Ternary composite cathode material and preparation method thereof and application in solid-state battery
By coating the surface of the ternary cathode material with polymer and oxide particles to form a composite material, the problem of the interface reaction between the sulfide electrolyte and the cathode in the solid-state battery is solved, the transfer rate and electrochemical performance of lithium ions are improved, and the electrochemical performance is simplified. process and improves battery stability and performance.
Patent Information
- Application Number
- CN202410962077.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-18
AI Technical Summary
In solid-state batteries, the interface reaction between the sulfide electrolyte and the cathode leads to an increase in resistance and material decomposition, affecting the transfer rate of lithium ions. The interface between the oxide cathode and the sulfide electrolyte causes slow migration of lithium ions, resulting in deterioration of electrochemical performance.
By coating the surface of the ternary cathode material with polymer and oxide particles to form a composite material, an electronic insulation layer is constructed to suppress the space charge layer effect, buffer volume changes, and improve material stability and electrochemical performance.
It effectively reduces space charge steric hindrance, promotes lithium ion transport, improves the cycle stability and rate performance of solid-state batteries, improves overall electrochemical performance, simplifies the process and avoids Li/Ni mixing problems caused by high-temperature sintering.
Smart Images

Figure CN118507699B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-ion batteries, and specifically to a ternary positive electrode composite material, a preparation method thereof, and an application in a solid-state battery; in particular, to a preparation method of a composite material of polymer and oxide particles coated on the surface of a ternary positive electrode, and an application in a solid-state battery. Background Art
[0002] Over the past two decades, lithium-ion batteries (LIBs) have dominated power batteries and energy storage batteries, but low energy density and safety issues such as leakage and fire caused by liquid organic electrolytes make it difficult for LIBs to meet the needs of high-power applications such as electric vehicles and grid energy storage. Solid-state batteries (SSBs) replace liquid organic electrolytes with safer solid electrolytes (SSEs) and are considered to be the next generation of batteries for energy storage.
[0003] However, the interfacial reaction between the cathode and the solid electrolyte (SSE) and the resulting resistance lead to the deterioration of battery performance, hindering its ultimate commercial use. The most important problem is that due to the lack of thermodynamic stability of sulfide electrolytes, the interface between the electrode and the sulfide electrolyte in solid-state batteries undergoes an interfacial reaction, resulting in the generation of byproducts in the sulfide electrolyte, causing the impedance to continue to increase, causing a sharp decrease in the transfer rate of lithium ions between different material interfaces. In addition, due to the narrow electrochemical window (1.7-2.4V) of sulfide electrolytes, material decomposition occurs at the interface between the cathode and the sulfide electrolyte, resulting in the formation of a Li-deficient phase on the cathode surface during the cycle, which leads to the obstruction of interfacial ion transport, such as the appearance of a low ionic conductivity rock salt phase such as NiO on the surface of the ternary cathode material. These problems all originate from the interface degradation caused by interface instability. A common method is to use a buffer layer to prevent direct contact between the active material and the electrolyte. In principle, either the electrode or the electrolyte can be coated to stabilize the electrode / electrolyte interface. Positive electrode coating is usually the first choice, which can be attributed to the fact that coating on the surface of sulfide electrolyte will hinder the migration of ions, resulting in a decrease in ionic conductivity.
[0004] Surface coating is one of the effective methods to solve the above-mentioned interface problem between the positive electrode and the sulfide electrolyte. Through the means of material composite, different materials can work synergistically to give the composite material different surface activity, physical, chemical and mechanical properties. Most of the oxide particle coating plays a role in stabilizing the structure of the positive electrode material, and can improve the interface contact between the positive electrode material and the sulfide electrolyte, effectively suppressing the problem of interface decomposition and byproducts caused by the chemical potential difference between the electrode and the sulfide electrolyte, and can improve the stability and conductivity of the positive electrode sulfide electrolyte interface, thereby improving the cycle stability and rate performance of the solid-state battery, and improving the electrochemical performance of the overall battery cell. However, in solid-state batteries, the oxide positive electrode is usually a mixed conductor with high ionic and electronic conductivity, while the sulfide electrolyte is a single lithium ion conductor. Therefore, the contact between the oxide positive electrode and the sulfide electrolyte interface will cause lithium ions to slowly move from the sulfide electrolyte to the oxide positive electrode, forming a space charge layer. The presence of the space charge layer will cause high electrode resistance, which seriously affects the electrochemical performance of solid-state batteries.
