Production method of preheating-welding-free NM450 wear-resistant steel plate
By controlling the chemical composition of NM450 wear-resistant steel plate and the rolling heat treatment process, the welding processing difficulties and brittle fracture problems are solved, and high strength and high toughness after preheating are achieved, meeting the needs of various mechanical equipment.
Patent Information
- Application Number
- CN202411005939.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-25
AI Technical Summary
The prior art is difficult to effectively solve the problems of welding processing difficulties and brittle fracture of NM450 grade wear-resistant steel plates, especially in preheating-free welding, which leads to obvious tendency for cold cracks in the material and softening and brittlement of the welding heat-affected zone.
By controlling the chemical composition of the steel plate and strictly rolling heat treatment process, low CEV composition design, quenching + tempering process are adopted, combined with dynamic light pressure or heavy pressure continuous casting technology, the grains are refined, and the strength and toughness of the steel plate are improved, so as to achieve Good strength and toughness after preheating is not allowed.
Production of NM450 wear-resistant steel plate with excellent strength, wear resistance and good welding molding performance, with a surface hardness of 420~480HBW, yield strength ≥1180MPa, and tensile strength ≥1400MPa, meeting the requirements of cold bending and low temperature impact, and no preheating The tensile strength and impact performance of the joints are significantly improved after welding.
Smart Images

Figure CN118910512A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy and relates to a preheat-free welding NM450 wear-resistant steel plate and a production method thereof. Technical Background
[0002] Wear-resistant steel is widely used in various fields such as metallurgy, mining, building materials, and railways. It plays an important role in the key wear parts of equipment such as mining dump trucks, coal mine scraper conveyors, bulldozers, excavators, mixers, and loaders. The service environment of wear-resistant materials is relatively harsh, so they are required to have extremely high strength, hardness, wear resistance, and low-temperature impact toughness to extend the service life of equipment, shorten the replacement cycle of components, and greatly improve the operation time. With the emergence of lightweight and complex design requirements for mechanical equipment, higher requirements are placed on the welding forming performance during the processing and manufacturing of wear-resistant steel, that is, the application equipment of wear-resistant steel has a longer life, and maintenance and downtime caused by maintenance are reduced, thereby reducing capital investment. The higher the hardness of wear-resistant steel, the better the wear resistance, but it also makes welding processing more difficult. 450HB grade wear-resistant steel belongs to the medium-to-high grade wear-resistant variety. Its surface Brinell hardness is between 420 and 480HB. The content of C and alloy elements such as Cr, Mo, and Ni is relatively high in composition design. The carbon equivalent of the steel plate is generally above 0.50%. The problem caused by this is that welding processing is difficult, resulting in a significant tendency for the material to cold crack. In addition, the softening and embrittlement of the welding heat-affected zone can easily lead to brittle fracture of the welded joint.
[0003] In order to avoid such problems, manufacturers usually adopt a combination of increasing the preheating temperature and strictly controlling the welding process; however, preheating before welding will increase energy consumption and cost and greatly reduce the welding processing efficiency. Chinese patent CN114734125B discloses a preheat-free welding method suitable for 500HB wear-resistant steel. The invention is aimed at the preheat-free welding method of 500HB wear-resistant steel plate. Through the groove design of the welding joint, 50kg-level welding wire, 80kg-level welding wire, and wear-resistant steel welding wire are used to form a gradient transition to complete the welding of wear-resistant steel. Compared with traditional wear-resistant steel welding joints, preheating before welding and post-welding heat treatment are not required. The welding process is simpler and higher, and the welding deformation is controllable, which reduces the generation of welding cracks; at the same time, the selection of welding wire with gradient transition strength is more cost-saving than the use of wear-resistant steel welding wire in the whole process. The patent focuses on the matching and welding method of 500HB wear-resistant steel preheat-free welding wire, and is not suitable for preheat-free welding of NM450 wear-resistant steel plate strength level.
[0004] Chinese patent CN116586816A discloses an arc welding rod for preheat-free welding of 1000MPa high-strength steel and a preparation method thereof. The arc welding rod is used to weld 1000MPa-grade high-strength steel, and the strength of the weld joint is not less than 1000MPa. At the same time, it is ensured that no cracks are generated during room temperature welding. The problem of insufficient toughness and strength of the weld joint during welding of 1000MPa-grade ultra-high-strength steel and cracking of the weld during welding is solved. The invention focuses on the arc welding rod for preheat-free welding of 1000MPa high-strength steel and a preparation method thereof, and cannot meet the strength level of preheat-free welding of NM450 wear-resistant steel plates. Summary of the invention
[0005] The object of the present invention is to provide a production method of NM450 wear-resistant steel plate without preheating welding. The produced wear-resistant steel plate is of NM450 grade, with a thickness of 6 to 20 mm, a surface hardness of 420 to 480 HBW, a yield strength of ≥1180 MPa, a tensile strength of ≥1400 MPa, an elongation of ≥16%, and meets 6a diameter 90° cold bending, -40°C impact AKV≥50J, and has good strength and toughness after preheating welding.
