Resin grinding wheel and preparation method and grinding method thereof

By using materials such as ceramic corundum, brown corundum, and zirconium corundum with compound binders such as liquid phenolic resin and epoxy compounds in the resin grinding wheel, the problems of brittleness and poor water resistance of the traditional resin grinding wheel are solved, and the grinding efficiency and stability are improved. , suitable for alkaline humid environments.

CN118514015BActive Publication Date: 2024-10-01珠海泰达砂轮有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410986189.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-01
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Due to the brittleness and poor water resistance of phenolic resin, traditional resin grinding wheels affect the grinding feel and stability of grinding performance, especially in alkaline humid environments.

Method used

Using a compound binder composed of ceramic corundum, brown corundum, zirconium corundum, liquid phenolic resin, epoxy compound, polyurethane resin and cryolite, a resin grinding wheel with good strength and toughness is formed through curing treatment to improve grinding efficiency and water resistance. .

Benefits of technology

Significantly improves the toughness, grinding efficiency and performance stability of the resin grinding wheel, extends its service life, and maintains good grinding performance in humid environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the field of grinding processing technology, and in particular to a resin grinding wheel and a preparation method and grinding method thereof. The resin grinding wheel is mainly made of the following components in parts by weight: 15-35 parts of ceramic corundum, 30-70 parts of brown corundum, 15-35 parts of zirconium corundum, 15-20 parts of phenolic resin powder, 6-10 parts of compound binder, 8-20 parts of cryolite and 0.5-2 parts of pigment; the compound binder includes 60%-90% of liquid phenolic resin, 0.5%-5% of epoxy compound, 4%-25% of polyurethane resin and 5%-10% of organic solvent in mass percentage. The resin grinding wheel of the present invention adopts a specific compound binder, which not only solves the problem of obvious brittleness of the existing phenolic resin binder after curing, but also ensures the grinding efficiency and improves the water resistance of the resin grinding wheel, thereby increasing the service life of the resin grinding wheel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of grinding processing, in particular to a resin grinding wheel and a preparation method and a grinding method thereof. Background Art

[0002] Grinding is a processing method that uses abrasives and grinding tools to cut on a grinding machine. It is one of the main methods for finishing parts. Grinding wheel is one of the main tools for grinding, which is mainly made of abrasives and binders. Grinding wheels are mainly divided into resin grinding wheels, ceramic grinding wheels, rubber grinding wheels, metal grinding wheels, etc. according to the type of binder. The performance of the binder has a significant impact on the strength, heat resistance, and service life of the grinding wheel. Phenolic resin is widely used in the preparation of resin grinding wheels due to its high strength.

[0003] However, when phenolic resin is used as a binder material in the preparation of resin grinding wheels, it is obviously brittle after curing and has poor water resistance, which not only affects the grinding feel of the grinding wheel, but also the stability of the grinding performance will be affected by the environment and deteriorate.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] One object of the present invention is to provide a resin grinding wheel that solves the brittleness problem of traditional resin grinding wheels, while improving grinding efficiency and durability, slowing down the performance degradation of the resin grinding wheel in an alkaline and humid environment, and improving the grinding feel.

[0006] Another object of the present invention is to provide a method for preparing a resin grinding wheel.

[0007] Another object of the present invention is to provide a grinding method using the resin grinding wheel.

[0008] In order to achieve the above-mentioned object of the present invention, the present invention provides a resin grinding wheel on one hand, which is mainly made of the following components in parts by weight:

[0009] 15-35 parts of ceramic corundum, 30-70 parts of brown corundum, 15-35 parts of zirconium corundum, 15-20 parts of phenolic resin powder, 6-10 parts of composite binder, 8-20 parts of cryolite and 0.5-2 parts of pigment;

[0010] The composite binder comprises, by mass percentage, 60% to 90% of liquid phenolic resin, 0.5% to 5% of epoxy compound, 4% to 25% of polyurethane resin and 5% to 10% of organic solvent;

[0011] The epoxy compound includes epoxy-containing silane compounds and epoxy compounds containing at least two epoxy groups.

[0012] In a specific embodiment of the present invention, in the epoxy compound, the mass ratio of the epoxy group-containing silane compound to the epoxy compound containing at least two epoxy groups is 1:(2-4).

[0013] In a specific embodiment of the present invention, in the composite binder, the mass ratio of the liquid phenolic resin to the epoxy compound is (20-30):1.

[0014] In a specific embodiment of the present invention, the epoxy compound containing at least two epoxy groups includes at least one of 1,6-hexanediol diglycidyl ether and glycerol tri(1,2-epoxy)propyl ether.

