A positive electrode catalyst composite material and its preparation method and application
By using small-particle cobalt catalyst dispersed on the surface of carbon nanotubes in Li-CO2 batteries, the problems of slow CO2 reduction reaction kinetics and difficulty in decomposing discharge products in Li-CO2 batteries were solved, thereby improving the specific capacity and cycle performance of the batteries.
Patent Information
- Application Number
- CN202410923881.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-11
AI Technical Summary
The slow kinetics of CO2 reduction reaction in Li-CO2 batteries make it difficult to decompose the discharge product Li2CO3, leading to increased electrode impedance, hindering electron conduction and gas diffusion, and reducing battery energy efficiency and cycle life.
A cathode catalyst composite material using highly dispersed small cobalt particles on the surface of carbon nanotubes is used to improve catalytic activity and enhance electron conduction and gas diffusion through specific structural design.
The specific capacity and cycle performance of the Li-CO2 battery were improved. The battery achieved a specific capacity of 38240.28 mAh/g at a current density of 100 mA/g and remained stable after 104 cycles, demonstrating excellent electrochemical performance.
Smart Images

Figure CN118507746B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrode materials, and more specifically, to a positive electrode catalyst composite material and a preparation method and application thereof. Background Art
[0002] Since the industrial age, human society's high dependence on fossil fuels has led to a continuous increase in the concentration of greenhouse gases in the atmosphere, especially CO2, which has caused a global environmental problem that needs to be urgently solved in this century. At present, the control of atmospheric CO2 emissions has become a research hotspot, including various electrochemical and photochemical methods.
[0003] In recent years, Li-CO2 batteries are considered to be the most promising secondary batteries due to their many advantages such as environmental friendliness, high energy density, cheap raw materials, and reversible electrochemical reactions. With the development of modern manufacturing technology, Li-CO2 batteries will be widely used in electronic equipment, communication devices and other fields compared to other energy storage systems. Although great progress has been made, the charge and discharge reactions of Li-CO2 batteries still need to be improved. During the discharge process, the stable carbon-oxygen double bond (C = O) in the CO2 molecule causes the CO2 reduction reaction kinetics to be slow. As the discharge reaction proceeds, Li2CO3, the main non-conductive discharge product, continues to accumulate on the surface of the electrode material or catalyst, which increases the impedance of the electrode and hinders Li + The transmission of Li2CO3 hinders the conduction of electrons and the diffusion of gases, shielding the electrochemical catalytic active sites, resulting in reduced battery energy efficiency and shortened cycle life; during the charging process, Li2CO3 is difficult to completely decompose due to its good thermodynamic stability and inert reaction kinetics, resulting in a decomposition voltage as high as 4.38-4.61 V (relative to Li / Li + ), causing severe polarization and decomposition of the electrolyte as well as a large number of side reactions.
[0004] Therefore, the slow kinetics of CO2 conversion reaction and the difficulty in decomposing and aggregating discharge products are key issues facing the development of Li-CO2 batteries, which seriously restrict their development.
[0005] Catalyst is one of the important materials in the positive electrode of Li-CO2 battery. The selection and design of catalyst has a great influence on the performance of Li-CO2 battery. It can improve the catalytic activity of the positive electrode of Li-CO2 battery, and can also greatly improve the specific capacity of Li-CO2 battery, and enhance the cycle performance of the battery. For example, Chinese patent application CN202011223114.4 discloses a method for preparing a cobalt-carbon nanotube / nitrogen-doped activated carbon oxygen reduction reaction catalyst, which introduces metallic cobalt to change the local charge and spin distribution, form a catalytic active center, and promote redox reaction to improve the electrochemical performance of lithium-carbon dioxide battery. However, its reserves are low and the preparation process is complicated, which is not suitable for industrial applications. Summary of the invention
[0006] Based on the above technical problems existing in the prior art, the present invention provides a method for preparing a positive electrode catalyst composite material. The composite material obtained by the method consists of carbon nanotubes and metallic cobalt on the surface thereof. The metallic cobalt is highly dispersed and attached to the surface of the carbon nanotubes in the form of small particles. By performing specific structural design on the positive electrode catalyst composite material, the problem of low battery energy efficiency and short cycle life caused by increased electrode impedance due to the catalytic activity of the catalyst during the cycle of the Li-CO2 battery in the prior art, which hinders electron conduction and gas diffusion, can be effectively solved, thereby improving the specific capacity and cycle performance of the Li-CO2 battery.