[0006] The technical solution of the present invention:
[0007] A method for producing high-strength and high-toughness wear-resistant steel, wherein the chemical composition of the steel is C=0.19%-0.20%, Si=0.25%-0.45%, Mn=1.10%-1.20%, P≤0.012%, S≤0.003%, Cr=0.65%-0.70%, Nb=0.015%-0.020%, Ti=0.008%-0.016%, Al T =0.070%~0.090%, B=0.0014%~0.0020%, H≤0.0015%, N≤0.0050%, O≤0.0015%, the rest is Fe and unavoidable impurities, CEV≤0.54%. The key process steps include:
[0008] (1) Converter smelting: top and bottom double-blowing converter, control the tapping temperature at 1575-1592°C, converter tapping P ≤ 0.012%, add deoxidizer and alloy for deoxidation and alloying during tapping, and use low P alloy to avoid P increase in molten steel;
[0009] (2) Refining: After the molten steel in the ladle is heated by electricity in the LF furnace, the chemical composition is precisely adjusted, and then it enters the RH furnace or VD furnace for vacuum treatment. The gas content of the molten steel is measured at the exit station: H≤0.0015%, N≤0.0050%, and O≤0.0015%;
[0010] (3) Continuous casting: The overheating degree of the tundish is ≤20℃ for continuous casting furnace and ≤25℃ for open casting furnace. Dynamic light pressure reduction or heavy pressure reduction technology is used to improve the internal quality of continuous casting billets. The thickness of continuous casting billets is 180-260mm and the width is 2000-2300mm.
[0011] (4) Heating: preheating section temperature 650 ~ 800 ° C, heating section temperature 1100 ~ 1240 ° C, soaking section temperature 1150 ~ 1230 ° C, furnace time 180 ~ 300 min;
[0012] (5) Rolling: adopt two-stage controlled rolling, the rough rolling temperature is 1150~980℃, the rough rolling cumulative compression ratio is ≥2.2, the intermediate billet thickness is 60~80mm, the 12mm finishing rolling start temperature is ≤960℃, the 20mm finishing rolling start temperature is ≤900℃, the finishing rolling cumulative compression ratio is ≥3.5, and the finishing rolling final rolling temperature is 760~830℃;
[0013] (6) Heat treatment: adopt quenching + tempering process, quenching heating temperature 880 ~ 900 ℃, heating rate 1.6 ~ 2.2 min / mm, holding time 10 ~ 30 min, quenching cooling rate 20 ~ 40 ℃ / s; tempering heating temperature 200 ~ 220 ℃, heating rate 3.5 ~ 4.0 min / mm, holding time 10 ~ 25 min.
[0014] Principle of the invention:
[0015] The wear-resistant steel of the present invention has high strength, high hardness, high toughness at low temperature, good tensile strength and impact resistance after preheating-free welding, and good bending performance. The role and mechanism of the main alloy elements in the chemical composition of the steel of the present invention are described below.
[0016] By controlling the C range, the surface hardness range of the steel plate is guaranteed to meet the target requirements; by adding Mn, B, Si, and Cr elements, the hardenability of the steel plate is improved to ensure uniform structure of the steel plate; by combining structure strengthening with alloy strengthening, the strength performance of the steel plate is improved; by combining the precipitation of Nb, Ti, and Al with a reasonable rolling heat treatment process to refine the grains to achieve the purpose of improving strength, toughness, and hardness; at the same time, the P, S, H, N, and O of the molten steel are strictly controlled. The present invention effectively combines scientific alloy element ratios and reasonable rolling heat treatment processes to ensure that the steel plate has excellent mechanical properties, welding properties, and processing properties. The design reasons for each main added element are as follows:
[0017] Carbon can effectively improve the strength of steel, increase hardenability, and significantly improve the surface hardness of wear-resistant steel plates; however, too much carbon has an adverse effect on the toughness, cold forming and welding properties of steel. Based on the above comprehensive considerations, the carbon content of the present invention is controlled at 0.19% to 0.20%.