[0015] In a specific embodiment of the present invention, the epoxy-containing silane compound includes at least one of 3-glycidyl propoxy trimethoxy silane, [8-(epoxypropyloxy)-n-octyl] trimethoxy silane and triethoxy (3-epoxypropyloxypropyl) silane.

[0016] In a specific embodiment of the present invention, the polyurethane resin comprises a silane-modified polyurethane resin. Further, the silane-modified polyurethane resin accounts for 20 wt% to 40 wt% of the polyurethane resin.

[0017] In a specific embodiment of the present invention, the organic solvent includes an ether solvent. Further, the ether solvent includes at least one of propylene glycol methyl ether, ethylene glycol butyl ether and dipropylene glycol butyl ether.

[0018] Another aspect of the present invention provides a method for preparing any one of the above-mentioned resin grinding wheels, comprising the following steps:

[0019] (a) mixing ceramic corundum, brown corundum, zirconium corundum, a composite binder and a pigment to obtain a first mixed material;

[0020] (b) mixing phenolic resin powder and cryolite uniformly, and then mixing the mixture with the first mixed material to obtain a second mixed material;

[0021] (c) adding part of the second mixed material into a mold, then laying a reinforcing mesh and flattening it, then adding part of the second mixed material, laying a reinforcing mesh and flattening it, then adding the remaining amount of the second mixed material, pressing and molding it, and obtaining a grinding wheel blank;

[0022] (d) subjecting the grinding wheel blank to a curing treatment.

[0023] In a specific embodiment of the present invention, the curing treatment includes: preheating at 60±5°C for 2 to 3 hours, heating to 80±5°C at a heating rate of ≤7°C / h, then heating to 120±5°C at a heating rate of ≤10°C / h, and keeping at 120±5°C for 2 to 3 hours, then heating to 170±5°C at a heating rate of 10 to 15°C / h, and keeping at 170±5°C for 5 to 9 hours, and then cooling to room temperature at a cooling rate of ≤10°C / h.

[0024] Another aspect of the present invention provides a grinding method, comprising the following steps: grinding a workpiece using any one of the above-mentioned resin grinding wheels.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] (1) The resin grinding wheel of the present invention uses a liquid phenolic resin, an epoxy compound, a polyurethane resin, etc. as a binder for the resin grinding wheel, which not only solves the problem of obvious brittleness of the existing phenolic resin binder after curing, but also ensures the grinding efficiency and improves the water resistance of the resin grinding wheel, thereby increasing the service life of the resin grinding wheel;

[0027] (2) The preparation of the resin grinding wheel of the present invention is simple and requires mild conditions. By optimizing the formulation of the resin grinding wheel and the curing conditions, the toughness, grinding efficiency and performance stability of the resin grinding wheel can be significantly improved. DETAILED DESCRIPTION

[0028] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0029] On the one hand, the present invention provides a resin grinding wheel, which is mainly made of the following components in parts by weight:

[0030] 15-35 parts of ceramic corundum, 30-70 parts of brown corundum, 15-35 parts of zirconium corundum, 15-20 parts of phenolic resin powder, 6-10 parts of composite binder, 8-20 parts of cryolite and 0.5-2 parts of pigment;

[0031] The compound binder includes, by mass percentage, 60% to 90% of liquid phenolic resin, 0.5% to 5% of epoxy compound, 4% to 25% of polyurethane resin and 5% to 10% of organic solvent;

[0032] The epoxy compounds include epoxy-containing silane compounds and epoxy compounds containing at least two epoxy groups.

[0033] The resin grinding wheel of the present invention uses liquid phenolic resin, epoxy compound, polyurethane resin and the like as a binder for the resin grinding wheel, which not only solves the problem of obvious brittleness of the existing phenolic resin binder after curing, but also ensures grinding efficiency and improves the water resistance of the resin grinding wheel, thereby increasing the service life of the resin grinding wheel.

[0034] Among them, polyurethane resin is introduced into the composite binder, and the toughness of polyurethane resin is utilized to improve the brittleness of phenolic resin and improve the binding property with abrasives and the like; the addition of epoxy compound allows the epoxy group to react with the phenolic hydroxyl group of phenolic resin during the curing process. On the one hand, epoxy compound with more than two epoxy groups can react with the phenolic hydroxyl group to form a three-dimensional cross-linked network structure, thereby ensuring the strength and having a strong grip on abrasives, which helps to improve the grinding efficiency and avoid burns and microcracks on the workpiece surface; at the same time, side chains such as alkyl groups are added to the phenolic resin molecules, While improving strength, toughness is ensured; on the other hand, the epoxy groups in epoxy silane compounds can react with phenolic hydroxyl groups and introduce hydrolyzable segments into the phenolic resin molecules. During use, when there is moisture in the environment, the corresponding segments are hydrolyzed and cross-linked to form an elastomer with a Si-O-Si structure, which can bond with the abrasive surface, not only avoiding the destruction of the bonding effect between the phenolic resin and the abrasive by moisture, but also further improving the strength, toughness and water resistance, thereby ensuring the grinding efficiency and grinding feel of the resin grinding wheel. Furthermore, the introduction of some silicon molecular chains into the system can improve the heat resistance of the resin grinding wheel.

