Fireproof gypsum board and preparation method thereof

By adding reinforcing fibers and modified polyacrylate to the gypsum board, and coating the surface with epoxy phenolic resin, the problem of insufficient strength and fire resistance of the gypsum board is solved, and higher strength and stability are achieved.

CN118515462BActive Publication Date: 2024-10-11FUXIN TAISHAN GYPSUM BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410987823.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-11
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Existing gypsum boards have deficiencies in strength and fire stability, especially when glass fiber is added.

Method used

A board core including gypsum, reinforcing fibers, water reducing agent and tackifier is used, and epoxy phenolic resin is coated on the surface to form a protective film. The strength of the gypsum board is enhanced through the curing of the epoxy phenolic resin and the polymer cross-linking structure. and fire resistance.

Benefits of technology

Significantly improves the strength and fire stability of fire-resistant gypsum boards, ensuring the board's performance in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a fireproof gypsum board and a preparation method thereof, and relates to the technical field of gypsum board preparation. The fireproof gypsum board in the invention is composed of a board core and a protective film; the board core includes gypsum, reinforcing fiber, a water reducer, a foaming agent and a tackifier, and the protective film is an epoxy phenolic resin; the tackifier is a modified polyacrylate; the modified polyacrylate is obtained by reacting terminal amino hyperbranched siloxane with maleic anhydride after ring-opening reaction, and then reacting with butyl acrylate, methyl methacrylate, hydroxyethyl acrylate and glycidyl methacrylate; the epoxy phenolic resin is obtained by reacting epoxy hydrogen silicone oil, tetramethyl disiloxane, ethyl orthosilicate and phenyl molybdate; the epoxy phenolic resin is coated on the surface of the board core and cured, and the epoxy phenolic resin forms hydrogen bonds with the board core, adheres to the surface of the board core, and enhances the strength and fire stability of the gypsum board.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gypsum board preparation, in particular to a fireproof gypsum board and a preparation method thereof. Background Art

[0002] Gypsum board is one of the new lightweight boards that are currently being developed due to its relatively light weight, high strength, thin thickness, easy processing, sound insulation, heat insulation and fire resistance. At present, gypsum board has been widely used in various buildings such as residences, office buildings, shops, hotels and industrial plants for interior partitions, ceilings, sound-absorbing panels, ground base panels and various decorative panels.

[0003] The strength and fire stability of gypsum board are two key points that customers pay attention to. In order to further improve the strength and fire stability of gypsum board, many gypsum board manufacturers have adopted the method of adding glass fiber to gypsum board, but it is often not ideal. Therefore, the present invention studies and prepares a high temperature resistant gypsum board to solve this problem. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a fireproof gypsum board with high heat resistance by adding glass fiber into the gypsum board.

[0005] The present invention proposes a technical solution to solve the above technical problems: a fireproof gypsum board, comprising a board core and a protective film; the board core comprises gypsum, reinforcing fiber, a water reducer, a foaming agent and a tackifier; the protective film is epoxy phenolic resin cured on the surface of the board core; the epoxy phenolic resin is prepared by reacting epoxy hydrogen silicone oil, tetramethyldisiloxane, ethyl orthosilicate and phenyl molybdate; the tackifier is modified polyacrylate; the modified polyacrylate is prepared by reacting terminal amino hyperbranched siloxane with maleic anhydride after ring-opening reaction, and then reacting with butyl acrylate, methyl methacrylate, hydroxyethyl acrylate and glycidyl methacrylate, under the emulsification of a composite emulsifier and the action of an initiator ammonium persulfate.

[0006] Preferably, the reinforcing fiber is hydroxyl glass fiber; the foaming agent is sodium lauryl sulfate; and the water reducing agent is sodium hexametaphosphate.

