Rail and method for manufacturing same
The rail composition and controlled cooling method address the challenge of breakage resistance in high axle-load railways by achieving uniform hardness and improved bending characteristics, enhancing rail durability and safety.
Patent Information
- Application Number
- PCT/JP2024/001010
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-01-16
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional rail manufacturing methods face challenges in achieving sufficient breakage resistance at the rail abdomen, particularly in high axle-load railways, due to issues with production efficiency, crack susceptibility, and variations in surface layer hardness, which can lead to increased rail replacement frequencies and potential railway accidents.
A rail composition with specific ranges of C, Si, Mn, Cr, and other elements, combined with controlled cooling rates during hot rolling, to achieve a uniform Vickers hardness and improved three-point bending characteristics, enhancing breakage resistance and fatigue damage resistance.
The solution provides a rail with excellent breakage resistance and fatigue damage resistance, extending the lifespan of rails and preventing railway accidents by ensuring consistent hardness and reduced stress concentration in the rail abdomen.
Smart Images

Figure JP2024001010_03102024_PF_FP_ABST
Abstract
Description
Rail and manufacturing method thereof
[0001] The present invention relates to a rail and a method for manufacturing the same.
[0002] In high-axle-load railways, which are primarily used for transporting ore, the load on the axles of freight cars is much higher than that of passenger cars, and the rails are used in harsh environments. For this reason, steel with a pearlite structure has traditionally been used for the rails, with an emphasis on wear resistance.
[0003] In recent years, efforts have been made to further increase the load weight of freight cars in order to improve the efficiency of rail transport. In addition, the number of wheels passing over the rails has also increased due to the expansion of transport capacity.
[0004] The passage of wheels applies repeated bending stress to the web of outer gauge rails laid in curved sections. As a result, the frequency of rail replacement due to web breakage tends to increase year by year. Therefore, there is a growing demand for rail steel with improved rail web breakage resistance.
[0005] Against this background, various studies have been conducted focusing on the rail web portion. For example, Patent Document 1 discloses a method of rapidly cooling the web portion at a cooling rate of 15°C / sec or more, then stopping the cooling at a temperature of 250 to 450°C, and cooling to the Ms point or below when bainite transformation reaches 30% or more to obtain a martensite structure, thereby forming a tempered martensite structure in the web portion with high toughness.
[0006] Patent document 2 discloses a method for manufacturing rails in which compressive residual stress is imparted by cooling the rail from the top to the upper neck or bottom with high-pressure gas or hydrated gas, thereby improving the fracture resistance of the rail fastening section.
[0007] Patent Document 3 discloses a rail having a predetermined chemical composition, in which 90 area % or more of the metal structure of the cross section of the web portion of the rail is a pearlite structure, the minimum hardness value of the cross section of the web portion of the rail is Hv 300 or more, and the difference between the maximum and minimum hardness values of the cross section of the web portion of the rail is Hv 40 or less, and the rail has excellent fatigue damage resistance in the web portion of the rail.
[0008] Japanese Patent Application Publication No. 62-99438 Japanese Patent Application Publication No. 59-47326 International Publication No. 2020 / 189232
[0009] However, the above-mentioned conventional technologies still have the following problems to be solved. The technology disclosed in Patent Document 1 requires maintaining the temperature until the bainite transformation begins, resulting in low production efficiency. Furthermore, the technology disclosed in Patent Document 2 places the highest priority on achieving the wear resistance and fatigue damage resistance of the head, so the desired crack propagation suppression ability of the abdomen is not necessarily achieved, and depending on the manufacturing conditions, there is a possibility of producing a martensite structure with high crack sensitivity. Furthermore, with the technology described in Patent Document 3, depending on the combination of ingredients and manufacturing conditions, variations in surface hardness may occur, making it difficult to say that the abdominal breakage resistance is sufficient.
[0010] The present invention has been made to advantageously solve the above-mentioned problems, and an object of the present invention is to provide a rail having excellent resistance to breakage of the rail web portion, together with a manufacturing method thereof.
[0011] To solve the above problems, the inventors produced rails with varying contents of C, Si, Mn, and Cr and thoroughly investigated the hardness and three-point bending properties of the rail web portion. As a result, they found that excellent breakage resistance can be obtained by ensuring a certain level of hardness at the web surface and by strictly controlling the hardness variation at that location.