[0007] In order to achieve the above object, the technical solution of the present invention is as follows:
[0008] A method for preparing a positive electrode catalyst composite material comprises the following steps:
[0009] S1, dissolving organic cobalt salt, urea, carbon dots and carbon nanotubes in water to obtain a precursor solution;
[0010] S2, heating the precursor solution to perform a hydrothermal reaction, and after the reaction is completed, cooling and drying to obtain a precursor material;
[0011] S3, calcining the precursor material in an argon-hydrogen mixed gas atmosphere to obtain the composite material.
[0012] In some embodiments, in step S2, the temperature of the hydrothermal reaction is 100-200°C.
[0013] In some embodiments, the hydrothermal reaction time is 1-10 h.
[0014] In some embodiments, in step S3, the calcination temperature is 400-700°C.
[0015] In some embodiments, in step S3, the volume ratio of argon to hydrogen in the argon-hydrogen mixed gas is 8-9:1-2.
[0016] In some embodiments, the carbon dots are carbon dots doped with at least one of N, S, and F.
[0017] In some embodiments, the carbon dots are N and S co-doped carbon dots, and the preparation method thereof comprises the following steps:
[0018] L-cysteine is dissolved in formaldehyde, and then sodium hydroxide is added while stirring to react; after the reaction is completed, the solid and liquid are separated, the liquid is poured out, and the remaining solid is dissolved with deionized water to obtain an aqueous solution; finally, the aqueous solution is transferred to a dialysis bag for dialysis; the dialyzed liquid is placed in a beaker and frozen in a refrigerator, and then freeze-dried to obtain the product N, S co-doped carbon dots.
[0019] The present invention also provides a positive electrode catalyst composite material obtained by the preparation method of any of the above embodiments, wherein the positive electrode catalyst composite material is composed of carbon nanotubes and metal cobalt on the surface thereof, and the metal cobalt is highly dispersed and attached to the surface of the carbon nanotubes in the form of small particles.
[0020] The present invention also provides a positive electrode material, which includes the positive electrode catalyst composite material.
[0021] In some embodiments, the cathode material includes 70-90% of the cathode catalyst composite material and 10-30% of a binder.
[0022] The present invention also provides a positive electrode, which includes the positive electrode material of any one of the above embodiments.
[0023] The present invention also provides a Li-CO2 battery, which comprises the positive electrode mentioned above.
[0024] In some embodiments, the battery further comprises a negative electrode, a separator, a current collector, nickel foam, and an electrolyte.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention obtains a catalyst composite material with a specific structure through a specific preparation method. The composite material is composed of carbon nanotubes and metal cobalt on the surface thereof. The metal cobalt is highly dispersed and attached to the surface of the carbon nanotubes in the form of small particles. By performing specific structural design on the positive electrode catalyst composite material, the problems of low battery energy efficiency and short cycle life caused by increased electrode impedance due to the catalytic activity of the catalyst during the cycle of the Li-CO2 battery in the prior art can be effectively solved, thereby improving the specific capacity and cycle performance of the Li-CO2 battery.
[0027] The composite material obtained by the present invention is applied to a Li-CO2 battery. At a current density of 100 mA / g, the voltage range is 2.3-4.5 V, and the specific capacity of the battery reaches 38240.28 mAh / g. When the current density is 400 mA / g and the cut-off capacity is 1000 mAh / g, the positive electrode of the Li-CO2 battery is stably cycled 104 times, showing excellent electrochemical performance, and has broad application prospects in the field of Li-CO2 batteries.