[0007] Preferably, the method for preparing the fireproof gypsum board comprises the following specific steps:

[0008] S1. The amino-terminated hyperbranched siloxane, maleic anhydride and isopropanol were mixed in a mass ratio of 50-70:15:3, heated to 72-76°C, reacted for 3-4h, and distilled under reduced pressure to obtain a carboxyl-terminated hyperbranched siloxane;

[0009] S2. Butyl acrylate, methyl methacrylate, hydroxyethyl acrylate and glycidyl methacrylate are mixed in a mass ratio of 10:10:1~1.4:0.3~0.6, and 0.6~0.9 times the mass of butyl acrylate carboxyl-terminated hyperbranched siloxane and 0.1~0.2 times the mass of butyl acrylate are added. The compound emulsifier is emulsified at 600~800rpm for 20~40min, the temperature is raised to 70~72°C, and an initiator is added in an amount of 0.2~0.3 times the mass of butyl acrylate. The temperature is raised to 80~82°C, and 0.2~0.3 times the mass of butyl acrylate is added every 30min. The initiator is a 2.5% ammonium persulfate solution by mass. After reacting for 4~6h, the reaction is kept warm for 1~2h, and the temperature is lowered to 38~42°C. The modified polyacrylate is obtained by discharging the material, which is a tackifier;

[0010] S3. Tetramethyldisiloxane, ethyl orthosilicate, ethanol, 1-3 mol / L hydrochloric acid and deionized water were mixed in a mass ratio of 1:0.9:10:3-5:20, heated to 80-90°C, reacted for 2-4 hours, added with an epoxy hydrogen silicone oil of the same mass as tetramethyldisiloxane and phenyl molybdate of 1.6-1.8 times the mass of tetramethyldisiloxane, cooled to 68-72°C, added with 0.03-0.05 times the mass of tetramethyldisiloxane sodium hydroxide, continued to react for 4-6 hours, and vacuum evaporated to obtain epoxy phenolic resin;

[0011] S4. Mix gypsum and reinforcing fiber, disperse them ultrasonically at 40-85kHz for 20-30min, add water reducing agent sodium hexametaphosphate, foaming agent sodium dodecyl sulfate and tackifier, and stir evenly to obtain a board core; mix boron trifluoride monoethylamine and ethylene glycol at a mass ratio of 1:5-6, stir evenly, add epoxy phenolic resin with a mass of 10-18 times that of boron trifluoride monoethylamine, stir evenly, and keep warm at 125-135℃ for 1.5-2.5h to obtain a protective film; pour the board core into a flat plate forming machine, apply the protective film on the surface of the board core, and cure for 6-8h to obtain a fireproof gypsum board

[0012] Preferably, in the above step S1, the preparation method of the amino-terminated hyperbranched siloxane is: heating allyl glycidyl ether to 60-80° C., adding a catalyst of 0.02-0.04 times the mass of allyl glycidyl ether at a rate of 1-3 ml / min, wherein the catalyst is an isopropanol solution of chloroplatinic acid with a mass fraction of 20-30%, and then adding 3,3-tetramethyldisiloxane of 0.5-0.7 times the mass of allyl glycidyl ether at a rate of 2-4 ml / min, reacting for 3-5 hours, cooling to room temperature, and then adding diethylenetriamine of 1-3 times the mass of allyl glycidyl ether at a rate of 2-4 ml / min, heating to 70-90° C., reacting for 2-4 hours, heating to 220-230° C., and reacting for 30-50 minutes to obtain the amino-terminated hyperbranched siloxane.

[0013] Preferably, in the above step S2, the compound emulsifier is prepared by mixing alkylphenol polyoxyethylene ether, sodium lauryl sulfate and deionized water in a mass ratio of 1:1:20-30.

[0014] Preferably, in the above step S3, the preparation method of the epoxy hydrogenated silicone oil is: toluene, KH-560 and platinum catalyst are mixed in a mass ratio of 8:30~50:0.4~0.5, heated to 95~105°C for reaction for 3~4h, then heated to 145~155°C for reaction for 5~6h, cooled to 78~82°C, distilled under reduced pressure, and then added with hydrogenated silicone oil 1.1~1.2 times the mass of toluene, and then added with platinum catalyst 0.01~0.03 times the mass of toluene, heated to 95~105°C for reaction for 3~4h, cooled to 78~82°C, and distilled under reduced pressure to obtain the epoxy hydrogenated silicone oil.

[0015] Preferably, in the above step S4, the preparation method of the reinforcing fiber is: heating the glass fiber to 400-450°C, heat-insulating for 1-2 hours, cooling to room temperature, immersing in 3-5 mol / L hydrochloric acid at 80-100°C, taking out after 8-10 hours and washing with deionized water for 8-10 times, and drying to obtain hydroxyl glass fiber, i.e., the reinforcing fiber.

[0016] Preferably, in the above step S4, the thickness of the protective film is 8-10 μm.