[0005] The prior patent 202311843494.5 discloses a composite-coated lithium-ion battery positive electrode material, a preparation method and an application thereof, wherein the lithium-ion battery positive electrode material comprises a positive electrode active material core and a composite coating layer coated on the surface of the positive electrode active material core, wherein the composite coating layer comprises a conductive polymer and an inorganic oxide, and the inorganic oxide is distributed in a dotted manner on the surface of the positive electrode active material core, and the inorganic oxide distributed in a dotted manner is dispersed in the conductive polymer matrix, extending from the surface of the positive electrode active material core to the surface of the composite coating layer. The preparation method comprises the following steps: (1) mixing a positive electrode active material core, a template agent and a pore-forming agent to obtain a positive electrode active material core coated with a template layer, and then removing the pore-forming agent to obtain a positive electrode active material core coated with a porous template layer; (2) mixing a solution containing an inorganic oxide with the positive electrode active material core coated with a porous template layer, filling the inorganic oxide powder into the pores of the template layer, sintering to remove the template layer, and obtaining a positive electrode active material core coated with an inorganic oxide with a point distribution; (3) mixing the positive electrode active material core coated with an inorganic oxide with a point distribution obtained in step (2) with a conductive polymer raw material solution to obtain a primary product; and (4) post-treating the primary product obtained in step (3) to obtain the composite coated lithium ion battery positive electrode material. However, this solution has complicated steps and introduces pore-forming agents such as lithium chloride and sodium chloride. When the pore-forming agents are removed by sintering, by-products are easily formed on the surface of the positive electrode material. Moreover, when sintered at high temperature, it is also easy to cause Li / Ni mixing of the ternary positive electrode material, affecting the electrochemical properties of the material.
[0006] Prior patent 201810962485.0 discloses a lithium-ion layered ternary positive electrode material modified by TiN and a conductive polymer composite and a preparation method thereof. First, nano-TiN and a ternary positive electrode material are mixed in a liquid phase to form a ternary positive electrode material with uniform adsorption of TiN particles; then, a layer of conductive polymer is polymerized on the surface of the material by a liquid phase oxidation polymerization method to form a composite coating layer of nano-TiN particles and conductive polymers, thereby obtaining a ternary positive electrode material with a composite coating of TiN and conductive polymers. However, if TiN is to be uniformly adsorbed on the surface of the ternary positive electrode, it is generally necessary to modify the material, and the anchor points are formed by charge adsorption or group attraction on the surface of the material, which is more difficult. In the present invention, the oxide particles can be anchored on the surface of the ternary positive electrode material by using a polymer as a binder. Summary of the invention
[0007] In view of this, the purpose of the present invention is to provide a ternary composite positive electrode material and its preparation method and application. The present invention obtains a composite material by coating a polymer and oxide particles on the surface of the ternary positive electrode to form an electronic insulation layer; effectively suppresses the space charge layer effect between the ternary positive electrode and the sulfide electrolyte, and promotes the transmission of lithium ions at the interface between the ternary positive electrode and the sulfide electrolyte. In addition, the ternary positive electrode has a certain volume change during the charge and discharge process. The polymer coating layer can buffer the volume expansion force between the positive electrode particles, prevent the oxide particles from falling off on the surface of the ternary positive electrode due to the influence of volume change stress, and improve the stability of the material in the electrochemical process.
[0008] The technical solution provided by the present invention is as follows:
[0009] <First aspect>
[0010] A method for preparing a ternary composite positive electrode material comprises the following steps:
[0011] (1) Adding the polymer into an organic solvent and dissolving it to obtain a polymer solution A;
[0012] (2) The oxide is dispersed in the polymer solution A to obtain a mixed solution B;
[0013] (3) placing the ternary cathode material in the mixed solution B and dispersing it to obtain a mixed solution C;
[0014] (4) Filter the mixed solution C, collect the precipitate, and dry it to obtain a ternary composite positive electrode material.
[0015] In step (1), the polymer includes one or more of polyimide, polyetherimide, and polyethersulfone.
[0016] In step (1), the organic solution includes one or more of methanol, ethanol, N-dimethylformamide, and N-methylpyrrolidone.
[0017] In the mixed solution C, the mass ratio of the polymer, the oxide, and the ternary positive electrode material is 5-50:15-50:100-500.
