB 17720-1999 "Review of porosity test for metallic coatings".
[0108] Test of bonding strength between coating and mold substrate: According to the dual specimen tensile method in ASTM C633-2001, a universal testing machine is used for testing, and the tensile speed is controlled at 1 mm / min.
[0109] Coating thickness variation coefficient detection: randomly select 10 points within the 20cm×20cm wear-resistant coating range to detect the coating thickness and calculate the coating thickness variation coefficient.
[0110] Coating surface friction coefficient test: Use MFT-4000 material surface performance tester for testing.
[0111] Coating corrosion resistance test: Each wear-resistant coating was cut into test samples of 10cm×10cm×0.5cm, and completely immersed in a hydrochloric acid aqueous solution with a concentration of 1 mol / L. An electrochemical corrosion test was performed using a three-electrode electrochemical cell system to detect the corrosion potential.
[0112] The specific results are shown in the following table:
[0113]
[0114] Furthermore, the wear resistance of the wear-resistant coatings of Examples 1-3 and Comparative Examples 1-2 was tested respectively. Specifically, a friction loss tester was used to conduct friction tests on each wear-resistant coating, the test environment temperature was 25°C, the relative humidity was 60%, the friction method was dry friction, the friction material was GCr15, the friction speed was 200rpm, the friction test force was 500N, and the friction test time was 30min; before the friction test, each wear-resistant coating sample was cleaned, dried, and weighed, recorded as W1; after the friction test, each wear-resistant coating sample was cleaned, dried, and weighed, recorded as W2; and the wear rate was calculated. The calculation method of the wear rate is: [(W1-W2) / W1]×100%.
[0115] The specific results are shown in the following table:
[0116]
[0117] Furthermore, the preparation method of the wear-resistant coating on the surface of the extrusion die of Example 2 and Comparative Example 1-2 was adopted. After the wear-resistant coating was prepared on the surface of the extrusion die (material 4Cr5MoSiV1), each extrusion die was used for continuous aluminum alloy extrusion treatment, and the working temperature of the extrusion die was specifically controlled to be 400°C, the extrusion traction speed was 3.0m / min, and the extrusion speed was 6mm / s; after each extrusion die worked continuously for 720h, it was cooled to observe whether the wear-resistant coating of the extrusion die was adhered to and diffused with the aluminum alloy billet; observe whether the wear-resistant coating of the extrusion die had bubbling and crack defects; and the above-mentioned method was used to detect the surface friction coefficient of the wear-resistant coating of each extrusion die and the bonding strength between the coating and the die substrate. The specific results are shown in the following table:
[0118]
[0119] It can be seen that the preparation method of the wear-resistant coating on the surface of the extrusion die of the present invention comprises the following steps: in the step of preparing the composite micropowder, nano-isostatically pressed graphite micropowder and zirconium silicon nano-micropowder are composited in an in-situ manner to obtain the composite micropowder; the composite micropowder is used as a matrix to load Ni / Zr composite metal clusters in a manner of first loading and then in-situ reduction to obtain metal cluster loaded micropowder; and the composite micropowder is combined with titanium powder, titanium carbide powder and aluminum-vanadium alloy powder to obtain a mixed powder of titanium-vanadium-aluminum-carbon ceramic and the composite micropowder (i.e., reinforced ceramic micropowder); and then In the preparation of the coating agent, metal cluster loaded micropowder, reinforced ceramic micropowder, silicon aluminum alloy and yttrium oxide powder are combined to obtain a premixed powder, and the viscosity is adjusted by water glass to obtain a coating agent; after the coating agent is applied to the surface of the extrusion die, a wear-resistant coating on the surface of the extrusion die is obtained by laser cladding, thereby completing the preparation of the wear-resistant coating on the surface of the extrusion die; wherein, the high hardness, isotropy and lubrication properties of the nano-isostatic graphite micropowder are combined with the zirconium silicon nano-powder and loaded with Ni / Zr composite metal clusters to obtain the metal cluster loaded micropowder, which can It can be evenly dispersed in the wear-resistant coating during the laser cladding process, react with the silicon-aluminum alloy at the interface, effectively combine to form hard points, and refine the coating structure. Combined with the promotion effect of the laser cladding process on the density of the coating, while improving the coating hardness, the bonding strength between the coating and the mold substrate, and the wear resistance of the coating, the coating defects are eliminated, the coating thickness uniformity is improved, and the friction between the aluminum alloy billet and the extrusion die during the extrusion process is reduced. The mutual scratches, adhesion and mutual diffusion between the aluminum alloy billet and the extrusion die are effectively avoided, the working stability of the extrusion die is improved, and the working stability of the wear-resistant coating in the high-temperature continuous production process is improved; further, the reinforced ceramic micropowder prepared by combining the composite micropowder with the di-titanium vanadium aluminum carbon ceramic is enhanced by using the reinforced ceramic micropowder as the hard phase and its synergistic effect with other raw materials. In the process of laser cladding to form the grain structure, the fine grain strengthening effect is used to further improve the coating hardness, the bonding strength between the coating and the mold substrate, the coating wear resistance and the coating stability, improve the coating corrosion resistance, and improve the long-term working stability of the coating.