[0017] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0018] The fireproof gypsum board of the present invention is composed of a board core and a protective film; the board core includes gypsum, reinforcing fiber, water reducing agent, foaming agent and tackifier, the protective film is epoxy phenolic resin solidified on the surface of the board core; the tackifier is modified polyacrylate;

[0019] The modified polyacrylate is prepared by reacting amino-terminated hyperbranched siloxane with maleic anhydride through a ring-opening reaction, and then reacting with butyl acrylate, methyl methacrylate, hydroxyethyl acrylate and glycidyl methacrylate; amino-terminated hyperbranched siloxane reacts with maleic anhydride through a ring-opening reaction to form a hyperbranched siloxane with a terminal carboxyl structure, which is introduced into the polyacrylate together with glycidyl methacrylate to form a polyacrylate with a long carbon chain structure containing epoxy groups and polycarboxyl groups, which can induce high molecular cross-linking in the board core, not only has excellent viscosity, but also can react with hydroxyl groups on the surface of reinforcing fibers to uniformly disperse the reinforcing fibers in the board core, thereby enhancing the strength and fire stability of the fireproof gypsum board;

[0020] Epoxy phenolic resin is prepared by the reaction of epoxy hydrogen silicone oil, tetramethyl disiloxane, ethyl orthosilicate and phenyl molybdate; after hydrolysis, tetramethyl disiloxane and ethyl orthosilicate can be condensed with phenyl molybdate to form phenolic resin, silicon and molybdenum are bonded to the main chain of the phenolic resin molecule with high bond energy chemical bonds, and epoxy hydrogen silicone oil is introduced during the reaction to form epoxy phenolic resin with an epoxy cross-linking structure, thereby enhancing fire stability; the epoxy phenolic resin is coated on the surface of the board core and cured, hydrogen bonds are formed between the epoxy phenolic resin and the board core, and the epoxy phenolic resin adheres to the surface of the board core, thereby enhancing the strength and fire stability of the gypsum board. DETAILED DESCRIPTION

[0021] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention. Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art.

[0022] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the test methods of various indicators of the fireproof gypsum boards prepared in the examples and comparative examples as follows:

[0023] Strength: The fireproof gypsum boards prepared in the examples and comparative examples were subjected to a breaking load test according to GB / T9775.

[0024] Fire stability: The fire retardant gypsum prepared in the examples and comparative examples was tested for fire stability according to GB / T9775.

[0025] Example 1

[0026] The preparation method of the fireproof gypsum board in this embodiment is:

[0027] S1. The allyl glycidyl ether is heated to 60°C, and a catalyst of 0.02 times the mass of the allyl glycidyl ether is added dropwise at a rate of 1 ml / min, wherein the catalyst is an isopropanol solution of chloroplatinic acid with a mass fraction of 20%, and then 3,3-tetramethyldisiloxane of 0.5 times the mass of the allyl glycidyl ether is added dropwise at a rate of 2 ml / min, and the reaction is carried out for 3 hours. The mixture is cooled to room temperature, and then diethylenetriamine of 1 times the mass of the allyl glycidyl ether is added dropwise at a rate of 2 ml / min, and the temperature is raised to 70°C, and the reaction is carried out for 2 hours. The temperature is raised to 220°C, and the reaction is carried out for 30 minutes to obtain an amino-terminated hyperbranched siloxane; amino-terminated hyperbranched siloxane, maleic anhydride, and isopropanol are mixed in a mass ratio of 50:15:3, the temperature is raised to 72°C, the reaction is carried out for 3 hours, and the mixture is distilled under reduced pressure to obtain a carboxyl-terminated hyperbranched siloxane;

[0028] S2. Butyl acrylate, methyl methacrylate, hydroxyethyl acrylate and glycidyl methacrylate were mixed in a mass ratio of 10:10:1:0.3, and a compound emulsifier of 0.6 times the mass of butyl acrylate and 0.1 times the mass of butyl acrylate was added, wherein the compound emulsifier was prepared by mixing alkylphenol polyoxyethylene ether, sodium lauryl sulfate and deionized water in a mass ratio of 1:1:20, emulsified at 600rpm for 20min, heated to 70°C, added with an initiator of 0.2 times the mass of butyl acrylate, heated to 80°C, and added with an initiator of 0.2 times the mass of butyl acrylate every 30min, wherein the initiator was a 2.5% ammonium persulfate solution by mass, reacted for 4h, kept warm for 1h, cooled to 38°C, and the modified polyacrylate was obtained by discharging the material, i.e., a tackifier;