[0018] Too high a polymer content will result in excessive internal resistance.
[0019] In step (2), the oxide is selected from one or more of zinc oxide, lithium niobate, lithium titanate, lithium lanthanum titanium oxide (LLTO), and lithium lanthanum zirconium oxide (LLZO).
[0020] High-voltage-resistant oxide particles and polymers can effectively alleviate the instability of the positive electrode / sulfide electrolyte interface; and lithium lanthanum titanium oxide (LLTO) can provide a lithium ion transmission channel, and the polymer coating can provide an effective electronic insulation layer. Through the composite effect of oxide particles and polyimide, an ion-conducting and electronically insulating coating layer can be constructed on the positive electrode surface to reduce the formation of space charge steric hindrance.
[0021] Preferably, the oxide is LLTO oxide particles. LLTO oxide particles are conducive to the migration and diffusion of lithium ions due to their unique structure. In addition, the surface coating of the polymer can produce a synergistic effect with LLTO, improve the space charge steric hindrance problem, and enhance the electrochemical performance of the material.
[0022] In steps (2) and (3), the dispersion method can be one or more of ultrasound, stirring, oscillation and the like.
[0023] In step (4), the filtration separation includes rotary evaporation, centrifugation, suction filtration, etc.
[0024] In step (4), the drying is carried out by vacuum drying at a temperature of 40 to 120° C. and a drying time of 1 to 24 hours.
[0025] <Second Aspect>
[0026] The ternary composite positive electrode material prepared by the preparation method as described above also falls within the protection scope of the present invention.
[0027] <Third Aspect>
[0028] The application of the ternary composite positive electrode material in solid-state batteries also falls within the protection scope of the present invention.
[0029] The key point of the present invention is that the polymer is first added to the organic solvent to dissolve to obtain the polymer solution A; then the oxide is placed in the polymer solution A and dispersed to obtain the mixed solution B. Through this step, the polymer layer is coated on the surface of the oxide particles; the ternary positive electrode material is further placed in the mixed solution B and dispersed to obtain the mixed solution C; the oxide particles coated with the polymer layer are coated on the surface of the ternary positive electrode material; the composite positive electrode material prepared by this method has a simple process, good material structure stability, and the oxide surface does not need to be treated. It can be evenly dispersed on the surface of the ternary positive electrode material through the bonding force of the polymer. The excellent deformation adaptability of the polymer coating layer can well buffer the volume deformation between the positive electrode particles, prevent the oxide particles from falling off on the surface of the ternary positive electrode, and improve the structural stability of the positive electrode composite material, thereby improving the cycle stability and rate performance of the solid-state battery, and improving the electrochemical performance of the overall battery core. The process of the scheme of the present invention is simple, no other substances such as pore-forming agents are introduced, there are few side reactions, and high-temperature re-sintering is not required. Generally, when the ternary positive electrode is re-sintered at high temperature, it is easy to cause Li / Ni mixing, which affects the performance of the electrochemical performance of the material.
[0030] However, there are the following problems when first coating an oxide layer on the surface of the positive electrode material and then coating the oxide layer with a polymer layer. For example, the oxide or ternary positive electrode needs to be surface modified to introduce functional groups to improve adhesion. Ensure the bonding strength between the oxide and the positive electrode interface. Otherwise, it is easy to cause the surface of the ternary positive electrode to be unable to be coated with an oxide layer, or the oxide layer is uneven on the surface of the ternary positive electrode.
[0031] A polymer layer is first coated on the surface of the positive electrode material, and then an oxide layer is coated on the surface of the polymer layer. The polymer layer is easily dissolved when coating the oxide layer, and the oxide particles obtained subsequently are easy to fall off the layer.