[0120] In comparative example 1, in the step of preparing composite micropowder, the addition of nano-isostatic graphite micropowder is omitted, and the step of loading metal clusters is omitted. In the subsequent coating preparation, the synergistic improvement effect of nano-isostatic graphite and Ni / Zr composite metal clusters on the wear-resistant coating is lacking, and the improvement effects on the hardness, bonding performance and wear resistance of the coating are all reduced to a certain extent. In addition, the friction between the aluminum alloy billet and the extrusion die during the extrusion process cannot be effectively avoided, and the working stability of the coating in the high-temperature continuous production process is reduced; specifically, the coating hardness, the bonding strength between the coating and the die substrate, the coating surface friction coefficient and its wear resistance show relatively obvious deterioration; and under the working temperature of 400°C, after the extrusion die has worked continuously for 720 hours, the coating surface friction coefficient and the bonding strength between the coating and the die substrate show relatively obvious deterioration, and there is adhesion and mutual diffusion between the extrusion die and the aluminum alloy billet.
[0121] In Comparative Example 2, in the metal cluster loading step, the addition of zirconium oxychloride octahydrate and the addition of reinforcing ceramic micropowder were omitted. Due to the lack of the reinforcing effect of the nickel-based metal clusters and the reinforcing ceramic micropowder on the coating, the coating hardness, the bonding strength between the coating and the mold substrate and its wear resistance were greatly deteriorated, and the working stability in the high-temperature continuous production process was significantly reduced. Under the working temperature of 400°C, after the extrusion die worked continuously for 720 hours, the coating was prone to defects, and the coating surface friction coefficient and the bonding strength between the coating and the mold substrate were significantly deteriorated.
[0122] Unless otherwise specified, all percentages used in the present invention are by mass.
[0123] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a wear-resistant coating on the surface of an extrusion die, characterized in that: The method comprises the following steps: preparing composite micropowder, loading metal clusters, preparing reinforced ceramic micropowder, preparing coating agent, and cladding treatment; The method for preparing the composite micropowder comprises the following steps: adding nano isostatic graphite micropowder and hexadecyltrimethylammonium bromide into ammonia water, dispersing them uniformly, stirring and heating them to 40-45° C., and stirring and keeping the temperature to obtain a premixed liquid; adding a first liquid into the premixed liquid under stirring conditions, and stirring and reacting the premixed liquid in a closed environment after the first liquid is added; then dripping the second liquid into the premixed liquid under stirring conditions, and stirring the premixed liquid after the second liquid is added, and then standing and aging the premixed liquid at a temperature of 45-50° C.; separating and obtaining a solid, and washing and drying the solid, and calcining the solid at 500-550° C. to obtain the composite micropowder; The first liquid is an ethanol solution of tetraethoxysilane, and the second liquid is a mixed ethanol solution of tetraethoxysilane and zirconium n-propoxide; The nano-isostatic graphite powder has a particle size of 400-500 nm, an anisotropy of 1.03-1.05, and an ash content of 60-70 ppm; The metal cluster loading method comprises: adding nickel nitrate hexahydrate and zirconium oxychloride octahydrate into deionized water, stirring and dissolving, and obtaining a loading liquid; adding the composite micropowder into the loading liquid, dispersing it evenly, stirring, and standing; separating and obtaining a solid, and after drying the solid, transferring it into a tubular furnace, heat-treating it at 420-450° C. in a hydrogen atmosphere, and naturally cooling it to room temperature to obtain a metal cluster loading micropowder; The method for preparing the reinforced ceramic micropowder comprises the following steps: uniformly grinding the composite micropowder, titanium powder, titanium carbide powder, aluminum-vanadium alloy powder and anhydrous ethanol, drying the mixture, transferring the mixture into a sintering furnace, controlling the sintering pressure to be 19-20.5 MPa in an argon atmosphere, heating the mixture to 1200-1300° C., sintering the mixture at a heat preservation temperature, naturally cooling the mixture to room temperature, and crushing the mixture to obtain the reinforced ceramic micropowder; The method for preparing the coating agent comprises: uniformly mixing metal cluster loaded micropowder, reinforced ceramic micropowder, yttrium oxide powder and aluminum silicon alloy powder to obtain a premixed powder; uniformly mixing the premixed powder with neutral water glass to obtain a coating agent; The cladding treatment method is to apply a coating agent to the surface of the extrusion die, dry it, and then perform laser cladding treatment to complete the preparation of the wear-resistant coating on the surface of the extrusion die.