[0029] S3. Toluene, KH-560 and platinum catalyst were mixed in a mass ratio of 8:30:0.4, heated to 95°C for reaction for 3h, then heated to 145°C for reaction for 5h, cooled to 78°C, and distilled under reduced pressure, and then 1.1 times the mass of toluene was added with hydrogen-containing silicone oil, and then 0.01 times the mass of toluene was added with platinum catalyst, heated to 95°C for reaction for 3h, cooled to 78°C, and distilled under reduced pressure to obtain epoxy hydrogen-containing silicone oil; tetramethyl disiloxane Alkane, tetraethyl orthosilicate, ethanol, 1 mol / L hydrochloric acid and deionized water were mixed in a mass ratio of 1:0.9:10:3:20, heated to 80°C, reacted for 2h, added with epoxy hydrogen silicone oil of the same mass as tetramethyldisiloxane and phenyl molybdate of 1.6 times the mass of tetramethyldisiloxane, cooled to 68°C, added with sodium hydroxide of 0.03 times the mass of tetramethyldisiloxane, continued to react for 4h, and evaporated under reduced pressure to obtain epoxy phenolic resin;

[0030] S4. The glass fiber is heated to 400°C, kept warm for 1 hour, cooled to room temperature, immersed in 3 mol / L hydrochloric acid at 80°C, taken out after 8 hours, washed 8 times with deionized water, and dried to obtain hydroxyl glass fiber, i.e., reinforcing fiber; gypsum and reinforcing fiber are mixed, ultrasonically dispersed at 40kHz for 20 minutes, and then a water reducer, sodium hexametaphosphate, a foaming agent, sodium dodecyl sulfate and a viscosity enhancer are added, and stirred evenly to obtain a board core; boron trifluoride monoethylamine and ethylene glycol are mixed in a mass ratio of 1:5, stirred evenly, and then an epoxy phenolic resin with a mass of 10 times that of boron trifluoride monoethylamine is added, stirred evenly, and kept warm at 125°C for 1.5 hours to obtain a protective film; the board core is poured into a flat plate forming machine, and a protective film is applied to the surface of the board core, the thickness of the protective film is 8μm, and cured for 6 hours to obtain a fireproof gypsum board.

[0031] Example 2

[0032] The preparation method of the fireproof gypsum board in this embodiment is:

[0033] S1. heating allyl glycidyl ether to 70°C, dropping a catalyst of 0.03 times the mass of allyl glycidyl ether at a rate of 1-3 ml / min, wherein the catalyst is an isopropanol solution of chloroplatinic acid with a mass fraction of 25%, and then dropping 3,3-tetramethyldisiloxane of 0.6 times the mass of allyl glycidyl ether at a rate of 3 ml / min, reacting for 4 hours, cooling to room temperature, and then dropping diethylenetriamine of 2 times the mass of allyl glycidyl ether at a rate of 2-4 ml / min, heating to 80°C, reacting for 3 hours, heating to 225°C, reacting for 40 minutes, and obtaining amino-terminated hyperbranched siloxane; mixing amino-terminated hyperbranched siloxane, maleic anhydride, and isopropanol in a mass ratio of 60:15:3, heating to 74°C, reacting for 3.5 hours, and distilling under reduced pressure to obtain carboxyl-terminated hyperbranched siloxane;

[0034] S2. Butyl acrylate, methyl methacrylate, hydroxyethyl acrylate and glycidyl methacrylate were mixed in a mass ratio of 10:10:1.2:0.45, and 0.75 times the mass of butyl acrylate was added. The end carboxyl hyperbranched siloxane and 0.15 times the mass of butyl acrylate were added. The composite emulsifier was prepared by mixing alkylphenol polyoxyethylene ether, sodium lauryl sulfate and deionized water in a mass ratio of 1:1:25, emulsified at 700rpm for 30min, heated to 71°C, 0.25 times the mass of butyl acrylate was added as an initiator, heated to 81°C, 0.25 times the mass of butyl acrylate was added as an initiator every 30min, the initiator was a 2.5% ammonium persulfate solution by mass fraction, reacted for 5h, kept warm for 1.5h, cooled to 40°C, and the modified polyacrylate was obtained by discharging, i.e., a tackifier;

