A circularly polarized fluorescent film and its preparation method and application
By hydrolyzing cellulose powder with sulfuric acid and reacting with L-lysine, formaldehyde and fluorescent substances, an efficient and environmentally friendly circular polarization fluorescent film was prepared, which solved the problems of high cost and optical characteristics of existing anti-counterfeiting materials, and achieved high fluorescence intensity and The effect of the large asymmetry factor.
Patent Information
- Application Number
- CN202410581735.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-11
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-05-11
AI Technical Summary
The existing anti-counterfeiting materials are expensive and complex in synthesis, so they cannot effectively impart fluorescence performance to cellulose nanocrystals (CNCs). At the same time, they cannot clearly solve the modified optical characteristics problems, and lack an efficient, simple and environmentally friendly method.
By hydrolyzing cellulose powder with an average particle size of 10-100μm, a cellulose nanocrystal suspension was formed, and reacted with L-lysine, formaldehyde and specific types of fluorescent substances in ethanol, Mannich reaction was used. Chemical modification was performed to prepare a circularly polarized fluorescent film with good optical characteristics and high fluorescence intensity.
The chemical modification of environmentally friendly and pollution-free cellulose nanocrystals was achieved, and a circularly polarized fluorescent film with high fluorescence intensity and large asymmetry factor was prepared. It is suitable for the preparation of anti-counterfeiting labels, with simple operation and easy access to raw materials.
Smart Images

Figure BDA0004834235230000091 
Figure BDA0004834235230000101 
Figure HDA0004834235240000011
Abstract
Description
Technical Field
[0001] The invention belongs to the field of material technology, and in particular relates to a circularly polarized fluorescent film and a preparation method and application thereof. Background Art
[0002] Counterfeit and substandard products pose a serious challenge to the sustainable development of the market, medical health and society. In order to meet these challenges, people continue to explore and develop various anti-counterfeiting technologies. One of the methods is to integrate multiple anti-counterfeiting elements into one system and use technologies such as structural color, phosphorescence and near-infrared irradiation to improve the anti-counterfeiting effect. However, existing anti-counterfeiting materials have the disadvantages of high synthesis cost and labor-intensive synthesis process, which makes it particularly important to develop an ideal anti-counterfeiting technology that is cost-effective, environmentally friendly and user-friendly.
[0003] Cellulose nanocrystals (CNC) are a sustainable material with unique optical properties obtained by hydrolyzing natural cellulose with sulfuric acid. The negatively charged sulfate groups on their surface provide colloidal stability, allowing CNC to self-assemble into a chiral nematic liquid crystal (LLC) phase at a certain concentration. This phase transition can lead to the appearance of iridescence and circular polarization of CNC films, providing new possibilities for the application of CNC in the field of anti-counterfeiting.
[0004] Although there have been some studies attempting to modify nanocellulose to impart new chemical properties, these methods generally involve complex steps, toxic reagents, and the use of organic solvents. In addition, these methods cannot clearly address the optical properties of the modified CNCs. Therefore, developing an efficient, simple, and environmentally friendly method to impart fluorescent properties to CNCs while maintaining their optical properties has become a focus and challenge of current research. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies of the above-mentioned prior art and to provide a circularly polarized fluorescent film with stronger fluorescence and a larger asymmetry factor, and a preparation method and application thereof.
[0006] To achieve the above object, in a first aspect of the present invention, the present invention provides a method for preparing a circularly polarized fluorescent film, the preparation method comprising the following steps:
[0007] (1) hydrolyzing cellulose powder with an average particle size of 10-100 μm with sulfuric acid to obtain a cellulose nanocrystal suspension;
[0008] (2) mixing a cellulose nanocrystal suspension, L-lysine, a formaldehyde solution, a fluorescent substance and ethanol to form a mixed solution and reacting the mixture, quenching the reaction after the reaction is completed and centrifuging the mixture, then collecting the precipitate and washing and dialyzing the precipitate;
[0009] (3) After the dialysis, the suspension is ultrasonicated and placed in a culture dish to dry, thereby obtaining a circularly polarized fluorescent film;
[0010] The fluorescent substance includes curcumin and / or fluorescein diacetate;
[0011] The molar ratio of L-lysine, formaldehyde and fluorescent substance is 1:(0.8-1.2):(0.025-0.60).