[0032] Compared with the prior art, the beneficial effects of the present invention are:
[0033] (1) High-voltage-resistant oxide particles and polymers can effectively alleviate the instability of the cathode / sulfide electrolyte interface and improve electrochemical stability;
[0034] (2) The lithium-ion-conducting oxide particles and the electronically insulating polymer coating layer work synergistically to reduce the formation of space charge steric hindrance and promote the transfer of lithium ions at the interface between the positive electrode and the sulfide electrolyte;
[0035] (3) The good deformation adaptability of the polymer coating effectively alleviates the volume expansion stress generated during the charging and discharging process of the positive electrode material and prevents the oxide particles from falling off the surface of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0037] Figure 1 The charge and discharge test of the solid-state battery assembled with the unmodified NCM positive electrode composite material prepared in Comparative Example 1;
[0038] Figure 2 The charge and discharge test of the solid-state battery assembled with the NCM@PI / LLTO-1 cathode composite material prepared in Example 1;
[0039] Figure 3 The charge and discharge test of the solid-state battery assembled with the NCM@PI / LLTO-2 cathode composite material prepared in Example 2;
[0040] Figure 4 Cyclic test of a solid-state battery assembled from the NCM@PI / LLTO-2 cathode composite material prepared in Example 2;
[0041] Figure 5 This is a charge and discharge test of a solid-state battery assembled with the NCM@PI / LLTO-3 positive electrode composite material prepared in Example 3. DETAILED DESCRIPTION
[0042] The present invention is described in detail below in conjunction with embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, some adjustments and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0043] Example 1
[0044] A method for coating polymer and oxide particles on the surface of a ternary cathode material and its application in a solid-state battery, comprising the following steps:
[0045] (1) Take 50 mg of polyimide (DuPont, USA) particles and add them into 10 mL of NMP organic solvent to dissolve and obtain polymer solution A;
[0046] (2) taking 50 mg of lithium lanthanum titanium oxide particles (LLTO) and placing them in the polymer solution A obtained in step (1), and performing ultrasonic dispersion to obtain a mixed solution B;
[0047] (3) Take 5g LiNi 0 .90 Co 0 .06 Mn 0 .04 O2 is placed in the mixed solution B obtained in step (2) and ultrasonically dispersed to obtain a mixed solution C.
[0048] (4) The mixed solution C was filtered to obtain a precipitate which was then vacuum dried at 60-80°C to obtain a NCM surface-coated PI and LLTO composite material, named NCM@PI / LLTO-1.
[0049] Example 2
[0050] A preparation method of a composite material of polymer and oxide particles coated on the surface of a ternary positive electrode and its application in a solid-state battery, comprising the following steps:
[0051] (1) Take 50 mg of polyimide particles (DuPont, USA) and add them into 10 mL of NMP organic solvent to dissolve and obtain polymer solution A;
[0052] (2) taking 150 mg of LLZO oxide particles and placing them in the polymer solution A obtained in step (1), and performing ultrasonic dispersion to obtain a mixed solution B;
[0053] (3) Take 5g LiNi 0 .90 Co 0 .06 Mn 0 .04 O2 is placed in the mixed solution B obtained in step (2) and ultrasonically dispersed to obtain a mixed solution C.
[0054] (4) The mixed solution C was filtered to obtain a precipitate, which was then vacuum dried at 60-80°C to obtain a composite material of NCM surface coated with PI and LLTO, named NCM@PI / LLTO-2.
[0055] Example 3
[0056] A preparation method of a composite material of polymer and oxide particles coated on the surface of a ternary positive electrode and its application in a solid-state battery, comprising the following steps:
[0057] (1) Take 250 mg of polyimide particles (DuPont, USA) and add them into 10 mL of NMP organic solvent to dissolve and obtain polymer solution A;
[0058] (2) taking 250 mg of LLTO oxide particles and placing them in the polymer solution A obtained in step (1), and performing ultrasonic dispersion to obtain a mixed solution B;
[0059] (3) Take 5g LiNi 0 .90 Co 0 .06 Mn 0 .04 O2 is placed in the mixed solution B obtained in step (2), and ultrasonic dispersion is performed to obtain a mixed solution C;
[0060] (4) The mixed solution C was filtered to obtain a precipitate, which was then vacuum dried at 60-80°C to obtain a composite material of NCM surface coated with PI and LLTO, named NCM@PI / LLTO-3.
[0061] Example 4
[0062] A preparation method of a composite material of polymer and oxide particles coated on the surface of a ternary positive electrode and its application in a solid-state battery, comprising the following steps:
[0063] (1) Take 500 mg of polyimide particles (DuPont, USA) and add them into 10 mL of NMP organic solvent to dissolve and obtain polymer solution A;
[0064] (2) taking 500 mg of LLTO oxide particles and placing them in the polymer solution A obtained in step (1), and performing ultrasonic dispersion to obtain a mixed solution B;
[0065] (3) Take 5g LiNi 0 .90 Co 0 .06 Mn 0 .04 O2 is placed in the mixed solution B obtained in step (2) and ultrasonically dispersed to obtain a mixed solution C.