[0035] S3. Toluene, KH-560 and platinum catalyst were mixed in a mass ratio of 8:40:0.45, heated to 100°C for reaction for 3.5h, then heated to 150°C for reaction for 5.5h, cooled to 80°C, and distilled under reduced pressure, and then 1.15 times the mass of toluene hydrogen-containing silicone oil was added, and then 0.02 times the mass of toluene platinum catalyst was added, heated to 100°C for reaction for 3.5h, cooled to 80°C, and distilled under reduced pressure to obtain epoxy hydrogen-containing silicone oil; Methyldisiloxane, ethyl orthosilicate, ethanol, 2 mol / L hydrochloric acid and deionized water were mixed in a mass ratio of 1:0.9:10:4:20, heated to 85°C, reacted for 3 hours, added with epoxy hydrogen silicone oil of the same mass as tetramethyldisiloxane and phenyl molybdate of 1.7 times the mass of tetramethyldisiloxane, cooled to 70°C, added with sodium hydroxide of 0.04 times the mass of tetramethyldisiloxane, continued to react for 5 hours, and evaporated under reduced pressure to obtain epoxy phenolic resin;

[0036] S4. The glass fiber is heated to 425°C, kept warm for 1.5 hours, cooled to room temperature, immersed in 4 mol / L hydrochloric acid at 90°C, taken out after 9 hours, washed 9 times with deionized water, and dried to obtain hydroxyl glass fiber, i.e., reinforcing fiber; gypsum and reinforcing fiber are mixed, ultrasonically dispersed at 65kHz for 25 minutes, and then a water reducer, sodium hexametaphosphate, a foaming agent, sodium dodecyl sulfate and a viscosity enhancer are added, and stirred evenly to obtain a board core; boron trifluoride monoethylamine and ethylene glycol are mixed at a mass ratio of 1:5.5, stirred evenly, and then epoxy phenolic resin with a mass of 14 times that of boron trifluoride monoethylamine is added, stirred evenly, and kept warm at 130°C for 2 hours to obtain a protective film; the board core is poured into a flat plate forming machine, and the protective film is applied to the surface of the board core, the thickness of the protective film is 9μm, and cured for 7 hours to obtain a fireproof gypsum board.

[0037] Example 3

[0038] The preparation method of the fireproof gypsum board in this embodiment is:

[0039] S1. The allyl glycidyl ether was heated to 80°C, and a catalyst of 0.04 times the mass of the allyl glycidyl ether was added dropwise at a rate of 3 ml / min, wherein the catalyst was a 30% mass fraction of chloroplatinic acid in isopropanol solution, and then 3,3-tetramethyldisiloxane of 0.7 times the mass of the allyl glycidyl ether was added dropwise at a rate of 4 ml / min, and the reaction was continued for 5 hours. The mixture was cooled to room temperature, and then diethylenetriamine of 3 times the mass of the allyl glycidyl ether was added dropwise at a rate of 4 ml / min, and the temperature was raised to 90°C, and the reaction was continued for 4 hours. The temperature was raised to 230°C, and the reaction was continued for 50 minutes to obtain an amino-terminated hyperbranched siloxane; amino-terminated hyperbranched siloxane, maleic anhydride, and isopropanol were mixed in a mass ratio of 70:15:3, the temperature was raised to 76°C, the reaction was continued for 4 hours, and the mixture was distilled under reduced pressure to obtain a carboxyl-terminated hyperbranched siloxane;

[0040] S2. Butyl acrylate, methyl methacrylate, hydroxyethyl acrylate and glycidyl methacrylate were mixed in a mass ratio of 10:10:1.4:0.6, and a compound emulsifier of 0.9 times the mass of butyl acrylate and 0.2 times the mass of butyl acrylate was added, wherein the compound emulsifier was prepared by mixing alkylphenol polyoxyethylene ether, sodium lauryl sulfate and deionized water in a mass ratio of 1:1:30, emulsified at 800rpm for 40min, heated to 72°C, added with an initiator of 0.3 times the mass of butyl acrylate, heated to 82°C, and added with an initiator of 0.3 times the mass of butyl acrylate every 30min, wherein the initiator was a 2.5% ammonium persulfate solution by mass, reacted for 6h, kept warm for 2h, cooled to 42°C, and the modified polyacrylate was obtained by discharging the material, i.e., a tackifier;