[0018] Manganese is the most effective alloying element for improving hardenability. It has a solid solution strengthening effect when dissolved in ferrite. It can also improve the heat treatment performance of steel, refine pearlite grains, and improve the strength and hardness of steel. It is beneficial to add a certain amount of manganese to steel, but the content should not be too high; this is because Mn is an element that is easy to segregate. During the solidification of molten steel, the Mn element will cause the molten steel to aggregate at the end of solidification to form central segregation, resulting in coarse cementite in the core of the steel plate, which is not good for the performance of the core. At the same time, Mn can reduce the martensite transformation temperature in the material. When Mn accumulates in the segregation zone to a certain proportion, high-hardness microstructures such as martensite and bainite will be produced during the cooling process after welding, and the toughness will be significantly reduced. Based on the above comprehensive considerations, the manganese content of the present invention is controlled at 1.10% to 1.20%.
[0019] Silicon is a good reducing agent and deoxidizing agent in the steelmaking process. It is easy to form a solid solution in ferrite, which improves the strength of the steel, especially the yield strength. However, when the Si content is too high, the low-temperature toughness decreases and it also makes it difficult to remove the iron oxide scale on the surface of the steel plate. The Si content of the steel of the present invention is controlled in the range of 0.25-0.45%, which is beneficial to the overall performance.
[0020] Phosphorus has a strong solid solution strengthening effect, which significantly increases the strength and hardness of steel, but phosphorus is an element that easily segregates, increases temper brittleness, and is very detrimental to the low-temperature toughness of steel. Therefore, the phosphorus content in steel should be strictly controlled, and the P content in the steel of the present invention is controlled to be below 0.012%.
[0021] Sulfur is a harmful element in steel and has a tendency to thermal cracking. Sulfide inclusions significantly reduce the toughness of steel, so the S content should be as low as possible. The S content in the steel of the present invention is controlled within 0.003%.
[0022] Niobium has a strong affinity with nitrogen and carbon in steel, and can form extremely stable Nb(C, N) compounds with them. Nb(C, N) particles dispersed along the austenite grain boundaries can greatly increase the coarsening temperature of the original austenite grains, thereby refining the ferrite grains and improving the impact toughness and strength. The Nb content of the present invention is controlled at 0.015% to 0.020%.
[0023] Titanium is a strong carbide-forming element, and has a strong bonding force with carbon and nitrogen. During the solidification of steel, Ti and N produce stable TiN, which can strongly hinder the migration of austenite grain boundaries, thereby refining austenite grains; Ti and C combine to form TiC, which can play a precipitation strengthening role. In the present invention, Ti is controlled at 0.008% to 0.016%.
[0024] Chromium is one of the basic elements of wear-resistant steel, which has the functions of improving hardenability, strengthening the matrix through solid solution, refining grains, improving the strength, hardness and wear resistance of steel, and significantly improving the oxidation resistance of steel and the corrosion resistance of steel. In the present invention, Cr is controlled at 0.65% to 0.70%.
[0025] Aluminum, as a deoxidizer in steel, can play a role in refining grains. In the present invention, Al is controlled at 0.070% to 0.090%.
[0026] Boron is a key element to improve the hardenability of steel plates. Adding a small amount of B (0.0008-0.0030%) to steel can significantly improve hardenability. Therefore, adding a small amount of B to quenched and tempered steel can effectively replace some expensive hardenability alloying elements. However, the B content in wear-resistant steel should not exceed 0.0040%, otherwise it is easy to produce non-solid borides and cause boron embrittlement. The B content of the present invention is controlled at 0.0014%-0.0020%.