[0066] (4) The mixed solution C was filtered to obtain a precipitate, which was then vacuum dried at 60-80°C to obtain a NCM surface-coated PI and LLTO composite material, named NCM@PI / LLTO-4.
[0067] (5) The NCM@PI / LLTO-4 composite material was used as the positive electrode, the sulfide electrolyte Li6PS5Cl was used as the electrolyte layer, and the In-Li alloy was used as the negative electrode to assemble a solid-state battery for electrochemical testing.
[0068] Comparative Example 1
[0069] The difference between this comparative example and Example 1 is that the unmodified LiNi 0 .90 Co 0 .06 Mn 0 .04 O2 material was used as the positive electrode, sulfide electrolyte Li6PS5Cl was used as the electrolyte layer, and In-Li alloy was used as the negative electrode to assemble a solid-state battery for electrochemical testing.
[0070] Comparative Example 2
[0071] The difference between this comparative example and Example 1 is that in step 1, polyimide is replaced by polyacrylonitrile.
[0072] Comparative Example 3
[0073] The difference between this comparative example and Example 1 is that in step 2, the LLTO oxide particles are replaced by silicon oxide.
[0074] Comparative Example 4
[0075] The difference between this comparative example and Example 1 is that: an oxide layer is first coated on the surface of the positive electrode material, and then a polymer layer is coated on the oxide layer to form NCM@LLTO-4@PI; specifically, the following steps are included:
[0076] (1) 250 mg of LLTO oxide particles were added to 10 mL of NMP organic solvent and ultrasonically dispersed to obtain solution A;
[0077] (2) Take 5g LiNi 0 .90 Co 0 .06 Mn 0 .04 O2 is placed in the mixed solution B obtained in step (1), and ultrasonic dispersion is performed to obtain a solution B;
[0078] (3) Filter solution B to obtain a precipitate, and then dry it in vacuum at 60-80°C to obtain NCM@LLTO-4;
[0079] (4) 250 mg of polyimide particles (DuPont, USA) were dissolved in 10 mL of NMP organic solvent to obtain polymer solution C;
[0080] (5) Take 5 g of NCM@LLTO-4 and place it in the polymer solution C obtained in step (4), and perform ultrasonic dispersion to obtain a mixed solution D.
[0081] (6) The mixed solution D was filtered to obtain a precipitate, which was then vacuum dried at 60-80 °C to obtain a composite positive electrode material, named NCM@LLTO-4@PI.
[0082] Comparative Example 5
[0083] First, a polymer layer is coated on the surface of the positive electrode material, and then an oxide layer is coated on the surface of the polymer layer to form NCM@PI@LLTO-4. The specific steps include:
[0084] (1) Take 250 mg of polyimide particles (DuPont, USA) and add them into 10 mL of NMP organic solvent to dissolve and obtain polymer solution A;
[0085] (2) Take 5g LiNi 0 .90 Co 0 .06 Mn 0 .04 O2 is placed in the polymer solution A obtained in step (1), and ultrasonic dispersion is performed to obtain a mixed solution B;
[0086] (3) Filter solution B to obtain a precipitate, and then dry it in vacuum at 60-80°C to obtain NCM@PI;
[0087] (4) 250 mg of LLTO oxide particles were placed in 10 mL of NMP organic solvent C and ultrasonically dispersed to obtain a mixed solution C;
[0088] (5) 5 g of NCM@PI was placed in the polymer solution C obtained in step (4), and ultrasonically dispersed to obtain a mixed solution D;
[0089] (6) The mixed solution D was filtered to obtain a precipitate, which was then dried in a vacuum oven at 60-80 °C to obtain a composite material of NCM surface coated with PI and LLTO, named NCM@PI@LLTO.
[0090] Comparative Example 6
[0091] (1) 10g of uncoated LiNi 0 .90 Co 0 .06 Mn 0 .04 O2 ternary material, 1g of polymethyl methacrylate as a template and 0.15g of sodium chloride (average particle size of 200nm) as a pore-forming agent were mixed together to obtain a ternary material core coated with a template layer, wherein the thickness of the template layer was 150nm.
[0092] (2) The ternary material core body coated with the template layer is dried at 80°C for 6 hours. Then, the pore-forming agent is removed by water washing to obtain a positive electrode active material core body coated with a porous template layer. Next, the positive electrode active material core body coated with a porous template layer is dried at 90°C for 12 hours to obtain a dried treated positive electrode active material core body.