[0041] S3. Toluene, KH-560 and platinum catalyst were mixed in a mass ratio of 8:50:0.5, heated to 105°C for reaction for 4h, then heated to 155°C for reaction for 6h, cooled to 82°C, and distilled under reduced pressure, and then 1.2 times the mass of toluene was added with hydrogen-containing silicone oil, and then 0.03 times the mass of toluene was added with platinum catalyst, heated to 105°C for reaction for 4h, cooled to 82°C, and distilled under reduced pressure to obtain epoxy hydrogen-containing silicone oil; tetramethyl disiloxane Oxyethane, tetraethyl orthosilicate, ethanol, 3 mol / L hydrochloric acid and deionized water were mixed in a mass ratio of 1:0.9:10:5:20, heated to 90°C, reacted for 4 hours, added with epoxy hydrogen silicone oil of the same mass as tetramethyldisiloxane and phenyl molybdate of 1.8 times the mass of tetramethyldisiloxane, cooled to 72°C, added with sodium hydroxide of 0.05 times the mass of tetramethyldisiloxane, continued to react for 6 hours, and evaporated under reduced pressure to obtain epoxy phenolic resin;

[0042] S4. The glass fiber is heated to 450°C, kept warm for 2 hours, cooled to room temperature, immersed in 5 mol / L hydrochloric acid at 100°C, taken out after 10 hours, washed 10 times with deionized water, and dried to obtain hydroxyl glass fiber, i.e., reinforcing fiber; gypsum and reinforcing fiber are mixed, ultrasonically dispersed at 85kHz for 30 minutes, and then a water reducer, sodium hexametaphosphate, a foaming agent, sodium dodecyl sulfate and a viscosity enhancer are added, and stirred evenly to obtain a board core; boron trifluoride monoethylamine and ethylene glycol are mixed in a mass ratio of 1:6, stirred evenly, and then an epoxy phenolic resin with a mass of 18 times that of boron trifluoride monoethylamine is added, stirred evenly, and kept warm at 135°C for 2.5 hours to obtain a protective film; the board core is poured into a flat plate forming machine, and a protective film is applied to the surface of the board core, the thickness of the protective film is 10μm, and cured for 8 hours to obtain a fireproof gypsum board.

[0043] Comparative Example 1

[0044] The preparation method of comparative example 1 is the same as that of example 2. The fireproof gypsum board is different from example 2 in that the board core only includes gypsum, reinforcing fiber, water reducing agent and foaming agent.

[0045] Comparative Example 2

[0046] The preparation method of Comparative Example 2 is the same as that of Example 2. The difference between the fireproof gypsum board and Example 2 is that the tackifier is polyacrylate.

[0047] Comparative Example 3

[0048] The preparation method of Comparative Example 3 is the same as that of Example 2. The difference between the fireproof gypsum board and Example 2 is that the epoxy phenolic resin is prepared by reacting epoxy hydrogenated silicone oil, phenol and phenyl molybdate.

[0049] Comparative Example 4

[0050] The preparation method of Comparative Example 4 is the same as that of Example 2. The fireproof gypsum board is different from Example 2 in that the fireproof gypsum board only includes a board core.

[0051] Effect example

[0052] Table 1 below shows the performance analysis results of the fireproof gypsum boards prepared using Examples 1 to 3 of the present invention and Comparative Examples 1 to 4:

[0053] Table 1

[0054]

[0055] By comparing the experimental data of the embodiments and the comparative examples in Table 1, it can be clearly found that the fireproof gypsum boards prepared using embodiments 1, 2 and 3 have excellent strength and fire stability.

[0056] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 1, Comparative Example 2, it can be found that after the amino-terminated hyperbranched siloxane reacts with maleic anhydride through a ring-opening reaction, the modified polyacrylate is reacted with butyl acrylate, methyl methacrylate, hydroxyethyl acrylate and glycidyl methacrylate to form a hyperbranched siloxane with a terminal carboxyl structure, which is introduced into the polyacrylate together with glycidyl methacrylate to form a polyacrylate with a long carbon chain structure containing epoxy groups and polycarboxyl groups, which can induce polymer cross-linking in the board core, not only has excellent viscosity, but also can react with the hydroxyl groups on the surface of the reinforcing fibers to uniformly disperse the reinforcing fibers in the board core, thereby enhancing the strength and fire stability of the fireproof gypsum board.