[0012] The present invention is based on the above findings and is summarized as follows: [1] A rail having a chemical composition containing 0.70 to 1.20 mass% C, 0.10 to 1.20 mass% Si, 0.10 to 1.50 mass% Mn, 0.035 mass% or less P, 0.020 mass% or less S, and 0.05 to 1.80 mass% Cr, with the balance being Fe and unavoidable impurities, wherein, when the Vickers hardness at a depth of 0.5 mm from the surface of the rail web portion is measured within a range of ±17.5 mm above and below the center of the rail height, the average Vickers hardness is Hv280 or more with a standard deviation of 5 or less. [2] The rail of [1], wherein the chemical composition further contains at least one selected from the group consisting of V: 0.30% by mass or less, Cu: 1.0% by mass or less, Ni: 1.0% by mass or less, Nb: 0.05% by mass or less, Mo: 2.0% by mass or less, Al: 0.07% by mass or less, W: 1.0% by mass or less, Co: 1.0% by mass or less, B: 0.005% by mass or less, Ti: 0.05% by mass or less, Sb: 0.05% by mass or less, Mg: 0.01% by mass or less, Ca: 0.02% by mass or less, and Sn: 0.05% by mass or less. [3] A rail manufacturing method according to [1] or [2], in which a steel material having the chemical composition according to [1] or [2] is hot-rolled to manufacture a rail, cooling after hot rolling is carried out so that the average cooling rate from a cooling start temperature of 750°C or higher to a cooling stop temperature of 450 to 600°C is 0.4 to 5.0°C / sec at each of the following positions in the rail web: the center position in the rail height, a position 20 mm above the center position in the rail height, and a position 20 mm below the center position in the rail height, and the difference in the average cooling rate at each position is within 0.5°C / sec.
[0013] According to the present invention, it is possible to provide a rail having excellent fatigue breakage resistance in the rail web portion, together with a manufacturing method thereof. The rail of the present invention contributes to extending the service life of rails for high axle load railways and preventing railway accidents, and is industrially useful. The rail manufacturing method of the present invention enables stable manufacturing of the rail of the present invention, and is industrially useful.
[0014] Fig. 1 is a cross-sectional view of a rail. Fig. 2 is a diagram showing the position where test pieces for measuring Vickers hardness of a rail web are taken. Fig. 3 is a schematic diagram showing a method for cooling a rail web. Fig. 4 is a diagram showing the position where test pieces for a three-point bending test of a rail web are taken. Fig. 5 is a diagram explaining the shape of a test piece for a three-point bending test of a rail web.
[0015] <Rail parts> First, the designations of the various rail parts in the present invention will be explained with reference to the rail cross section in Figure 1. In the rail 1 shown in Figure 1, 11 denotes the rail head part, 12 denotes the rail web part, and 13 denotes the rail foot part. Hereinafter, the rail head part, rail web part, and rail foot part may also be referred to as the head part, web part, and foot part, respectively.
[0016] <Composition of Rail> Next, the composition of the steel of the rail of the present invention will be described. In the following description, "%" represents "mass %" unless otherwise specified.
[0017] C: 0.70 to 1.20% C is an essential element for ensuring the strength of the pearlite structure, i.e., breakage resistance. If the C content is less than 0.70%, it is difficult to obtain excellent breakage resistance. Furthermore, if the C content exceeds 1.20%, a large amount of proeutectoid cementite is formed at the austenite grain boundaries during cooling after hot rolling, resulting in a decrease in breakage resistance. Although proeutectoid cementite is present even when the C content is 1.20% or less, the amount formed is so small that its impact on breakage resistance is negligible. For these reasons, the C content is set to the range of 0.70 to 1.20%, preferably 0.70 to 0.89%, and more preferably 0.70 to 0.85%.
[0018] Si: 0.10 to 1.20% In addition to its effect as a deoxidizer, Si contributes to strengthening the pearlite structure by increasing the pearlite equilibrium transformation temperature and reducing lamellar spacing, thereby improving breakage resistance. From this perspective, the Si content must be 0.10% or more. However, if it exceeds 1.20%, bainite and martensite structures are likely to form in the surface layer, promoting hardness variation and resulting in reduced breakage resistance. Furthermore, the increase in Si oxides also deteriorates weldability. For these reasons, the Si content is limited to a range of 0.10 to 1.20%, preferably 0.15 to 1.10%, and more preferably 0.20 to 1.00%.