[0035] In the resin grinding wheel, the components are measured by weight, and the amounts used can be as follows, but are not limited thereto:

[0036] The amount of ceramic corundum can be 15 parts, 20 parts, 25 parts, 30 parts, 35 parts or a range consisting of any two of them;

[0037] The amount of brown corundum can be 30 parts, 40 parts, 50 parts, 60 parts, 70 parts or any two of them;

[0038] The amount of zirconium corundum can be 15 parts, 20 parts, 25 parts, 30 parts, 35 parts or any two of them;

[0039] The amount of phenolic resin powder can be 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts or a range consisting of any two of them;

[0040] The dosage of the composite binder can be 6 parts, 7 parts, 8 parts, 9 parts, 10 parts or a range consisting of any two of them;

[0041] The amount of cryolite can be 8 parts, 10 parts, 12 parts, 15 parts, 18 parts, 20 parts or any two of them;

[0042] The amount of the pigment can be 0.5 parts, 0.8 parts, 1 parts, 1.2 parts, 1.5 parts, 1.8 parts, 2 parts or a range consisting of any two of them.

[0043] For the composite binder, the liquid phenolic resin can wet the abrasive and dissolve the resin powder. The viscosity of the liquid phenolic resin of the present invention is 800-1200mpa·s, which ensures the wetting performance, makes the materials mixed evenly, and ensures the plasticity of the mixture. For example, in different embodiments, the viscosity of the liquid phenolic resin can be 800mpa·s, 900mpa·s, 1000mpa·s, 1100mpa·s, 1200mpa·s or a range consisting of any two of them. In the composite binder of the present invention, the mass percentage of the liquid phenolic resin can be 60%, 65%, 70%, 75%, 80%, 85%, 90% or a range consisting of any two of them. Avoid too little liquid phenolic resin, poor wetting performance, and poor mixing uniformity; also avoid too much liquid phenolic resin, and the toughness of the resin grinding wheel binder is poor.

[0044] In the composite binder, an appropriate amount of epoxy compound is used to fully crosslink the epoxy compound with the phenolic resin to improve the bonding strength and water resistance; on the other hand, too much epoxy compound is avoided, and excessive crosslinking in the system is avoided, resulting in the introduction of the polyurethane resin being unable to compensate for the brittleness of the phenolic resin, making the resin grinding wheel more prone to cracking and other problems. In the composite binder of the present invention, the mass percentage of the epoxy compound can be 0.5%, 1%, 2%, 3%, 4%, 5% or a range consisting of any two of them.

[0045] In the composite binder, the introduction of polyurethane resin is mixed with phenolic resin in the system to form an interpenetrating network structure, which can significantly improve the brittleness of the product. The present invention regulates the amount of polyurethane resin within a certain range, taking into account both improving brittleness and ensuring bonding performance. If the amount of polyurethane resin is too low, the improvement of brittleness cannot be achieved; if the amount of polyurethane resin is too high, the bonding performance between the abrasive and the binder in the resin grinding wheel will be insufficient. In the composite binder of the present invention, the mass percentage of polyurethane resin can be 4%, 5%, 8%, 10%, 15%, 20%, 25% or a range consisting of any two of them.

[0046] In the composite binder of the present invention, the mass percentage of the organic solvent can be 5%, 6%, 7%, 8%, 9%, 10% or a range consisting of any two of them, so as to fully wet the abrasive and dissolve the phenolic resin powder to ensure the uniformity of material mixing.

[0047] In a specific embodiment of the present invention, in the epoxy compound, the mass ratio of the epoxy group-containing silane compound to the epoxy compound containing at least two epoxy groups is 1:(2-4).

[0048] The present invention has been found in the research that the ratio of epoxy-containing silane compounds and epoxy compounds containing at least 2 epoxy groups in epoxy compounds will affect the grinding efficiency and performance stability of resin grinding wheels to a certain extent. When the amount of epoxy-containing silane compounds is lower than the above range, the water resistance and brittleness of the resin grinding wheel are not significantly improved; and when the amount of epoxy-containing silane compounds is higher than the above range, the water resistance and brittleness of the resin grinding wheel are improved, but the strength of the resin grinding wheel is insufficient, resulting in a significant reduction in grinding efficiency. For example, in different embodiments, in epoxy compounds, the mass ratio of epoxy-containing silane compounds and epoxy compounds containing at least 2 epoxy groups can be 1:2, 1:2.5, 1:3, 1:3.5, 1:4 or a range composed of any two of them, which can further take into account the improvement of the water resistance, brittleness and grinding efficiency of the resin grinding wheel.