[0057] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 3, Comparative Example 4, it can be found that the epoxy phenolic resin prepared by the reaction of epoxy hydrogen silicone oil, tetramethyldisiloxane, tetraethyl orthosilicate and phenyl molybdate, after hydrolysis of tetramethyldisiloxane and tetraethyl orthosilicate, can be condensed with phenyl molybdate to form a phenolic resin, silicon and molybdenum are bonded to the main chain of the phenolic resin molecule with high bond energy chemical bonds, and epoxy hydrogen silicone oil is introduced during the reaction process to form an epoxy phenolic resin with an epoxy cross-linked structure, thereby enhancing heat resistance; the epoxy phenolic resin is coated on the surface of the board core and cured, hydrogen bonds are formed between the epoxy phenolic resin and the board core, and the epoxy phenolic resin adheres to the surface of the board core, thereby enhancing the strength and fire stability of the gypsum board.

[0058] Obviously, the above embodiments are merely examples for clearly illustrating the embodiments of the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. However, these obvious changes or modifications derived from the spirit of the present invention are still within the scope of protection of the present invention.

Claims

1. A fireproof gypsum board, characterized in that: It includes a board core and a protective film; the board core includes gypsum, reinforcing fiber, water reducing agent, foaming agent and tackifier; the protective film is epoxy phenolic resin solidified on the surface of the board core; the tackifier is modified polyacrylate; The tackifier is prepared by mixing amino-terminated hyperbranched siloxane, maleic anhydride and isopropanol in a mass ratio of 50-70:15:3, heating to 72-76°C, reacting for 3-4 hours, and performing reduced pressure distillation to obtain carboxyl-terminated hyperbranched siloxane; mixing butyl acrylate, methyl methacrylate, hydroxyethyl acrylate and glycidyl methacrylate in a mass ratio of 10:10:1-1.4:0.3-0.6, adding carboxyl-terminated hyperbranched siloxane and propylene glycol in an amount of 0.6-0.9 times the mass of butyl acrylate; The compound emulsifier with the mass of 0.1~0.2 times of butyl acrylate is emulsified at 600~800rpm for 20~40min, the temperature is raised to 70~72℃, the initiator with the mass of 0.2~0.3 times of butyl acrylate is added, the temperature is raised to 80~82℃, the initiator with the mass of 0.2~0.3 times of butyl acrylate is added every 30min, the initiator is 2.5% ammonium persulfate solution, the reaction is continued for 4~6h, the reaction is kept warm for 1~2h, the temperature is lowered to 38~42℃, and the material is obtained; The epoxy phenolic resin is prepared by mixing tetramethyldisiloxane, ethyl orthosilicate, ethanol, 1-3 mol / L hydrochloric acid and deionized water in a mass ratio of 1:0.9:10:3-5:20, heating to 80-90° C., reacting for 2-4 hours, adding epoxy hydrogen silicone oil of the same mass as tetramethyldisiloxane and phenyl molybdate of 1.6-1.8 times the mass of tetramethyldisiloxane, cooling to 68-72° C., adding sodium hydroxide of 0.03-0.05 times the mass of tetramethyldisiloxane, continuing the reaction for 4-6 hours, and performing vacuum rotary evaporation to obtain the epoxy phenolic resin; The reinforcing fiber is hydroxy glass fiber; the foaming agent is sodium lauryl sulfate; and the water reducing agent is sodium hexametaphosphate.