[0019] Mn: 0.10 to 1.50% Mn is an element that lowers the pearlite transformation temperature and narrows the lamellar spacing, thereby strengthening the pearlite structure and improving breakage resistance. A Mn content of less than 0.10% does not provide sufficient effects. On the other hand, a Mn content of more than 1.50% tends to cause bainite and martensite structures to form in the surface layer, promoting hardness variation and resulting in reduced breakage resistance. Furthermore, because Mn has the effect of shifting the eutectoid point toward the low-C side, excessive addition promotes the formation of pro-eutectoid cementite, resulting in reduced breakage resistance. For these reasons, the Mn content is set to a range of 0.10 to 1.50%, preferably 0.20 to 1.40%, and more preferably 0.30 to 1.30%.
[0020] P: 0.035% or less If P is contained in an amount exceeding 0.035%, breakage resistance and ductility will be deteriorated. Therefore, the P content is set to 0.035% or less, preferably 0.020% or less. The lower limit of the P content is not particularly limited and may be 0%, but industrially it is usually set to more than 0%, and excessively reducing the P content will increase refining costs. From an economical standpoint, it is preferable that the P content be 0.001% or more.
[0021] S: 0.020% or less S is an element present in steel mainly in the form of A-type inclusions. However, if the S content exceeds 0.020%, the amount of these inclusions increases significantly and coarse inclusions form, resulting in deterioration of breakage resistance and ductility. Therefore, the S content is set to 0.020% or less, preferably 0.015% or less, and more preferably 0.010% or less. The lower limit of the S content is not particularly limited and may be 0%, but industrially it is usually set to above 0%, and excessively reducing the S content increases refining costs. From an economic standpoint, it is preferable that the S content be 0.0005% or more.
[0022] Cr: 0.05 to 1.80% Cr is an element that increases the pearlite equilibrium transformation temperature and refines lamellar spacing, thereby strengthening the pearlite structure and improving breakage resistance. A Cr content of less than 0.05% does not provide sufficient effects. On the other hand, a Cr content of more than 1.80% increases the hardenability of the steel and makes it more likely for bainite and martensite structures to form in the surface layer, which increases hardness variation and results in reduced breakage resistance. For these reasons, the Cr content is set to a range of 0.05 to 1.80%, preferably 0.10 to 1.60%, and more preferably 0.15 to 1.40%.
[0023] The chemical composition of the rail used in the present invention may optionally contain, in addition to the above-mentioned essential elements, at least one element selected from the following: V: 0.30 mass% or less, Cu: 1.0 mass% or less, Ni: 1.0 mass% or less, Nb: 0.05 mass% or less, Mo: 2.0 mass% or less, Al: 0.07 mass% or less, W: 1.0 mass% or less, Co: 1.0 mass% or less, B: 0.005 mass% or less, Ti: 0.05 mass% or less, Sb: 0.05 mass% or less, Mg: 0.01 mass% or less, Ca: 0.02 mass% or less, and Sn: 0.05 mass% or less. The reasons for the above-mentioned optional elements are explained below.
[0024] V: 0.30% or less V is an element that forms carbonitrides in steel and disperses and precipitates in the matrix, improving breakage resistance. If the V content exceeds 0.30%, not only does breakage resistance and ductility deteriorate, but alloy costs, i.e., rail manufacturing costs, also increase. For these reasons, when the composition contains V, it is preferable to set the V content upper limit to 0.30%. To achieve the effect of improving breakage resistance, the V content is preferably 0.001% or more. A more preferable range for the V content is 0.001 to 0.15%.
[0025] Cu: 1.0% or less Like Cr, Cu is an element that can further increase the strength of steel through solid solution strengthening. If the Cu content exceeds 1.0%, Cu cracking is more likely to occur, so if the composition contains Cu, the Cu content is preferably 1.0% or less. A more preferred range for the Cu content is 0.001 to 0.5%.
[0026] Ni: 1.0% or less Ni is an element that can increase the strength of steel without degrading ductility. Furthermore, adding Ni in combination with Cu can suppress Cu cracking, so it is desirable to also include Ni when the composition contains Cu. However, if the Ni content exceeds 1.0%, the hardenability of the steel increases, the amount of martensite and bainite formed increases, and breakage resistance decreases. For these reasons, if the composition contains Ni, the Ni content is preferably 1.0% or less. A more preferred range for the Ni content is 0.001 to 0.5%.