[0049] In a specific embodiment of the present invention, in the composite binder, the mass ratio of the liquid phenolic resin to the epoxy compound is (20-30):1.

[0050] For example, in different embodiments, in the composite binder, the mass ratio of the liquid phenolic resin to the epoxy compound can be 20:1, 22:1, 25:1, 28:1, 30:1 or a range consisting of any two of them to better improve the various properties of the resin grinding wheel.

[0051] In a specific embodiment of the present invention, the epoxy compound containing at least two epoxy groups includes at least one of 1,6-hexanediol diglycidyl ether and glycerol tri(1,2-epoxy)propyl ether.

[0052] In a specific embodiment of the present invention, the epoxy group-containing silane compound includes at least one of 3-glycidyl propoxy trimethoxy silane, [8-(epoxypropyloxy)-n-octyl] trimethoxy silane and triethoxy (3-epoxypropyloxypropyl) silane.

[0053] In a specific embodiment of the present invention, the polyurethane resin includes a silane-modified polyurethane resin. Further, the silane-modified polyurethane resin accounts for 20 wt% to 40 wt% of the polyurethane resin.

[0054] By introducing part of the silane-modified polyurethane resin into the system, the polyurethane molecular chain can improve the toughness of the product. The introduction of part of the silane-modified polyurethane resin, in a water-containing environment, the silane alkoxyl group is hydrolyzed and cross-linked to form an elastomer with a Si-O-Si structure, and can be bonded to the abrasive surface, further improving the performance of the resin grinding wheel, and avoiding the performance attenuation in a humid environment. At the same time, the silane-modified polyurethane resin can react and bond with epoxy-containing silane compounds in a water-containing environment to improve the compatibility of phenolic resin molecules and polyurethane resins. And further research has found that if the polyurethane resin is all silane-modified polyurethane resin, not only the cost is increased, but also the silicon oxygen segments of the excessive silane-modified polyurethane resin tend to be enriched on the surface, resulting in uneven distribution of the polyurethane resin, so that the overall performance of the obtained resin grinding wheel is uneven. The present invention takes into account the water resistance, toughness, grinding efficiency and cost of the resin grinding wheel by regulating the proportion of silane-modified polyurethane resin in the polyurethane resin. For example, in different embodiments, the silane-modified polyurethane resin may account for 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt% of the weight of the polyurethane resin, or a range consisting of any two thereof.

[0055] In a specific embodiment of the present invention, the organic solvent includes an ether solvent. Further, the ether solvent includes at least one of propylene glycol methyl ether, ethylene glycol butyl ether and dipropylene glycol butyl ether.

[0056] In a specific embodiment of the present invention, the ceramic corundum is ceramic corundum 22# to 30#; the brown corundum includes brown corundum 24# to 36#; and the zirconium corundum is zirconium corundum 24# to 36#. Furthermore, in the brown corundum, the mass ratio of brown corundum 24# to brown corundum 30# is 1:1.

[0057] In a specific embodiment of the present invention, the particle size of the phenolic resin powder is 325 mesh.

[0058] In a specific embodiment of the present invention, the cryolite includes potassium cryolite and sodium cryolite in a mass ratio of 1: (0.8-1.2). Further, the particle size of the cryolite is 400 mesh.

[0059] In a specific embodiment of the present invention, the pigment comprises iron red. Further, the particle size of the pigment is 325 mesh.

[0060] Another aspect of the present invention provides a method for preparing any one of the above resin grinding wheels, comprising the following steps:

[0061] (a) mixing ceramic corundum, brown corundum, zirconium corundum, a composite binder and a pigment to obtain a first mixed material;

[0062] (b) mixing phenolic resin powder and cryolite uniformly, and then mixing the mixture with the first mixed material uniformly to obtain a second mixed material;

[0063] (c) adding part of the second mixed material into the mold, then laying a reinforcing mesh and flattening it, then adding part of the second mixed material, laying a reinforcing mesh and flattening it, then adding the remaining second mixed material, pressing and molding it, and obtaining a grinding wheel blank;

[0064] (d) The grinding wheel blank is cured.

[0065] In actual operation, the reinforcing mesh can be glass fiber mesh, carbon fiber mesh, etc. commonly used in existing resin grinding wheels, for example, the woven glass fiber fabric is impregnated in a resin impregnant and dried. The present invention is not limited to the type of reinforcing mesh, and conventional glass fiber reinforced mesh cloth, etc. can be used. In step (c), the second mixed material is added three times, and the ratio of the amount of the second mixed material added three times can be 3:4:5, but is not limited thereto.