[0012] In a preparation method of a circularly polarized fluorescent film provided by the present invention, cellulose powder with an average particle size within a certain range is selected for sulfuric acid hydrolysis, and the cellulose nanocrystal suspension obtained by hydrolysis is mixed with L-lysine, formaldehyde, a specific type of fluorescent substance and ethanol in a certain molar ratio range to form a mixed solution and react, and the circularly polarized fluorescent film obtained by corresponding post-treatment after the reaction has good optical properties, high fluorescence intensity and large asymmetry factor. Specifically, the preparation method provided by the present invention uses a one-pot method to regulate the interfacial properties of cellulose nanocrystals through the Mannich reaction, realizes the implementation of a chemical modification strategy in a water-based medium, and the overall preparation process is environmentally friendly and pollution-free, and the raw materials used in the preparation method of the present invention are widely available, and the preparation process is simple to operate.
[0013] As a preferred embodiment of the preparation method of the present invention, the molar ratio of L-lysine, formaldehyde and fluorescent substance is 1:(0.9-1.1):(0.18-0.40).
[0014] The present invention has found that the molar ratio of L-lysine, formaldehyde and fluorescent substance not only affects the fluorescence intensity of the product, but also affects the polarization effect of the product. In the preparation method provided by the present invention, L-lysine is used as a linker, and curcumin and / or fluorescein diacetate can be effectively grafted onto cellulose nanocrystals under the reaction system provided by the present invention. When the molar ratio of L-lysine, formaldehyde and fluorescent substance is further selected to be within the range of 1:(0.8-1.2):(0.025-0.60) given by the present invention, especially within the range of 1:(0.9-1.1):(0.18-0.40), the comprehensive performance of the obtained product is better.
[0015] As a preferred embodiment of the preparation method of the present invention, the mass percentage of cellulose nanocrystals in the cellulose nanocrystal suspension is 2-4%.
[0016] The present invention has found that the mass percentage of cellulose nanocrystals in a cellulose nanocrystal suspension affects the subsequent grafting efficiency with fluorescent substances, thereby affecting the optical properties of the product. When the mass percentage of cellulose nanocrystals is further selected to be within the range given by the present invention, the fluorescence and polarization phenomena of the obtained product are more obvious.
[0017] As a preferred embodiment of the preparation method of the present invention, in step (2), the mass percentage of ethanol is 20-80% based on the mixed solution.
[0018] Preferably, in step (2), the mass percentage of ethanol in the mixed liquid is 40-60%.
[0019] The present invention has found that the mass percentage of ethanol in the mixed solution during the reaction process will also affect the performance of the product. When the mass percentage of ethanol is further selected to be 20-80%, especially 40-60%, the comprehensive performance of the obtained product is better.
[0020] As a preferred embodiment of the preparation method of the present invention, in step (2), the reaction temperature is 20-30°C and the reaction time is 12-24h.
[0021] The preparation method provided by the present invention is simple to operate and can react at room temperature. The present invention has found that the reaction temperature and time will affect the grafting efficiency of the reaction process to a certain extent. When the reaction temperature and reaction time are further selected within the range given by the present invention, the obtained product has stronger fluorescence and more obvious polarization phenomenon.
[0022] As a preferred embodiment of the preparation method of the present invention, the step of sulfuric acid hydrolysis is:
[0023] S1. Mix cellulose powder and sulfuric acid and heat to 40-50°C for hydrolysis for 0.5-3h. After hydrolysis, add water to terminate the reaction and let the reaction solution stand for 20-28h.
[0024] S2, remove the upper liquid after standing, then collect the precipitate by centrifugation, and place the precipitate in a dialysis bag for 7 days or more until the pH value is stable;
[0025] S3. The dialyzed solution is then centrifuged and the upper layer solution is collected to obtain a cellulose nanocrystal suspension.