[0027] Nb: 0.05% or less Nb combines with C in the steel during and after hot rolling to form a rail, precipitating as carbides. This effectively refines the pearlite colony size, significantly improving breakage resistance, wear resistance, fatigue damage resistance, and ductility, thereby significantly contributing to extending the service life of the rail. However, even if the Nb content exceeds 0.05%, the improvement in each property saturates, and no effect commensurate with the increase in content is obtained. For these reasons, when the composition contains Nb, the upper limit of the Nb content is preferably 0.05%. To obtain a sufficient effect on extending the service life of the rail, the Nb content is preferably 0.001% or more. A more preferred range of Nb content is 0.001 to 0.03%.
[0028] Mo: 2.0% or less Mo is an element that can further increase the strength of steel through solid solution strengthening. Mo also has the effect of shifting the eutectoid point toward the high-C side, thereby suppressing the formation of pro-eutectoid cementite. However, if the Mo content exceeds 2.0%, the amount of bainite formed in the steel increases, resulting in a decrease in breakage resistance. For these reasons, if the composition contains Mo, the Mo content is preferably 2.0% or less. From the viewpoint of increasing strength, the Mo content is preferably 0.001% or more. A more preferred range of Mo content is 0.001 to 1.0%.
[0029] Al: 0.07% or less Al is an element that can be added as a deoxidizer. If the Al content exceeds 0.07%, the high bonding strength of Al with oxygen causes the formation of large amounts of oxide-based inclusions in the steel, resulting in a decrease in the steel's breakage resistance and ductility. Therefore, if the composition contains Al, the Al content is preferably 0.07% or less. There is no particular lower limit for the Al content, but for deoxidation purposes, it is preferably 0.001% or more. A more preferred range for the Al content is 0.001 to 0.03%.
[0030] W: 1.0% or less W is an element that precipitates as carbides during and after hot rolling to form the rail shape, improving the strength and breakage resistance of the rail through precipitation strengthening. If the W content exceeds 1.0%, martensite forms in the steel, resulting in a decrease in breakage resistance. For these reasons, if the composition contains W, the W content is preferably 1.0% or less. There is no particular lower limit for the W content, but to achieve the aforementioned effect of improving strength and breakage resistance, a W content of 0.001% or more is preferred. A more preferred range for the W content is 0.001 to 0.5%.
[0031] Co: 1.0% or less Co is an element that can further increase the strength of steel by increasing the pearlite equilibrium transformation temperature and reducing lamellar spacing. Co also has the effect of suppressing the precipitation of proeutectoid cementite. If the Co content exceeds 1.0%, martensite forms in the steel, resulting in a decrease in breakage resistance. For these reasons, if the composition contains Co, the Co content is preferably 1.0% or less. There is no particular lower limit for the Co content, but for high strength, it is preferably 0.001% or more. A more preferred range of Co content is 0.001 to 0.5%.
[0032] B: 0.005% or less B is an element that precipitates as a nitride in steel during and after hot rolling to form a rail shape, improving the strength and breakage resistance of the steel through precipitation strengthening. If the B content exceeds 0.005%, martensite is formed, resulting in a decrease in breakage resistance. For these reasons, if the composition contains B, the B content is preferably 0.005% or less. There is no particular lower limit for the B content, but in order to achieve the effect of improving the strength and breakage resistance described above, it is preferably 0.001% or more. The B content is more preferably 0.001 to 0.003%.
[0033] Ti: 0.05% or less Ti precipitates in steel as carbides, nitrides, or carbonitrides during and after hot rolling to form a rail shape, improving the strength and breakage resistance of the steel through precipitation strengthening. If the Ti content exceeds 0.05%, coarse carbides, nitrides, or carbonitrides are formed, resulting in reduced breakage resistance. For these reasons, if the composition contains Ti, the Ti content is preferably 0.05% or less. While there is no particular lower limit for the Ti content, a Ti content of 0.001% or more is preferred to achieve the aforementioned effect of improving strength and breakage resistance. A more preferred range of Ti content is 0.001 to 0.03%.
[0034] Sb: 0.05% or less Sb is an element that has a significant effect of preventing decarburization of steel during reheating of rail steel material in a heating furnace before hot rolling. If the Sb content exceeds 0.05%, it adversely affects breakage resistance and toughness. Therefore, if the composition contains Sb, the Sb content is preferably 0.05% or less. While there is no particular lower limit for the Sb content, a content of 0.001% or more is preferred to achieve the effect of reducing the decarburized layer. A more preferred range of Sb content is 0.001 to 0.03%.