[0028] The method of the invention has simple process and is easy to operate, adopts environmentally friendly and non-toxic reagents, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 XRD pattern of the Li-CO2 battery cathode catalyst material prepared in Example 1;
[0030] Figure 2 This is a SEM image of the Li-CO2 battery cathode catalyst material prepared in Example 1;
[0031] Figure 3 The first cycle discharge curve of the Li-CO2 battery prepared in Example 3 at different current densities;
[0032] Figure 4 The first cycle charge and discharge curves of the Li-CO2 battery of Example 3 at different rates;
[0033] Figure 5 The long cycle curve of the Li-CO2 battery of Example 3 at a current density of 400 mA / g and a cut-off capacity of 1000 mAh / g;
[0034] Figure 6 This is the SEM image of the Co@CNTs composite material obtained in Comparative Example 2;
[0035] Figure 7 is the SEM image of the Co-CDs composite material obtained in Comparative Example 3;
[0036] Figure 8 The first cycle charge and discharge curves of the Li-CO2 batteries of Example 3, Comparative Examples 1-3 and the control group at a current density of 50 mA / g and a cutoff capacity of 1000 mAh / g. DETAILED DESCRIPTION
[0037] Many specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar modifications without violating the connotation of the present invention, so the present invention is not limited to the specific implementation disclosed below.
[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0039] The carbon dots used in the following examples and comparative examples are N, S co-doped carbon dots (N,S-CDs), which are prepared by:
[0040] L-cysteine was dissolved in formaldehyde, and then sodium hydroxide was added while stirring to react for 2 hours; after the reaction was completed, the solid and liquid were separated, the liquid was poured out, and the remaining solid was dissolved with deionized water to obtain an aqueous solution; finally, the aqueous solution was transferred to a dialysis bag for dialysis; the dialyzed liquid was placed in a beaker and frozen in a refrigerator, and then freeze-dried to obtain the product N, S co-doped carbon dots (N,S-CDs). Example 1
[0041] A method for preparing a positive electrode catalyst material for a Li-CO2 battery comprises the following steps:
[0042] S1. Take 2.52g (~10mmol) Co(CHCOO)2·4H2O and 0.45g (~75mmol) urea, add them into 90mL deionized water, stir and dissolve, add 0.1g N,S-CDs after they are completely dissolved, keep stirring until there are no solid particles; then weigh 80mg multi-walled carbon nanotubes and add them into the above mixture in batches, stir for 10min and then ultrasonicate for 10min;
[0043] S2. The mixed solution was transferred to a reactor with a capacity of 120 ml, placed in a hydrothermal oven, and hydrothermaled at 120°C for 2 hours. After cooling, it was washed with deionized water 5 times, and then dried at 60°C in a vacuum drying oven for 8 hours. The mixture was calcined at 500°C for 2 hours in a tubular furnace with argon-hydrogen mixed gas, where the ratio of argon to hydrogen was 9:1, to obtain a Co-based metal composite catalyst material (Co-CDs@CNTs) with morphology regulated by N, S-CDs.
[0044] The catalyst material obtained in this example was characterized, and the characterization results are as follows Figure 1 and Figure 2 shown.
[0045] See also Figure 1 , Figure 1 The XRD pattern of the Li-CO2 battery cathode catalyst material prepared by the present invention is shown. Figure 1 It can be seen that Co metal exists in the form of a single substance, and the crystal form is Co#05-0727.
[0046] See also Figure 2 , Figure 2 The SEM image of the Li-CO2 battery cathode catalyst material prepared by the present invention is shown. Figure 2 It can be seen that under the morphology regulation of carbon dots, the Co metal element is granular and dispersed around the carbon nanotubes. Example 2
[0047] A positive electrode material for a Li-CO2 battery, which is composed, by weight percentage, of 90% of the positive electrode catalyst material obtained in Example 1 and 10% of a binder (CMC).