[0026] The present invention has found that when the cellulose powder with an average particle size of 10-100 μm is used to carry out the sulfuric acid hydrolysis step, the obtained cellulose nanocrystal suspension is further subjected to subsequent modification and grafting, and the comprehensive effect of the obtained product is more excellent.
[0027] Preferably, in step S1, the mass ratio of cellulose powder to sulfuric acid is 1:(8-12).
[0028] Preferably, the sulfuric acid is a sulfuric acid aqueous solution with a mass concentration of 60-70%.
[0029] Preferably, water is added after the hydrolysis to terminate the reaction, and the amount of water added is 18-22 times the volume of the reaction system.
[0030] Preferably, in step S2, the molecular weight cut-off of the dialysis bag is 8000D.
[0031] Preferably, in step S2, the pH value being stable means that the pH value changes by less than 0.1 for 1 hour. As a preferred embodiment of the preparation method of the present invention, in step (2), at least one of the following is satisfied:
[0032] a. Calculated on the basis of formaldehyde solution, the mass percentage of formaldehyde is 35-40%;
[0033] b. Quench the reaction using anhydrous ethanol 1-2 times the volume of the reaction solution;
[0034] c. The centrifugal speed is 7000-9000rpm and the centrifugal time is 8-12min;
[0035] d. Washing is done by using anhydrous ethanol;
[0036] e. The molecular cutoff of the dialysis bag used for dialysis is 8000D;
[0037] f. Dialysis duration ≥ 7 days.
[0038] The present invention has found that when the parameters in step (2) are selected in the above-mentioned types or ranges, it can help achieve a product with better overall effect.
[0039] As a preferred embodiment of the preparation method of the present invention, in step (3), the ultrasonic time is 8-12 minutes;
[0040] And / or, the drying temperature is 40-50° C., and the drying time is 24-48 hours.
[0041] The present invention has found that the ultrasound in step (3) can disperse the modified cellulose nanocrystals uniformly, thereby achieving a good drying effect and obtaining a circularly polarized fluorescent film with excellent comprehensive performance.
[0042] In a second aspect of the present invention, the present invention provides a circularly polarized fluorescent film, and the circularly polarized fluorescent film is prepared by the preparation method of the present invention.
[0043] The circularly polarized fluorescent film provided by the invention has good optical properties, high fluorescence intensity and large asymmetry factor.
[0044] In the third aspect of the present invention, the present invention provides the use of the circularly polarized fluorescent film in the preparation of anti-counterfeiting labels.
[0045] Compared with the prior art, the present invention has the following beneficial effects:
[0046] In a preparation method of a circularly polarized fluorescent film provided by the present invention, cellulose powder with an average particle size within a certain range is selected for sulfuric acid hydrolysis, and the cellulose nanocrystal suspension obtained by hydrolysis is mixed with L-lysine, formaldehyde and a specific type of fluorescent substance in a certain molar ratio range in ethanol for reaction, and L-lysine is used as a linker. After the reaction, modified cellulose nanocrystals are obtained, which are further prepared into a film. The obtained product has good optical properties, high fluorescence intensity and large asymmetry factor, and can therefore be widely used in the preparation of anti-counterfeiting labels. At the same time, the preparation method of the circularly polarized fluorescent film provided by the present invention is simple to operate, environmentally friendly and green, and the raw material source is convenient, which is conducive to actual production. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 This is an optical test image of the product prepared in Example 1:
[0048] a is the fluorescence spectrum, b is the circular polarization fluorescence asymmetry factor diagram;
[0049] Figure 2 This is an optical test image of the product prepared in Example 2-3:
[0050] a is the fluorescence spectrum, b is the circular polarization fluorescence asymmetry factor diagram;
[0051] Figure 3 Optical test images of the products prepared in Examples 1, 4 and 5:
[0052] a is the fluorescence spectrum, b is the circular polarization fluorescence asymmetry factor diagram;
[0053] Figure 4 Optical test images of the products prepared in Examples 1, 6, 7 and 8:
[0054] a is the fluorescence spectrum, b is the circular polarization fluorescence asymmetry factor diagram;
[0055] Figure 5 Optical test images of the products prepared in Examples 1, 9, 10, 11 and 12:
[0056] a is the fluorescence spectrum, b is the circular polarization fluorescence asymmetry factor diagram;
[0057] Figure 6 Optical test images of the products prepared in Example 1 and Comparative Examples 1 and 2:
[0058] a is the fluorescence spectrum, b is the circular polarization fluorescence asymmetry factor diagram;
[0059] Figure 7 This is a comparison chart of the fluorescence intensities of the products prepared in Example 1, Comparative Examples 3-4, and Comparative Examples 6-7. DETAILED DESCRIPTION
[0060] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0061] Unless otherwise specified, the raw materials or equipment used in the present invention can be conventionally purchased equipment.