[0035] Mg: 0.01% or less Mg is an element that combines with oxygen to precipitate MgO, further increasing strength. If the Mg content exceeds 0.01%, the increase in MgO has a negative effect on the breakage resistance and toughness of the steel. Therefore, if the composition contains Mg, the Mg content is preferably 0.01% or less. There is no particular lower limit for the Mg content, but in order to achieve the above-mentioned strength-improving effect, it is preferably 0.001% or more. A more preferred range for the Mg content is 0.001 to 0.005%.
[0036] Ca: 0.02% or less Ca is an element that combines with oxygen to precipitate CaO, further increasing strength. If the Ca content exceeds 0.02%, the increase in CaO has a negative effect on the breakage resistance and toughness of the steel. Therefore, if the composition contains Ca, the Ca content is preferably 0.02% or less. There is no particular lower limit for the Ca content, but in order to achieve the above-mentioned strength-improving effect, it is preferably 0.001% or more. A more preferred range of Ca content is 0.001 to 0.01%.
[0037] Sn: 0.05% or less Sn is an element that has a significant effect of preventing decarburization of steel during reheating of rail steel material in a heating furnace before hot rolling. Sn content exceeding 0.05% adversely affects the ductility and toughness of steel, so if the composition contains Sn, the Sn content is preferably 0.05% or less. While there is no particular lower limit for the Sn content, a value of 0.001% or more is preferred to achieve the effect of reducing the decarburized layer. A more preferred range of Sn content is 0.001 to 0.01%.
[0038] The chemical composition of the steel for rails of the present invention, other than the above-mentioned essential and optional elements, consists of Fe and unavoidable impurities. Examples of unavoidable impurities include N and O, with N content up to 0.008% and O content up to 0.004%. Depending on the raw materials, resources, and manufacturing equipment, impurities other than N and O may be unavoidably mixed into the steel. Examples of raw materials include iron ore, reduced iron, and scrap. The above impurities are also acceptable as long as they do not impair the objectives of the present invention. Examples of impurities other than N and O include Pb, Zr, Bi, Zn, Se, As, Te, Tl, Cd, Hf, Ag, Hg, Ga, Ge, and REM.
[0039] <Rail Microstructure> The rail of the present invention is a pearlitic rail, and the rail microstructure is pearlite in an area ratio of 95% or more. The remaining structure other than pearlite is permissible as long as its total area ratio is 5% or less, since it does not significantly affect the fatigue crack propagation resistance. Examples of the remaining structure include ferrite, pro-eutectoid cementite, bainite, and martensite.
[0040] <Vickers hardness> In the present invention, it is not sufficient for the chemical composition to simply satisfy the above-mentioned ranges. To obtain excellent breakage resistance in the web portion, it is important to control the Vickers hardness Hv at a depth of 0.5 mm from the surface of the rail web portion within a range of 17.5 mm above and below the center of the rail height (a total range of 35 mm) within a specified range. In other words, the average Vickers hardness of the above-mentioned locations should be 280 or more, with its standard deviation not exceeding 5. To stably improve breakage resistance, it is preferable that the average Vickers hardness of the above-mentioned locations be 300 Hv or more, with a standard deviation not exceeding 4.
[0041] In Figure 2, the rail height is represented by the length A from the bottom of the foot to the top of the rail, and the center position of the rail height is the center position of the rail height A (position A / 2). The range of 17.5 mm above and below the center position of the rail height (a total range of 35 mm) is within the shaded area in Figure 2. The Vickers hardness of the present invention can be measured, for example, with a pressing load of 98 N at a position 0.5 mm deep from the surface of the relevant location, within the range of 17.5 mm above and below the center position of the rail height (a total range of 35 mm), at 1 mm intervals from the top to the bottom of the rail.
[0042] The reason for setting the hardness within the range of 17.5 mm above and below the center position of the rail height (a range of 35 mm in total) as the specified range is as follows.