[0093] (3) 0.1 g of Li with a particle size of 50 nm 1.3 Al 0.3 Ti 1.7 (PO4)3(LATP) was dispersed in deionized water and stirred to form a uniformly dispersed sol dispersion. 10g of the treated positive electrode active material core was slowly added to the LATP dispersion and stirred at 65°C to obtain a mixture slurry, and the solvent was finally completely evaporated to obtain a precursor. The precursor was placed in a sintering furnace, the sintering temperature was set to 550°C, and sintered for 6 hours to obtain a ternary material coated with an inorganic oxide with a dot distribution;
[0094] (4) Accurately weigh 1g of polyimide particles and add them to a beaker containing 34g of dimethylformamide, seal and stir at room temperature for 20min to obtain a conductive polymer raw material solution. Add 10g of the above-mentioned ternary material coated with inorganic oxide to the conductive polymer raw material solution, stir and disperse at 45°C for 5h, and then dry the mixture at 80°C for 10h. Finally, the dried material is heat-treated at 220°C for 1h to finally obtain a ternary positive electrode material with a cyclization rate of 50% of polyacrylonitrile polymer and inorganic oxide composite coating.
[0095] Performance test case
[0096] Detection method:
[0097] Solid-state battery preparation: The composite positive electrode materials prepared in Examples 1-4 and Comparative Examples 1-3 were mixed with the sulfide solid electrolyte material Li6PS5Cl (a total of 20 mg) at a ratio of 7:3 and pressed into sheets as the positive electrode; the sulfide electrolyte Li6PS5Cl (100 mg) was pressed into sheets; and finally assembled with Li-Ln sheets into a half-cell. The charge and discharge performance and cycle stability were tested. Charge and discharge test conditions: 0.2C; cycle test conditions: 1C.
[0098] Test results see Figure 1-5 With Table 1:
[0099] Figure 1 The charge and discharge test of the solid-state battery assembled with the unmodified NCM positive electrode composite material prepared in Comparative Example 1;
[0100] Figure 2 The charge and discharge test of the solid-state battery assembled with the NCM@PI / LLTO-1 cathode composite material prepared in Example 1;
[0101] Figure 3 The charge and discharge test of the solid-state battery assembled with the NCM@PI / LLTO-2 cathode composite material prepared in Example 2;
[0102] Figure 4 Cyclic test of a solid-state battery assembled from the NCM@PI / LLTO-2 cathode composite material prepared in Example 2;
[0103] Figure 5 This is a charge and discharge test of a solid-state battery assembled with the NCM@PI / LLTO-3 positive electrode composite material prepared in Example 3.
[0104] Table 1 Electrochemical performance test results
[0105]
[0106] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. A method for preparing a ternary composite positive electrode material, characterized in that: The following steps are involved: (1) Adding the polymer into an organic solvent and dissolving it to obtain a polymer solution A; (2) The oxide is dispersed in the polymer solution A to obtain a mixed solution B; (3) placing the ternary cathode material in the mixed solution B and dispersing it to obtain a mixed solution C; (4) Filter the mixed solution C, collect the precipitate, and dry it to obtain a ternary composite positive electrode material; In step (1), the polymer includes one or more of polyimide, polyetherimide, and polyethersulfone; In step (2), the oxide is selected from one or more of zinc oxide, lithium niobate, lithium titanate, lithium lanthanum titanium oxide, and lithium lanthanum zirconium oxide.
2. The preparation method according to claim 1, characterized in that: In step (1), the organic solvent includes one or more of methanol, ethanol, N-dimethylformamide, and N-methylpyrrolidone.
3. The preparation method according to claim 1, characterized in that: In the mixed solution C, the mass ratio of the polymer, the oxide, and the ternary positive electrode material is 5-50:15-50:100-500.
4. The preparation method according to claim 1, characterized in that: In steps (2) and (3), the dispersion method includes one or more of ultrasound, stirring, and shaking.
5. The preparation method according to claim 1, characterized in that: In step (4), the drying is carried out by vacuum drying at a temperature of 40 to 120° C. and a drying time of 1 to 24 hours.
6. A ternary composite positive electrode material prepared by the preparation method according to any one of claims 1 to 5.
7. Use of the ternary composite cathode material as claimed in claim 6 in a sulfide solid-state battery.