[0027] The main innovation of the present invention is: adopting low CEV component design, combining strict controlled rolling process, quenching + low temperature tempering heat treatment process, and performing preheating-free welding process-performance evaluation during the research and development process, and developing preheating-free NM450 wear-resistant steel plate with excellent parent material performance and welding performance. Its beneficial effects: The NM450 wear-resistant steel produced by the method of the present invention has excellent strength, toughness, wear resistance and preheating-free welding forming performance. Its mechanical properties are as follows: surface hardness 420~480HBW, yield strength ≥1120MPa, tensile strength ≥1370MPa, elongation ≥11.5%, meeting 6a diameter 90° cold bending, -40℃ impact AKV ≥32J. The tensile strength of the butt joint after preheat-free welding is ≥780MPa, and the impact energy of the weld, fusion line, and heat-affected zone in the Charpy V-notch test at -5°C are 83J / 75J / 97J, 109J / 94J / 117J, and 138J / 156J / 185J, respectively. The steel plate produced by the method of the present invention can be used for wear-resistant parts and structural parts of excavators, bulldozers, loaders, dump trucks, scraper conveyors, etc. It has excellent mechanical properties and excellent welding formability, and is a promising green steel product. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 , Figure 2 The metallographic structure photos of the steel produced in Example 1 and Example 2 are respectively;
[0029] Figure 3 This is the hardness distribution diagram of the steel plate after preheating-free welding in the example. DETAILED DESCRIPTION
[0030] Embodiment 1:
[0031] A method for producing a preheat-free welding NM450 wear-resistant steel plate, smelting one furnace of NM450 wear-resistant steel to roll a 12 mm thick steel plate, the chemical composition weight percentage of the steel is shown in Table 1; the method includes the following key process steps:
[0032] (1) Converter smelting: The top and bottom combined blowing converter is used for smelting, the tapping temperature is 1581°C, the P content at the converter tapping end point is 0.010%, alloying is performed during the tapping process, deoxidizers such as aluminum iron and aluminum blocks are added, and alloys such as low-carbon ferrochrome and metallic manganese are added;
[0033] (2) Refining: LF furnace is heated and the composition is adjusted. After the composition adjustment, the temperature is raised to 1600°C and the furnace is put into VD furnace for vacuum treatment. The vacuum time is 17 minutes. After the vacuum is broken, the furnace is soft-blown and left for 19 minutes. Samples are taken for testing. H = 0.00012%, N = 0.0031%, O = 0.0011%;
[0034] (3) Continuous casting: The liquidus of molten steel is about 1509°C, the temperature of the tundish is controlled at 1513-1526°C, and the cross-section thickness × width of the ingot is 260 × 2090 mm;
[0035] (4) Heating: The heating system is as follows: preheating section 710°C, heating section 1120-1240°C, soaking section temperature 1170-1219°C, slab out-of-furnace temperature 1230°C, and furnace time 210 min;
[0036] (5) Rolling: Rolling 12*2100mm (thickness*width) specification steel plates, using two-stage controlled rolling, the rolling process parameters are shown in Table 2;
[0037] (6) Heat treatment: quenching heating target temperature 890 °C, single row distribution; tempering heating target temperature 210 °C. Detailed heat treatment parameters are shown in Table 3.
[0038] Preheat-free welding experiment: The specific process parameters of preheat-free welding are shown in Table 4. The mechanical properties test results of the steel plate base material are shown in Table 5; the tensile and impact properties after preheat-free welding are shown in Table 6; the hardness distribution diagram is shown in Table 6. Figure 3 , the test results are shown in Table 7.
[0039] Embodiment 2:
[0040] A method for producing a preheat-free welding NM450 wear-resistant steel plate, smelting one furnace of NM450 wear-resistant steel to roll a 20 mm thick steel plate, the chemical composition weight percentage of the steel is shown in Table 1; the method includes the following key process steps:
[0041] (1) Converter smelting: The top and bottom combined blowing converter is used for smelting, the tapping temperature is 1578°C, the P content at the converter tapping end point is 0.009%, alloying is performed during the tapping process, deoxidizers such as aluminum iron and aluminum blocks are added, and alloys such as low-carbon ferrochrome and metallic manganese are added;
[0042] (2) Refining: LF furnace is heated and the composition is adjusted. After the composition adjustment, the temperature is raised to 1602°C and the furnace is put into VD furnace for vacuum treatment. The vacuum time is 16 minutes. After the vacuum is broken, the furnace is soft-blown and left to stand for 17 minutes. Samples are taken for testing. H = 0.00013%, N = 0.0037%, O = 0.0010%;
[0043] (3) Continuous casting: The liquidus of molten steel is about 1510°C, the temperature of the tundish is controlled at 1517-1528°C, and the cross-section thickness × width of the ingot is 260 × 2090 mm;
[0044] (4) Heating: The heating system is as follows: preheating section 700°C, heating section 1100-1230°C, soaking section temperature 1165-1220°C, slab out-of-furnace temperature 1216°C, and furnace time 238 min;
[0045] (5) Rolling: Rolling 20*2200mm (thickness*width) specification steel plates, using two-stage controlled rolling, the rolling process parameters are shown in Table 2;
[0046] (6) Heat treatment: quenching heating target temperature 890 °C, single row distribution; tempering heating target temperature 210 °C. Detailed heat treatment parameters are shown in Table 3.
[0047] Preheat-free welding experiment: The specific process parameters of preheat-free welding are shown in Table 4. The mechanical properties test results of the steel plate base material are shown in Table 5; the tensile and impact properties after preheat-free welding are shown in Table 6; the hardness distribution diagram is shown in Table 6. Figure 3 , the test results are shown in Table 7.