[0043] As mentioned above, repeated bending stress is applied to the web of an outer gauge rail laid in a curved section. Meanwhile, roll marks or markings are provided within a vertical range of 17.5 mm from the center of the rail height on the web of the rail. The inventors have discovered that when bending stress is applied, a portion of the roll mark or marking becomes a stress concentration source, causing breakage from this area. Based on this finding, the present invention controls the hardness of the rail web within a predetermined range within a vertical range of 17.5 mm from the center of the rail height.
[0044] In this way, by strengthening the pearlite structure in the rail web portion and strictly controlling the variation in hardness in the surface layer of the rail web portion, it becomes possible to suppress stress concentration in locally softened areas, significantly improving the breakage resistance of the rail web portion. Excellent breakage resistance in the rail web portion is a characteristic generally required of rails, and is effective in extending the service life and preventing railway accidents for rails used in straight sections and rails without roll marks or stamps on the rail web portion, for example.
[0045] <Rail Shape> The shape of the rail in the present invention is not particularly limited, and may be any of the rail shapes described in JIS E 1101:2001, BS EN13674-1:2011, American Railway Engineering and Maintenance-of-Way Association (AREMA), etc.
[0046] <Method for manufacturing a rail> A method for manufacturing a rail of the present invention will now be described. The rail of the present invention can be manufactured by sequentially carrying out the following treatments on a steel material having the above-described chemical composition.
[0047] The steel material used as the rail material has the above-mentioned rail composition and can be produced by any method. In general, it is preferable to produce the steel material by casting, particularly continuous casting.
[0048] (1) Hot Rolling After the steel material is heated, it can be hot rolled into the shape of a rail.
[0049] (Heating Temperature) When heating the steel material prior to hot rolling, the heating temperature is preferably 1350°C or less. If the heating temperature exceeds 1350°C, the steel material may be partially melted due to excessive temperature rise, which may cause defects inside the rail. On the other hand, although there is no particular lower limit for the heating temperature, it is preferably 1150°C or more in order to reduce deformation resistance during rolling.
[0050] (Finishing Rolling Temperature) In hot rolling, the finishing rolling temperature is preferably 850°C or higher. If the finishing rolling temperature is lower than 850°C, rolling is performed in the low austenite temperature range, and processing strain is introduced into the austenite grains, which makes it easier for the hardness of the pearlite structure formed by accelerated cooling to vary. Therefore, the finishing rolling temperature is preferably 850°C or higher. There is no particular upper limit for the finishing rolling temperature, but if the prior austenite grain size becomes extremely coarse, breakage resistance and toughness will decrease, so it is preferably 1050°C or lower. Here, the finishing rolling temperature is the surface temperature of the center of the rail web portion at the entrance side of the final rolling mill, and can be measured with a radiation thermometer.
[0051] Other hot rolling conditions are not particularly limited.
[0052] (2) Accelerated Cooling Rails can be obtained by cooling after hot rolling. Accelerated cooling is performed on the rail web portion. When the rail height is A, the average cooling rate is controlled to be 0.4 to 5.0°C / sec from the cooling start temperature of 750°C or higher to the cooling stop temperature of 450 to 650°C at each of the following positions: the center position of the rail height (A / 2 position), a position 20 mm above the center position of the rail height (upper 20 mm position), and a position 20 mm below the center position of the rail height (lower 20 mm position). The difference in average cooling rates at these three positions is controlled to be within 0.5°C / sec.
[0053] The accelerated cooling method is not particularly limited, and can be performed, for example, by cooling using online heat treatment equipment. The cooling medium is not particularly limited, and one or more selected from air, spray water, mist, etc. can be used, but air is preferably used.
[0054] During this accelerated cooling, if the average cooling rate at either the center position (position A / 2) or the positions 20 mm above and below the center position (the upper 20 mm position and the lower 20 mm position) is less than 0.4°C / sec, the lamellar spacing in the abdominal surface layer will become coarse and pro-eutectoid cementite will be more likely to form, resulting in a decrease in breakage resistance. In addition, the cooling time in the low-temperature range will increase, reducing productivity and potentially increasing rail manufacturing costs. Therefore, the average cooling rate at each of the three positions is set to 0.4°C / sec or more, preferably 1.0°C / sec or more. On the other hand, if any of the average cooling rates at the three positions exceeds 5.0°C / sec, bainite or martensite structures will form, resulting in a decrease in breakage resistance. Therefore, the average cooling rate within each of the above ranges is set to 5.0°C / sec or less, preferably 4.0°C / sec or less.