[0066] In a specific embodiment of the present invention, the curing treatment includes: preheating at 60±5°C for 2 to 3 hours, heating to 80±5°C at a heating rate of ≤7°C / h, then heating to 120±5°C at a heating rate of ≤10°C / h, and keeping at 120±5°C for 2 to 3 hours, then heating to 170±5°C at a heating rate of 10 to 15°C / h, and keeping at 170±5°C for 5 to 9 hours, and then cooling to room temperature at a cooling rate of ≤10°C / h.

[0067] The present invention combines the formula of the resin grinding wheel to adjust the curing conditions, and further improves the grinding feel, grinding efficiency and performance stability of the resin grinding wheel. For example, in different embodiments, the heating rate from 60±5℃ to 80±5℃ can be 4℃ / h, 5℃ / h, 6℃ / h, 7℃ / h, etc.; the heating rate from 80±5℃ to 120±5℃ can be 5℃ / h, 6℃ / h, 8℃ / h, 10℃ / h, etc.; the heating rate from 120±5℃ to 170±5℃ can be 10℃ / h, 12℃ / h, 15℃ / h, etc.; the cooling rate from 170±5℃ to room temperature can be 5℃ / h, 6℃ / h, 8℃ / h, 10℃ / h, etc. The insulation time at 120±5°C can be 2h, 2.5h, 3h, etc., and the insulation time at 170±5°C can be 5h, 6h, 7h, 8h, 9h, etc.

[0068] In a specific embodiment of the present invention, during the compression molding, the temperature of the mold is 45-50° C., the compression pressure is 5-10 MPa, and the holding time is ≥2.5 s.

[0069] Another aspect of the present invention provides a grinding method, comprising the following steps: grinding a workpiece using any one of the above-mentioned resin grinding wheels.

[0070] The resin grinding wheel of the present invention can be made into resin grinding wheels with different specifications according to actual needs, such as resin grinding wheels with diameters of 100 mm, 125 mm, 150 mm, 180 mm, etc., but is not limited thereto.

[0071] When the resin grinding wheel (with a diameter of 100 mm, a hole diameter of 16 mm, and a thickness of 6 mm) of the present invention is used to grind a workpiece, such as a Q235 workpiece, the grinding ratio can reach 7 to 13, preferably 8 to 10; the grinding efficiency can reach 8 to 18 g / min, preferably 14 to 18 g / min; and the workpiece can be prevented from being burned.

[0072] The grinding ratio can be 8, 9, 10, 11, 12, 13 or any two of them, and the grinding efficiency can be 8g / min, 9g / min, 10g / min, 11g / min, 12g / min, 13g / min, 14g / min, 15g / min, 16g / min, 18g / min or any two of them. The grinding performance of the resin grinding wheel of the present invention can significantly improve the grinding efficiency, while ensuring a certain grinding ratio to avoid burning the workpiece.

[0073] The grinding wheel of the present invention has a rotational strength of 23,000 to 27,000 rpm. When the grinding wheel of the present invention is immersed in water at room temperature (25±2° C.) for 2 hours, the decrease rate of the rotational strength is ≤3.2%, preferably ≤2.5%.

[0074] The information of some materials used in the following specific embodiments may be as follows, but is not limited thereto:

[0075] Liquid phenolic resin, manufacturer: Zhuhai Bangrui Synthetic Materials Co., Ltd., model 2508;

[0076] Phenolic resin powder, manufacturer: Zhuhai Bangrui Synthetic Materials Co., Ltd., model 25100;

[0077] Polyurethane resin, manufacturer: Shenzhen Jitian Chemical Co., Ltd., model 1624;

[0078] Silane modified polyurethane resin, manufacturer: BOSTIK, model ISR 70-03.

[0079] Example 1

[0080] The present embodiment provides a resin grinding wheel and a preparation method thereof. The resin grinding wheel is mainly prepared from the following components in parts by weight: 25 parts of ceramic corundum 24#, 25 parts of brown corundum 24#, 25 parts of brown corundum 30#, 25 parts of zirconium corundum 30#, 18 parts of 325 mesh phenolic resin powder, 8 parts of composite binder, 7 parts of 400 mesh potassium cryolite, 7 parts of 400 mesh sodium cryolite and 1 part of 325 mesh pigment iron red.

[0081] The composite binder includes 75% of liquid phenolic resin, 3% of epoxy compound, 14% of polyurethane resin and 8% of propylene glycol methyl ether by mass percentage; the epoxy compound includes 3-glycidyl propoxy trimethoxy silane and 1,6-hexanediol diglycidyl ether in a mass ratio of 1:3. In the polyurethane resin, the mass proportion of silane-modified polyurethane resin is 30%.