[0062] Example 1
[0063] An embodiment of the present invention provides a circularly polarized fluorescent film, and a method for preparing the circularly polarized fluorescent film comprises the following steps:
[0064] (1) 10 g of cellulose powder (average particle size of 90 μm) was mixed with 100 g of 64% sulfuric acid aqueous solution and hydrolyzed at 45° C. for 2.5 hours; after the hydrolysis was completed, the suspension was diluted 20 times with water to terminate the reaction; the suspension was then allowed to stand for 12 hours, and then the solution after removing the transparent top solution was centrifuged at 8000 rpm to collect the precipitate; the resulting precipitate was placed in a dialysis bag (8000D) and dialyzed against water for at least 7 days until the pH value remained stable (the change was less than 0.1 for 1 hour); the solution after the dialysis was centrifuged again at 8000 rpm for 10 minutes, and the upper solution was collected to obtain a cellulose nanocrystal suspension;
[0065] (2) Add 50 g of anhydrous ethanol to 50 g of the cellulose nanocrystal suspension prepared in step (1) (the mass percentage of the cellulose nanocrystals is 2% based on the cellulose nanocrystal suspension), and then add 0.18 g of L-lysine (1.23 mmol), 100 μL of 37% formaldehyde solution (the molar ratio of formaldehyde is 1.34 mmol) and 0.2 g of diacetate fluorescein (0.48 mmol) for reaction (the molar ratio of L-lysine, formaldehyde and diacetate fluorescein is 1:1.089:0.39); after reacting at room temperature (25° C.) for 12 hours, add 1 volume of anhydrous ethanol to quench the reaction; then centrifuge the reaction mixture at 8000 rpm for 10 minutes, collect the precipitate and wash it with anhydrous ethanol and centrifuge it twice; put the resulting precipitate into a dialysis bag (8000D) and dialyze it in water for at least 7 days;
[0066] (3) The suspension after dialysis in step (2) was sonicated for 10 minutes, then transferred to a culture dish, and dried at 45° C. for 24 hours to obtain a circularly polarized fluorescent film.
[0067] Example 2
[0068] An embodiment of the present invention provides a circularly polarized fluorescent film, and a method for preparing the circularly polarized fluorescent film comprises the following steps:
[0069] (1) 10 g of cellulose powder (average particle size of 25 μm) was mixed with 100 g of 64% sulfuric acid aqueous solution and hydrolyzed at 45° C. for 2 hours; after the hydrolysis was completed, the suspension was diluted 20 times with water to terminate the reaction; the suspension was then allowed to stand for 12 hours, and then the solution after removing the transparent top solution was centrifuged at 8000 rpm to collect the precipitate; the resulting precipitate was placed in a dialysis bag (8000D) and dialyzed against water for at least 7 days until the pH value remained stable (the change was less than 0.1 for 1 hour); the solution after the dialysis was centrifuged again at 8000 rpm for 10 minutes, and the upper solution was collected to obtain a cellulose nanocrystal suspension;
[0070] (2) adding 50 g of anhydrous ethanol to 50 g of the cellulose nanocrystal suspension prepared in step (1) (the mass percentage of the cellulose nanocrystals is 2% based on the cellulose nanocrystal suspension), and then adding 0.18 g of L-lysine (1.23 mmol), 100 μL of 37% formaldehyde solution (the molar ratio of formaldehyde is 1.34 mmol) and 0.18 g of curcumin (0.49 mmol) for reaction (the molar ratio of L-lysine, formaldehyde and curcumin is 1:1.089:0.39); reacting at room temperature (25° C.) for 12 hours, adding 1 volume of anhydrous ethanol to quench the reaction; then centrifuging the reaction mixture at 8000 rpm for 10 minutes, collecting the precipitate and washing it with anhydrous ethanol and centrifuging it twice; placing the resulting precipitate in a dialysis bag (8000D) and dialyzing it in water for at least 7 days;
[0071] (3) The suspension after dialysis in step (2) was sonicated for 10 minutes, then transferred to a culture dish, and dried at 45° C. for 24 hours to obtain a circularly polarized fluorescent film.