[0055] Furthermore, if the difference in the average cooling rates at the above three positions exceeds 0.5°C / sec, the hardness of the rail web surface layer will vary greatly, making stress concentration more likely to occur in locally softened areas when bending stress is applied, and reducing breakage resistance. Therefore, the difference in the average cooling rates at the above three positions should be within 0.5°C / sec, and preferably within 0.3°C / sec. The difference in the average cooling rates at the three positions is the difference between the largest and smallest average cooling rates among the average cooling rates at the three positions.
[0056] Here, we will explain how to control the average cooling rate at the center position (A / 2), the upper 20 mm position, and the lower 20 mm position. The areas above and below A / 2 are susceptible to heat inflow from the rail head and base, respectively, due to radiant heat and thermal conduction. It is estimated that if the average cooling rates at the three positions—A / 2, the upper 20 mm position, and the lower 20 mm position—are controlled within an appropriate range (0.4–5.0°C / sec) and the difference in the average cooling rates among the three positions is controlled within a certain range (within 0.5°C / sec), the average cooling rate within a 20 mm range above and below A / 2 (a total of 40 mm) will be appropriate and uniform.
[0057] By appropriately strengthening the accelerated cooling at the upper side of the A / 2 position and the lower side of the A / 2 position, the difference in the average cooling rate at the above three positions can be stably kept within 0.5°C / sec.
[0058] For example, the nozzles can be installed in three vertical tiers so that they directly hit the A / 2 position, the upper side of the A / 2 position, and the lower side, respectively, and the injection amount and type of coolant at the three tiers can be changed according to the temperature and shape of the rail.For example, as shown in Figure 3, the air nozzles can be installed in three tiers, with the injection amount at the top 20 mm position being the highest, the injection amount at the bottom 20 mm position being the second highest, and the injection amount at the A / 2 position being the lowest.
[0059] The surface temperatures at the A / 2 position, the top 20 mm position, and the bottom 20 mm position are used as representative temperatures for determining the average cooling rate in accelerated cooling. These can be measured with a radiation thermometer. Here, the cooling start temperature is the surface temperature of the rail web portion measured with a radiation thermometer at the start of accelerated cooling, and the cooling stop temperature is the surface temperature of the rail web portion measured with a radiation thermometer after accelerated cooling has stopped (before reheating).
[0060] In the manufacturing method of the present invention, it is important to cool the rail web portion after hot rolling so that the surface temperature satisfies the above-mentioned condition, and as long as this condition is satisfied, there are no particular restrictions on the cooling method for other parts of the rail (rail head portion, rail base portion, etc.). The rail head and base portions may be naturally cooled or may be subjected to accelerated cooling.
[0061] (3) Others After cooling, the rail material may be subjected to known treatments, for example, cold roller straightening.
[0062] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the examples, and appropriate modifications can be made within the scope of the spirit of the present invention, and all of these modifications are included in the technical scope of the present invention.
[0063] Steel materials with the chemical compositions shown in Table 1 were heated and hot-rolled under the conditions shown in Table 2. After hot rolling, they were accelerated and cooled to produce 60 kg rails conforming to JIS E1101. The average cooling rate (°C / sec) was calculated by converting the temperature change from the start to the end of cooling to a value per unit time (seconds). After cooling was stopped, the rails were allowed to cool naturally. In the examples, accelerated cooling of the rail web portion was performed using the air nozzles shown in Figure 3. The amount of injected air was appropriately adjusted to change the cooling rate. In Comparative Example Test No. 34, accelerated cooling was performed using only one set of air nozzles installed at the A / 2 height among the air nozzles shown in Figure 3. At the start and end of accelerated cooling, the surface temperatures at the A / 2 position, the upper 20 mm position, and the lower 20 mm position were measured using a two-dimensional radiation thermometer capable of measuring the temperature distribution along the height of the rail web portion. The average cooling rate at these three positions was calculated.
[0064]
[0065]
[0066] The rails obtained were pearlitic rails. The Vickers hardness and three-point bending properties of the web portion of each rail were evaluated. The test results are shown in Table 2. The details of each evaluation are explained below.
[0067] <Vickers Hardness> After the accelerated cooling was completed, the rail tip was cut and then sampled from the rail web within 20 mm above and below the center of the rail height (A / 2 position) shown in Figure 2 (a total of 40 mm), including the rail web surface. These specimens were used for Vickers hardness measurement. The test specimens were embedded in resin and mirror-polished. Vickers hardness measurements were performed at 36 points, 1 mm apart, from the top to the bottom of the rail, over a range of 17.5 mm above and below the center of the rail height (A / 2 position) (a total of 35 mm). The average and standard deviation of the Vickers hardness measurements were then calculated.