[0082] The preparation method of the composite binder comprises: stirring and mixing polyurethane resin and propylene glycol methyl ether evenly, then adding liquid phenolic resin and stirring evenly, and then adding epoxy compound and stirring evenly to obtain the composite binder.

[0083] The preparation method of the resin grinding wheel comprises the following steps:

[0084] (1) Ceramic corundum 24#, brown corundum 24#, brown corundum 30#, zirconium corundum 30#, a composite binder and pigment iron red are stirred (for about 20 to 30 minutes) until they are uniformly mixed to obtain a first mixed material;

[0085] (2) Phenolic resin powder, potassium cryolite and sodium cryolite are mixed evenly, and then added into the first mixed material and stirred (for about 20 to 30 minutes) to obtain a second mixed material;

[0086] (3) Add the second mixed material into the mold, spread the material in a rotating manner, lay the first glass fiber reinforced mesh and flatten it, then add a portion of the second mixed material, spread the material in a rotating manner, lay the second glass fiber reinforced mesh and flatten it, then add a portion of the second mixed material, and press it into shape to obtain a grinding wheel blank; wherein, the spreading time is 4 to 5 seconds, and the second mixed material is added three times, and the ratio of the amount of the second mixed material added is 1:1:1; during the pressing and molding, the mold temperature is 45°C, the press pressure is 10 MPa, and the holding time is 8 seconds.

[0087] (4) Curing the grinding wheel blank to obtain a resin grinding wheel; the curing treatment includes: preheating at 60°C for 2h, heating to 80°C at a heating rate of 5°C / h, then heating from 80°C to 120°C at a heating rate of 10°C / h, and keeping at 120°C for 2.5h, then heating to 170°C at a heating rate of 10°C / h, and keeping at 170°C for 7h, and then cooling from 170°C to room temperature at a cooling rate of 10°C / h.

[0088] Example 2

[0089] This embodiment refers to the resin grinding wheel and preparation method thereof of Example 1, with the only difference being that the composition of the epoxy compound in the composite binder is different.

[0090] In this embodiment, the epoxy compound includes 3-glycidyl propoxy trimethoxy silane and 1,6-hexanediol diglycidyl ether in a mass ratio of 1:2.

[0091] Example 3

[0092] This embodiment refers to the resin grinding wheel and preparation method thereof of Example 1, with the only difference being that the composition of the epoxy compound in the composite binder is different.

[0093] In this embodiment, the epoxy compound includes 3-glycidyl propoxy trimethoxy silane and 1,6-hexanediol diglycidyl ether in a mass ratio of 1:4.

[0094] Example 4

[0095] This embodiment refers to the resin grinding wheel and preparation method thereof of Example 1, with the only difference being that the composition of the epoxy compound in the composite binder is different.

[0096] In this embodiment, the epoxy compound includes 3-glycidyl propoxy trimethoxy silane and 1,6-hexanediol diglycidyl ether in a mass ratio of 1:1.

[0097] Example 5

[0098] This embodiment refers to the resin grinding wheel and preparation method thereof of Example 1, with the only difference being that the composition of the epoxy compound in the composite binder is different.

[0099] In this embodiment, the epoxy compound includes 3-glycidyl propoxy trimethoxy silane and 1,6-hexanediol diglycidyl ether in a mass ratio of 1:5.

[0100] Example 6

[0101] This embodiment refers to the resin grinding wheel and preparation method thereof of Example 1, the only difference being that the amount of epoxy compound used in the composite binder is different.

[0102] In this embodiment, the composite binder includes, by mass percentage, 75% of liquid phenolic resin, 3.75% of epoxy compound, 14% of polyurethane resin and 7.25% of propylene glycol methyl ether.

[0103] Example 7

[0104] This embodiment refers to the resin grinding wheel and preparation method thereof of Example 1, the only difference being that the amount of epoxy compound used in the composite binder is different.

[0105] In this embodiment, the composite binder includes, by mass percentage, 75% of liquid phenolic resin, 2.5% of epoxy compound, 14% of polyurethane resin and 8.5% of propylene glycol methyl ether.

[0106] Example 8

[0107] This embodiment refers to the resin grinding wheel and preparation method thereof of Example 1, the only difference being that the amount of epoxy compound used in the composite binder is different.

[0108] In this embodiment, the composite binder includes, by mass percentage, 75% of liquid phenolic resin, 1% of epoxy compound, 14% of polyurethane resin and 10% of propylene glycol methyl ether.

[0109] Example 9

[0110] This embodiment refers to the resin grinding wheel and preparation method thereof of Example 1, the only difference being that the amount of epoxy compound used in the composite binder is different.