[0048] The Li-CO2 battery positive electrode sheet containing the above-mentioned Li-CO2 battery positive electrode material is prepared in the following steps:
[0049] (1) Dissolve 45 mg of the positive electrode catalyst material and 5 mg of carboxymethyl cellulose (CMC) in 2 ml of nitrogen methyl pyrrolidone (NMP), stir on a magnetic stirrer for 5 h, and mix well to obtain a liquid mixture;
[0050] (2) The above liquid mixture was applied on carbon paper (model: HCP020N, diameter: 12 mm, purchased from Shanghai Hesen Electric Co., Ltd.), the film surface was as flat as possible, and it was dried in advance. After drying in an oven at 80 °C for 12 h, the positive electrode sheet of the Li-CO2 battery was prepared. Example 3
[0051] When the Li-CO2 battery positive electrode sheet obtained in Example 2 is used to assemble a cylindrical Li-CO2 battery, it is carried out in an inert glove box filled with high-purity argon gas, and the H2O and O2 contents are controlled below 1 ppm. The steps are as follows:
[0052] a. Place the black positive electrode sheet, negative electrode sheet, battery shell, separator, current collector, nickel foam, electrolyte, pipette, pipette tip, plastic tweezers, and sealed bag into the glove box;
[0053] b. A self-made electrode disc is used as the positive electrode, a lithium sheet is used as the negative electrode, a glass fiber diaphragm is used as the diaphragm, and the electrolyte is 1M LITFSI / TEGDME;
[0054] c. Place nickel foam, black positive electrode lithium sheet (with the material side facing up), diaphragm on the positive electrode shell in sequence, then drop 130 microliters of electrolyte, and finally place the lithium sheet;
[0055] d. Cover the battery case and press it with insulated pliers to fully close it;
[0056] e. Use plastic tweezers to put the battery into a sealed bag and move it out of the glove box.
[0057] The Li-CO2 battery obtained in this example was subjected to electrochemical performance tests. The test results are as follows: Figure 3-Figure 5 shown.
[0058] See also Figure 3 , Figure 3 The first cycle discharge curve of the Li-CO2 battery cathode catalyst material prepared by the present invention at different current densities; the test conditions are: current density 50 mA / g and 100 mA / g, voltage range 2.3-4.5V.
[0059] from Figure 3 It can be seen that when the current density is 50 mA / g, the specific capacity of the Li-CO2 battery positive electrode is 24450.43 mAh / g; when the current density is 100 mAh / g, the specific capacity of the Li-CO2 battery positive electrode is as high as 38240.28 mAh / g.
[0060] See also Figure 4 , Figure 4 The first cycle charge and discharge curves of the positive electrode catalyst material of Li-CO2 battery at different rates. The test conditions are: 1C is 100mA / g, and the cut-off capacity is 1000mAh / g.
[0061] from Figure 4 It can be seen that Li-CO2 has excellent rate performance, small first-cycle polarization, and an overpotential of only 0.71 V at a current density of 1 C. The charging platform is around 3.1 V, indicating that the Co-based metal composite material regulated by N, S-CDs plays a role in reducing the charging platform.
[0062] See also Figure 5 , the long cycle curve of the positive electrode catalyst material of Li-CO2 battery at a current density of 400mA / g and a cut-off capacity of 1000mAh / g. Figure 5 , at high current density, Li-CO2 can stably operate for 520h, a total of 104 cycles, with good cycle stability. Compared with the single positive electrode catalyst of Co metal and carbon nanotube materials without N, S-CDs, such as Figure 8 As shown in the first cycle charge and discharge curve at a current density of 50 mA / g and a cutoff capacity of 1000 mAh / g, the electrocatalytic performance of the positive electrode of the Li-CO2 battery has been greatly improved, and it has broad application prospects in the field of Li-CO2 batteries. Comparative Example 1
[0063] Using carbon nanotubes as catalyst materials, the positive electrode sheet of Li-CO2 battery and Li-CO2 battery were prepared according to the methods of Examples 2 and 3, and then the electrochemical performance was tested according to the method in Example 3. The test results are as follows: Figure 8 shown. Comparative Example 2
[0064] A method for preparing a positive electrode catalyst material for a Li-CO2 battery comprises the following steps:
[0065] S1. Take 2.52g (~10mmol) Co(CHCOO)2·4H2O and 0.45g (~75mmol) urea, add them into 90mL deionized water and stir to dissolve. After they are completely dissolved, add 80mg multi-walled carbon nanotubes in batches into the above solution, stir for 10min and then ultrasonicate for 10min.