[0048] Table 1 Chemical composition mass percentage (wt.%)
[0049] Example C Si Mn P S AT Cr Nb Ti B Pc CEV 1 0.20 0.31 1.12 0.010 0.0006 0.077 0.66 0.016 0.016 0.0014 0.31 0.52 2 0.20 0.28 1.13 0.009 0.0016 0.079 0.65 0.018 0.013 0.0018 0.31 0.52
[0050] Table 2 Rolling process parameters
[0051] Example Thickness mm Blank thickness mm Intermediate billet mm Finish rolling start temperature ℃ Finishing rolling temperature℃ 1 12 260 70 950 830 2 20 260 75 890 811
[0052] Table 3 Heat treatment process parameters
[0053]
[0054]
[0055] Table 4 Preheat-free welding process parameters
[0056]
[0057] Table 5 Mechanical properties test results of the parent material of the embodiment
[0058]
[0059] Table 6 Mechanical properties after preheating-free welding
[0060]
[0061] Table 7 Hardness results after preheat-free welding
[0062]
Claims
1. A method for producing NM450 wear-resistant steel without preheating welding, characterized in that: The chemical composition of steel is C=0.19%~0.20%, Si=0.25%~0.45%, Mn=1.10%~1.20%, P≤0.012%, S≤0.003%, Cr=0.65%~0.70%, Nb=0.015%~0.020%, Ti=0.008%~0.016%, Al T =0.070%~0.090%, B=0.0014%~0.0020%, H≤0.0015%, N≤0.0050%, O≤0.0015%, the rest are Fe and unavoidable impurities, CEV≤0.54%; The key process steps include: (1) Converter smelting: top and bottom double-blowing converter, control the tapping temperature at 1575-1592°C, converter tapping P ≤ 0.012%, add deoxidizer and alloy for deoxidation and alloying during tapping, and use low P alloy to avoid P increase in molten steel; (2) Refining: After the molten steel in the ladle is heated by electricity in the LF furnace, the chemical composition is precisely adjusted, and then it enters the RH furnace or VD furnace for vacuum treatment. The gas content of the molten steel is measured at the exit station: H≤0.0015%, N≤0.0050%, and O≤0.0015%; (3) Continuous casting: The overheating degree of the tundish is ≤20℃ for continuous casting furnace and ≤25℃ for open casting furnace. Dynamic light pressure reduction or heavy pressure reduction technology is used to improve the internal quality of continuous casting billets. The thickness of continuous casting billets is 180-260mm and the width is 2000-2300mm. (4) Heating: preheating section temperature 650-800°C, heating section temperature 1100-1240°C, soaking section temperature 1150-1230°C, furnace time 180-300 min; (5) Rolling: adopt two-stage controlled rolling, the rough rolling temperature is 1150~980℃, the rough rolling cumulative compression ratio is ≥2.2, the intermediate billet thickness is 60~80mm, the 12mm finishing rolling start temperature is ≤960℃, the 20mm finishing rolling start temperature is ≤900℃, the finishing rolling cumulative compression ratio is ≥3.5, and the finishing rolling final rolling temperature is 760~830℃; (6) Heat treatment: quenching + tempering process, quenching heating temperature 880 ~ 900 ° C, heating rate 1.6 ~ 2.2 min / mm, holding time 10 ~ 30 min, quenching cooling rate 20 ~ 40 ° C / s; tempering heating temperature 200 ~ 220 ° C, heating rate 3.5 ~ 4.0 min / mm, holding time 10 ~ 25 min, the wear-resistant steel surface hardness 4420 ~ 480 HBW, yield strength ≥ 1180 MPa, tensile strength ≥ 1400 MPa, elongation ≥ 16%, meet 6a diameter 90 ° cold bending, -40 ° C impact AKV ≥ 50 J.
Citation Information
Patent Citations
High-strength and high-toughness NM450 wear-resistant steel plate and production method thereof
CN116926431A
Low-carbon-equivalent high-toughness NM400 wear-resistant steel plate and production method thereof
CN117107155A
Production method of NM450 wear-resistant steel plate with high and low temperature toughness
CN117344198A
Production method of NM400 wear-resistant steel plate
CN117431468A
High-strength and high-toughness marine structural thick plate and production method thereof
CN117987737A
Cited By
High-strength ultralow-temperature toughness steel NM450 and production method thereof
CN120026255A
Preheat-welding-free NM500 wear-resistant steel plate and production method thereof
CN120138505A
Production method of high-toughness NM500 wear-resistant steel plate
CN120843966A
Production method of high-toughness NM450 wear-resistant steel plate
CN120989500A