[0072] Example 3
[0073] An embodiment of the present invention provides a circularly polarized fluorescent film, and a method for preparing the circularly polarized fluorescent film comprises the following steps:
[0074] (1) 10 g of cellulose powder (average particle size of 10 μm) was mixed with 100 g of 64% sulfuric acid aqueous solution and hydrolyzed at 45° C. for 0.5 h; after the hydrolysis was completed, the suspension was diluted 20 times with water to terminate the reaction; the suspension was then allowed to stand for 12 h, and then the solution after removing the transparent top solution was centrifuged at 8000 rpm to collect the precipitate; the resulting precipitate was placed in a dialysis bag (8000D) and dialyzed against water for at least 7 days until the pH value remained stable (the change was less than 0.1 for 1 h); the solution after the dialysis was centrifuged again at 8000 rpm for 10 minutes, and the upper solution was collected to obtain a cellulose nanocrystal suspension;
[0075] (2) Add 50 g of anhydrous ethanol to 50 g of the cellulose nanocrystal suspension prepared in step (1) (the mass percentage of the cellulose nanocrystals is 2% based on the cellulose nanocrystal suspension), and then add 0.18 g of L-lysine (1.23 mmol), 100 μL of 37% formaldehyde solution (the molar ratio of formaldehyde is 1.34 mmol) and 0.09 g of curcumin (0.49 mmol) for reaction (the molar ratio of L-lysine, formaldehyde and fluorescein diacetate is 1:1.089:0.19); after reacting for 12 hours at room temperature (25° C.), add 1 volume of anhydrous ethanol to quench the reaction; then centrifuge the reaction mixture at 8000 rpm for 10 minutes, collect the precipitate and wash it with anhydrous ethanol and centrifuge it twice; put the resulting precipitate into a dialysis bag (8000D) and dialyze it in water for at least 7 days;
[0076] (3) The suspension after dialysis in step (2) was sonicated for 10 minutes, then transferred to a culture dish, and dried at 45° C. for 24 hours to obtain a circularly polarized fluorescent film.
[0077] Example 4
[0078] An embodiment of the present invention provides a circularly polarized fluorescent film. The only difference between the preparation method of the circularly polarized fluorescent film and that of Example 1 is that in step (2), the mass of fluorescein diacetate and the volume of the formaldehyde aqueous solution are changed so that the molar ratio of L-lysine, formaldehyde and fluorescein diacetate is 1:1.2:0.60.
[0079] Example 5
[0080] The embodiment of the present invention provides a circularly polarized fluorescent film. The only difference between the preparation method of the circularly polarized fluorescent film and that of Example 1 is that in step (2), the mass of fluorescein diacetate and the volume of the formaldehyde aqueous solution are changed so that the molar ratio of L-lysine, formaldehyde and fluorescein diacetate is 1:0.8:0.025.
[0081] Example 6
[0082] The embodiment of the present invention provides a circularly polarized fluorescent film. The only difference between the preparation method of the circularly polarized fluorescent film and that of embodiment 1 is that the mass percentage of cellulose nanocrystals in the cellulose nanocrystal suspension in step (2) is 4%.