2. A method for preparing a fireproof gypsum board according to claim 1, characterized in that: The specific steps include: S1. The amino-terminated hyperbranched siloxane, maleic anhydride and isopropanol were mixed in a mass ratio of 50-70:15:3, heated to 72-76°C, reacted for 3-4h, and distilled under reduced pressure to obtain a carboxyl-terminated hyperbranched siloxane; S2. Butyl acrylate, methyl methacrylate, hydroxyethyl acrylate and glycidyl methacrylate are mixed in a mass ratio of 10:10:1~1.4:0.3~0.6, and 0.6~0.9 times the mass of butyl acrylate carboxyl-terminated hyperbranched siloxane and 0.1~0.2 times the mass of butyl acrylate are added. The compound emulsifier is emulsified at 600~800rpm for 20~40min, the temperature is raised to 70~72°C, and an initiator is added in an amount of 0.2~0.3 times the mass of butyl acrylate. The temperature is raised to 80~82°C, and 0.2~0.3 times the mass of butyl acrylate is added every 30min. The initiator is a 2.5% ammonium persulfate solution by mass. After reacting for 4~6h, the reaction is kept warm for 1~2h, and the temperature is lowered to 38~42°C. The modified polyacrylate is obtained by discharging the material, which is a tackifier; S3. Tetramethyldisiloxane, ethyl orthosilicate, ethanol, 1-3 mol / L hydrochloric acid and deionized water were mixed in a mass ratio of 1:0.9:10:3-5:20, heated to 80-90°C, reacted for 2-4 hours, added with an epoxy hydrogen silicone oil of the same mass as tetramethyldisiloxane and phenyl molybdate of 1.6-1.8 times the mass of tetramethyldisiloxane, cooled to 68-72°C, added with 0.03-0.05 times the mass of tetramethyldisiloxane sodium hydroxide, continued to react for 4-6 hours, and vacuum evaporated to obtain epoxy phenolic resin; S4. Mix gypsum and reinforcing fiber, disperse them ultrasonically at 40-85kHz for 20-30min, add water reducing agent sodium hexametaphosphate, foaming agent sodium dodecyl sulfate and viscosity enhancer, stir evenly to obtain a board core; mix boron trifluoride monoethylamine and ethylene glycol at a mass ratio of 1:5-6, stir evenly, add epoxy phenolic resin with a mass of 10-18 times that of boron trifluoride monoethylamine, stir evenly, and keep warm at 125-135℃ for 1.5-2.5h to obtain a protective film; pour the board core into a flat plate forming machine, apply the protective film on the surface of the board core, and cure for 6-8h to obtain a fireproof gypsum board.

3. The method for preparing a fireproof gypsum board according to claim 2, characterized in that: In the above step S1, the preparation method of the amino-terminated hyperbranched siloxane is as follows: heating allyl glycidyl ether to 60-80° C., adding a catalyst in an amount of 0.02-0.04 times the mass of allyl glycidyl ether at a rate of 1-3 ml / min, wherein the catalyst is an isopropanol solution of chloroplatinic acid with a mass fraction of 20-30%, and then adding 3,3-tetramethyldisiloxane in an amount of 0.5-0.7 times the mass of allyl glycidyl ether at a rate of 2-4 ml / min, reacting for 3-5 hours, cooling to room temperature, and then adding diethylenetriamine in an amount of 1-3 times the mass of allyl glycidyl ether at a rate of 2-4 ml / min, heating to 70-90° C., reacting for 2-4 hours, heating to 220-230° C., and reacting for 30-50 minutes to obtain the amino-terminated hyperbranched siloxane.

4. The method for preparing a fireproof gypsum board according to claim 2, characterized in that: In the above step S2, the compound emulsifier is prepared by mixing alkylphenol polyoxyethylene ether, sodium lauryl sulfate and deionized water in a mass ratio of 1:1:20-30.

5. The method for preparing a fireproof gypsum board according to claim 2, characterized in that: In the above step S3, the preparation method of epoxy hydrogenated silicone oil is as follows: toluene, KH-560 and platinum catalyst are mixed in a mass ratio of 8:30~50:0.4~0.5, heated to 95~105°C for reaction for 3~4h, then heated to 145~155°C for reaction for 5~6h, cooled to 78~82°C, distilled under reduced pressure, and then 1.1~1.2 times the mass of toluene of hydrogenated silicone oil is added, and then 0.01~0.03 times the mass of toluene of platinum catalyst is added, heated to 95~105°C for reaction for 3~4h, cooled to 78~82°C, and distilled under reduced pressure to obtain epoxy hydrogenated silicone oil.

6. The method for preparing a fireproof gypsum board according to claim 2, characterized in that: In the above step S4, the preparation method of the reinforcing fiber is: heating the glass fiber to 400~450℃, keeping it warm for 1~2h, cooling it to room temperature, immersing it in 3~5mol / L hydrochloric acid at 80~100℃, taking it out after 8~10h and washing it with deionized water for 8~10 times, and drying it to obtain hydroxyl glass fiber, which is the reinforcing fiber.

7. The method for preparing a fireproof gypsum board according to claim 2, characterized in that: In the above step S4, the thickness of the protective film is 8-10 μm.