2. The method for preparing the wear-resistant coating on the surface of the extrusion die according to claim 1, characterized in that: In the preparation of the composite micropowder, the concentration of ammonia water is 1.2-1.5wt%; The molar concentration of tetraethoxysilane in the first liquid is 0.2-0.25 mol / L; The molar concentration of tetraethoxysilane in the second liquid is 1-1.1 mol / L, and the molar concentration of zirconium n-propoxide is 0.15-0.2 mol / L; The weight ratio of nano-isostatic graphite powder, hexadecyltrimethylammonium bromide, ammonia water, the first liquid and the second liquid is 6-7:1.2-1.4:550-600:10-11:10-11.
3. The method for preparing the wear-resistant coating on the surface of the extrusion die according to claim 1, characterized in that: In the preparation of the composite micropowder, the addition time of the first liquid is controlled to be 20-35s; After the first liquid is added, the reaction is stirred in a closed environment for 4-5 hours.
4. The method for preparing the wear-resistant coating on the surface of the extrusion die according to claim 1, characterized in that: In the preparation of the composite micropowder, the dripping rate of the second liquid is 2-2.5 mL / min; After the second liquid is added, the aging time is 22-24 hours at 45-50°C; The drying temperature is 90-100°C, the drying time is 7-9h, and the roasting time is 9-10h.
5. The method for preparing the wear-resistant coating on the surface of the extrusion die according to claim 1, characterized in that: In the loaded metal cluster, the weight ratio of the composite micropowder to the loaded liquid is 1:4-5; The weight ratio of nickel nitrate hexahydrate, zirconium oxychloride octahydrate and deionized water in the loading liquid is 22-23:7-7.5:180-190.
6. The method for preparing the wear-resistant coating on the surface of the extrusion die according to claim 1, characterized in that: In the loaded metal cluster, the composite micropowder is put into the loading liquid, the stirring time is 7-8 hours, and the standing time is 10-12 hours; Control the hydrogen pressure in the tubular furnace to 0.06-0.08MPa; The heat treatment time at 420-450℃ is 3-4h.
7. The method for preparing the wear-resistant coating on the surface of the extrusion die according to claim 1, characterized in that: In the preparation of the reinforced ceramic micropowder, the weight ratio of the composite micropowder, titanium powder, titanium carbide powder, aluminum-vanadium alloy powder and anhydrous ethanol is 6.8-7.2:13-13.5:16.5-17.5:11-11.5:24-26.
8. The method for preparing the wear-resistant coating on the surface of the extrusion die according to claim 1, characterized in that: In the preparation of the reinforced ceramic powder, the heating rate to 1200-1300° C. is 12-15° C. / min; The heat preservation sintering time is 2.5-3.5h.
9. The method for preparing the wear-resistant coating on the surface of the extrusion die according to claim 1, characterized in that: In the preparation of the coating agent, the weight ratio of the metal cluster loaded micropowder, the reinforced ceramic micropowder, the yttrium oxide powder, and the aluminum silicon alloy powder is 10-12:25-28:2.5-3:15-17; The weight ratio of premixed powder to neutral water glass is 1:4.2-4.6; The silicon content of aluminum silicon alloy powder is 11-12wt%; The modulus of neutral water glass is 3.1-3.3 and the Baume degree is 44-45°Bé.
10. The method for preparing the wear-resistant coating on the surface of the extrusion die according to claim 1, characterized in that: In the cladding process, the coating thickness of the coating agent is controlled to be 0.7-0.8 mm; Laser cladding treatment is carried out in an argon atmosphere environment using a transverse flow CO2 laser with a laser wavelength of 10.6μm; and the laser output power is controlled to be 2500-3000W, the scanning speed is 4-5mm / s, the spot diameter is 2-4mm, and the argon gas introduction rate is 22-25L / min.