[0111] In this embodiment, the composite binder includes, by mass percentage, 75% of liquid phenolic resin, 5% of epoxy compound, 14% of polyurethane resin and 6% of propylene glycol methyl ether.

[0112] Example 10

[0113] This embodiment refers to the resin grinding wheel and preparation method thereof of embodiment 1, the only difference being that the composition of the polyurethane resin in the compound binder is different.

[0114] In this embodiment, the mass proportion of the silane-modified polyurethane resin in the polyurethane resin is 20%.

[0115] Embodiment 11

[0116] This embodiment refers to the resin grinding wheel and preparation method thereof of embodiment 1, the only difference being that the composition of the polyurethane resin in the compound binder is different.

[0117] In this embodiment, the mass proportion of the silane-modified polyurethane resin in the polyurethane resin is 40%.

[0118] Example 12

[0119] This embodiment refers to the resin grinding wheel and preparation method thereof of embodiment 1, the only difference being that the composition of the polyurethane resin in the compound binder is different.

[0120] In this embodiment, the mass proportion of the silane-modified polyurethane resin in the polyurethane resin is 10%.

[0121] Embodiment 13

[0122] This embodiment refers to the resin grinding wheel and preparation method thereof of embodiment 1, the only difference being that the composition of the polyurethane resin in the compound binder is different.

[0123] In this embodiment, the mass proportion of the silane-modified polyurethane resin in the polyurethane resin is 50%.

[0124] Embodiment 14

[0125] This embodiment refers to the resin grinding wheel and its preparation method of embodiment 1, the only difference is that the curing treatment in step (4) is different.

[0126] In this embodiment, the curing treatment includes: after preheating at 60°C for 2h, heating up to 80°C at a heating rate of 5°C / h, then heating from 80°C to 100°C at a heating rate of 10°C / h, and keeping at 100°C for 1h, then heating to 120°C at a heating rate of 10°C / h, and keeping at 120°C for 1.5h, then heating to 170°C at a heating rate of 10°C / h, and keeping at 170°C for 7h, and then cooling from 170°C to room temperature at a cooling rate of 10°C / h.

[0127] Comparative Example 1

[0128] Comparative Example 1 refers to the resin grinding wheel and preparation method thereof of Example 1, except that an equal weight of liquid phenolic resin is used to replace the composite binder in Example 1.

[0129] Comparative Example 2

[0130] Comparative Example 2 refers to the resin grinding wheel and preparation method thereof of Example 1, except that: the composition of the epoxy compound in the composite binder is different.

[0131] In Comparative Example 2, the epoxy compound only includes 3-glycidylpropoxytrimethoxysilane.

[0132] Comparative Example 3

[0133] Comparative Example 3 refers to the resin grinding wheel and preparation method thereof of Example 1, except that: the composition of the epoxy compound in the composite binder is different.

[0134] In Comparative Example 3, the epoxy compound includes only 1,6-hexanediol diglycidyl ether.

[0135] Comparative Example 4

[0136] Comparative Example 4 refers to the resin grinding wheel and preparation method thereof of Example 1, except that the amount of the epoxy compound in the composite binder is different.

[0137] In Comparative Example 4, the composite binder includes, by mass percentage, 75% of liquid phenolic resin, 0.2% of epoxy compound, 14% of polyurethane resin and 10.8% of propylene glycol methyl ether.

[0138] Comparative Example 5

[0139] Comparative Example 5 refers to the resin grinding wheel and preparation method thereof of Example 1, except that the amount of the epoxy compound in the composite binder is different.

[0140] In Comparative Example 5, the composite binder includes, by mass percentage, 75% of liquid phenolic resin, 6% of epoxy compound, 14% of polyurethane resin and 5% of propylene glycol methyl ether.

[0141] Comparative Example 6

[0142] Comparative Example 6 refers to the resin grinding wheel and preparation method thereof of Example 1, except that: the amounts of the components in the compound binder are different.

[0143] In Comparative Example 6, the composite binder includes, by mass percentage, 87% of liquid phenolic resin, 3% of epoxy compound, 2% of polyurethane resin and 8% of propylene glycol methyl ether.

[0144] Comparative Example 7

[0145] Comparative Example 7 refers to the resin grinding wheel and preparation method thereof of Example 1, except that: the amounts of the components in the compound binder are different.

[0146] In Comparative Example 7, the composite binder includes, by mass percentage, 60% of liquid phenolic resin, 3% of epoxy compound, 29% of polyurethane resin and 8% of propylene glycol methyl ether.