[0066] S2. Transfer the mixed solution to a reactor with a capacity of 120 ml, place it in a hydrothermal oven, hydroheat it at 120°C for 2 hours, and after cooling, wash it with deionized water 5 times, and then dry it at 60°C in a vacuum drying oven for 8 hours; calcine it at 500°C for 2 hours in a tubular furnace into which argon-hydrogen mixed gas is introduced, wherein the ratio of argon to hydrogen is 9:1, to obtain a composite catalyst material (Co@CNTs).
[0067] The SEM image of the composite catalyst material obtained in this comparative example is as follows Figure 6 shown.
[0068] The composite catalyst material of this comparative example was used to prepare a positive electrode sheet of a Li-CO2 battery and a Li-CO2 battery according to the methods of Examples 2 and 3, respectively. Then, the electrochemical performance was tested according to the method in Example 3. The test results are shown in FIG. Figure 8 shown. Comparative Example 3
[0069] A method for preparing a positive electrode catalyst material for a Li-CO2 battery comprises the following steps:
[0070] S1. Take 2.52g (~10mmol) Co(CHCOO)2·4H2O and 0.45g (~75mmol) urea, add them to 90mL deionized water and stir to dissolve. After they are completely dissolved, add 0.1g N,S-CDs and keep stirring until there are no solid particles.
[0071] S2. Transfer the mixed solution to a reactor with a capacity of 120 ml, place it in a hydrothermal oven, hydroheat it at 120°C for 2 hours, and after cooling, wash it with deionized water 5 times, and then dry it at 60°C in a vacuum drying oven for 8 hours; calcine it at 500°C for 2 hours in a tubular furnace into which an argon-hydrogen mixture is introduced, wherein the ratio of argon to hydrogen is 9:1, to obtain a Co-based metal composite catalyst material (Co-CDs) whose morphology is regulated by N, S-CDs.
[0072] The SEM image of the composite catalyst material obtained in this comparative example is as follows Figure 7 shown.
[0073] The positive electrode sheet of Li-CO2 battery and Li-CO2 battery were prepared according to the methods of Examples 2 and 3, respectively, and then the electrochemical performance was tested according to the method in Example 3. The test results are as follows: Figure 8 As shown; wherein, the catalyst material used in this comparative example is a mixed material obtained by mixing Co-CDs and carbon nanotubes prepared in this comparative example in a mass ratio of 8:1.
[0074] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0075] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a positive electrode catalyst composite material, characterized in that: The following steps are involved: S1, dissolving organic cobalt salt, urea, carbon dots and carbon nanotubes in water to obtain a precursor solution; S2, heating the precursor solution to perform a hydrothermal reaction, and after the reaction is completed, cooling and drying to obtain a precursor material; S3, calcining the precursor material in an argon-hydrogen mixed gas atmosphere to obtain the composite material; In step S2, the temperature of the hydrothermal reaction is 100-200°C; in step S3, the calcination temperature is 400-700°C; in the argon-hydrogen mixed gas, the volume ratio of argon to hydrogen is 8-9:1-2; The positive electrode catalyst composite material consists of carbon nanotubes and metal cobalt on the surface of the carbon nanotubes. The metal cobalt is highly dispersed and attached to the surface of the carbon nanotubes in the form of small particles.
2. The method for preparing the cathode catalyst composite material according to claim 1, characterized in that: The carbon dots are carbon dots doped with at least one of N, S and F.
3. A cathode catalyst composite material obtained by the preparation method according to any one of claims 1 to 2.
4. A positive electrode material, characterized in that Includes the positive electrode catalyst composite material as described in claim 3.
5. The positive electrode material according to claim 4, characterized in that It comprises 70-90% of the positive electrode catalyst composite material and 10-30% of a binder.
6. A positive electrode, characterized in that Comprising the positive electrode material according to claim 4 or 5.
7. A Li-CO2 battery, characterized in that: Comprising the positive electrode as claimed in claim 6.