[0068] <Three-Point Bending Characteristics> Test specimens were taken from the rail web at two locations, 17.5 mm above and 17.5 mm below the rail height center (A / 2 position), as shown in Figure 4, so as to include the rail web surface. The test specimens had the following dimensions: length L = 100 mm, width H = 10 mm, and thickness B = 10 mm, as shown in Figure 5. A notch was formed in the surface of the test specimen, corresponding to the rail web surface, at the center (L / 2) of the length L. The notch depth N = 0.5 mm, width C = 1.0 mm, and the bottom of the notch had a radius of curvature R = 0.5 mm. The test specimen was placed with the notch facing down on a support with a 17 mm radius and a 50 mm distance between supports. A bending strain was applied from the opposite side of the notch at a rate of 0.1 mm / sec using an indenter with a 16 mm radius of curvature. Tests were conducted on the test pieces taken from the two locations mentioned above, and if neither fractured at a displacement of 1.0 mm, the rail web was evaluated as having excellent breakage resistance.
[0069] As shown in Table 2, the test results for the rail materials of the examples (Test Nos. 1 to 39 in Table 2) showed little variation in hardness of the surface layer of the rail web, and all of them exhibited good three-point bending properties. On the other hand, the comparative examples (Test Nos. 40 to 52 in Table 2) in which the chemical composition of the rail material did not satisfy the conditions of the present invention or in which a manufacturing method outside the scope of the present invention was not applied broke before reaching the specified displacement in the three-point bending test.
[0070] According to the present invention, it is possible to provide a rail with excellent resistance to breakage of the rail web portion, together with a manufacturing method thereof. The rail of the present invention contributes to extending the service life of rails for high axle load railways and preventing railway accidents, and is industrially useful. The rail manufacturing method of the present invention enables stable manufacturing of the rail of the present invention, and is industrially useful.
[0071] 1 Rail 11 Rail head (head) 12 Rail body (body) 13 Rail foot (foot)
Claims
1. A rail having a chemical composition containing 0.70 to 1.20 mass% C, 0.10 to 1.20 mass% Si, 0.10 to 1.50 mass% Mn, 0.035 mass% or less P, 0.020 mass% or less S, and 0.05 to 1.80 mass% Cr, with the balance being Fe and unavoidable impurities; and when the Vickers hardness at a position 0.5 mm deep from the surface of the rail web part is measured within a range of ±17.5 mm above and below the center of the rail height, the average Vickers hardness is Hv280 or more with a standard deviation of 5 or less.
2. A rail according to claim 1, wherein the chemical composition further contains at least one selected from the group consisting of V: 0.30 mass% or less, Cu: 1.0 mass% or less, Ni: 1.0 mass% or less, Nb: 0.05 mass% or less, Mo: 2.0 mass% or less, Al: 0.07 mass% or less, W: 1.0 mass% or less, Co: 1.0 mass% or less, B: 0.005 mass% or less, Ti: 0.05 mass% or less, Sb: 0.05 mass% or less, Mg: 0.01 mass% or less, Ca: 0.02 mass% or less, and Sn: 0.05 mass% or less.
3. A method for manufacturing a rail as claimed in claim 1 or 2, in which a steel material having the chemical composition as claimed in claim 1 or 2 is hot-rolled to produce a rail, and cooling after hot rolling is carried out so that the average cooling rate from the cooling start temperature of 750°C or higher to the cooling stop temperature of 450 to 650°C at each of the following positions in the rail web part: the center position of the rail height, a position 20 mm above the center position of the rail height, and a position 20 mm below the center position of the rail height is 0.4 to 5.0°C / sec, and the difference in the average cooling rate at each position is within 0.5°C / sec.
Citation Information
Patent Citations
Production of rail having excellent resistance to edge rupture
JP1984047326A
Wear-resistant high-efficiency rail having instable fracture propagation stopping capacity
JP1987099438A
rail
WO2020189232A1
Rail
WO2013187470A1
rail
WO2016117692A1
Cited By
rail
JP7953254B1
rail
WO2026094371A1
rail
WO2026210886A1