[0147] Experimental Example 1

[0148] Each embodiment and comparative example was processed into a resin grinding wheel of the same size, with a diameter of 100 mm, a hole diameter of 16 mm, and a thickness of 6 mm (the specifications of the resin grinding wheel used in the maximum single-point lateral load test are: a diameter of 180 mm, a hole diameter of 22.2 mm, and a thickness of 6 mm). The performance of the resin grinding wheel was tested, and each resin grinding wheel was used to grind a Q235 material workpiece, and the following parameter tests were performed. The test results are shown in Table 1.

[0149] Maximum single-point lateral load: tested according to JB / T 4175-2016 and GB 2494-2003;

[0150] Grinding wheel rotation strength: tested according to GB / T 2493-2013;

[0151] Water resistance: Test the initial rotation strength X0 of the grinding wheel, then soak the resin grinding wheel in room temperature water for 2 hours, and then test the rotation strength X1 of the grinding wheel again. Calculate the decrease rate of rotation strength = (X0-X1) / X0, which reflects the water resistance;

[0152] The test method for grinding performance of grinding wheels refers to the standard JB / T 3715-2016.

[0153] Table 1 Test results of different resin grinding wheels

[0154]

[0155] From the above test results, it can be seen that the resin grinding wheel of the present invention, by compounding liquid phenolic resin, epoxy compound, polyurethane resin, etc. as the binder of the resin grinding wheel, not only solves the problem of obvious brittleness of the existing phenolic resin binder after curing, but also ensures the grinding efficiency and improves the water resistance of the resin grinding wheel, thereby increasing the service life of the resin grinding wheel.

[0156] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. Resin grinding wheel, characterized in that: It is mainly made of the following components by weight: 15-35 parts of ceramic corundum, 30-70 parts of brown corundum, 15-35 parts of zirconium corundum, 15-20 parts of phenolic resin powder, 6-10 parts of composite binder, 8-20 parts of cryolite and 0.5-2 parts of pigment; The composite binder comprises, by mass percentage, 60% to 90% of liquid phenolic resin, 0.5% to 5% of epoxy compound, 4% to 25% of polyurethane resin and 5% to 10% of organic solvent; The epoxy compound includes epoxy-containing silane compounds and epoxy compounds containing at least 2 epoxy groups; In the composite binder, the mass ratio of the liquid phenolic resin to the epoxy compound is (20-30):1; The epoxy compound containing at least two epoxy groups includes at least one of 1,6-hexanediol diglycidyl ether and glycerol tri(1,2-epoxy)propyl ether.

2. The resin grinding wheel according to claim 1, characterized in that: In the epoxy compound, the mass ratio of the epoxy group-containing silane compound to the epoxy compound containing at least two epoxy groups is 1:(2-4).

3. The resin grinding wheel according to claim 1, characterized in that: The epoxy-containing silane compound includes at least one of 3-glycidyl propoxy trimethoxy silane, [8-(epoxypropyloxy)-n-octyl] trimethoxy silane and triethoxy (3-epoxypropyloxypropyl) silane.

4. The resin grinding wheel according to claim 1, characterized in that: The polyurethane resin includes a silane-modified polyurethane resin.

5. The resin grinding wheel according to claim 4, characterized in that: The silane-modified polyurethane resin accounts for 20 wt % to 40 wt % of the polyurethane resin.

6. The resin grinding wheel according to claim 1, characterized in that: The organic solvent includes an ether solvent; the ether solvent includes at least one of propylene glycol methyl ether, ethylene glycol butyl ether and dipropylene glycol butyl ether.

7. The method for preparing a resin grinding wheel according to any one of claims 1 to 6, characterized in that: The steps include: (a) mixing ceramic corundum, brown corundum, zirconium corundum, a composite binder and a pigment to obtain a first mixed material; (b) mixing phenolic resin powder and cryolite uniformly, and then mixing the mixture with the first mixed material to obtain a second mixed material; (c) adding part of the second mixed material into a mold, then laying a reinforcing mesh and flattening it, then adding part of the second mixed material, laying a reinforcing mesh and flattening it, then adding the remaining amount of the second mixed material, pressing and molding it, and obtaining a grinding wheel blank; (d) subjecting the grinding wheel blank to a curing treatment.

8. The method for preparing a resin grinding wheel according to claim 7, characterized in that: The curing treatment includes: preheating at 60±5°C for 2 to 3 hours, heating to 80±5°C at a heating rate of ≤7°C / h, then heating to 120±5°C at a heating rate of ≤10°C / h, and keeping at 120±5°C for 2 to 3 hours, then heating to 170±5°C at a heating rate of 10 to 15°C / h, and keeping at 170±5°C for 5 to 9 hours, and then cooling to room temperature at a cooling rate of ≤10°C / h.

9. A grinding method, characterized in that: The method comprises the following steps: grinding a workpiece using the resin grinding wheel described in any one of claims 1 to 6 or the resin grinding wheel prepared by the preparation method described in any one of claims 7 to 8.