[0083] Example 7
[0084] The embodiment of the present invention provides a circularly polarized fluorescent film. The only difference between the preparation method of the circularly polarized fluorescent film and that of embodiment 1 is that in step (2), the mass percentage of cellulose nanocrystals in the cellulose nanocrystal suspension is 1%.
[0085] Example 8
[0086] The embodiment of the present invention provides a circularly polarized fluorescent film. The only difference between the preparation method of the circularly polarized fluorescent film and that of embodiment 1 is that in step (2), the mass percentage of cellulose nanocrystals in the cellulose nanocrystal suspension is 6%.
[0087] Example 9
[0088] The embodiment of the present invention provides a circularly polarized fluorescent film. The only difference between the preparation method of the circularly polarized fluorescent film and that of embodiment 1 is that the amount of anhydrous ethanol added in step (2) is changed so that the mass percentage of anhydrous ethanol in the mixed solution is 20%.
[0089] Example 10
[0090] The embodiment of the present invention provides a circularly polarized fluorescent film. The only difference between the preparation method of the circularly polarized fluorescent film and that of embodiment 1 is that the amount of anhydrous ethanol added in step (2) is changed so that the mass percentage of anhydrous ethanol in the mixed solution is 80%.
[0091] Embodiment 11
[0092] The embodiment of the present invention provides a circularly polarized fluorescent film. The only difference between the preparation method of the circularly polarized fluorescent film and that of embodiment 1 is that the amount of anhydrous ethanol added in step (2) is changed so that the mass percentage of anhydrous ethanol in the mixed solution is 10%.
[0093] Example 12
[0094] The embodiment of the present invention provides a circularly polarized fluorescent film. The only difference between the preparation method of the circularly polarized fluorescent film and that of embodiment 1 is that the amount of anhydrous ethanol added in step (2) is changed so that the mass percentage of anhydrous ethanol in the mixed solution is 90%.
[0095] Comparative Example 1
[0096] The comparative example of the present invention provides a circularly polarized fluorescent film. The only difference between the preparation method of the circularly polarized fluorescent film and that of Example 1 is that in step (1), the average particle size of the cellulose powder is 250 μm.
[0097] Comparative Example 2
[0098] The comparative example of the present invention provides a circularly polarized fluorescent film. The only difference between the preparation method of the circularly polarized fluorescent film and that of Example 1 is that the mass of fluorescein diacetate is changed in step (2) so that the molar ratio of L-lysine, formaldehyde and fluorescein diacetate is 1:0.6:1.10.
[0099] Comparative Example 3
[0100] The comparative example of the present invention provides a circularly polarized fluorescent film. The only difference between the preparation method of the circularly polarized fluorescent film and that of Example 1 is that the mass of fluorescein diacetate is changed in step (2) so that the molar ratio of L-lysine, formaldehyde and fluorescein diacetate is 1:1.4:0.01.
[0101] Comparative Example 4
[0102] The comparative example of the present invention provides a circularly polarized fluorescent film. The only difference between the preparation method of the circularly polarized fluorescent film and that of Example 1 is that fluorescein is used instead of fluorescein diacetate in step (2).
[0103] Comparative Example 5
[0104] The comparative example of the present invention provides a circularly polarized fluorescent film. The only difference between the preparation method of the circularly polarized fluorescent film and that of Example 1 is that no formaldehyde solution is added in step (2).
[0105] Comparative Example 6
[0106] The comparative example of the present invention provides a circularly polarized fluorescent film. The only difference between the preparation method of the circularly polarized fluorescent film and that of Example 1 is that L-lysine is not added in step (2).
[0107] Effect example
[0108] The effect examples of the present invention verify the optical properties of the circularly polarized fluorescent films prepared in Examples 1-12 and Comparative Examples 1-6. The fluorescence performance of the products is tested by a fluorescence spectrometer (Fluorolog-4), and the polarization of the products is tested by a circularly polarized fluorescence spectrometer (CPL-200). The results are shown in Table 1.
[0109] Table 1
[0110]
[0111]
[0112] As can be seen from Table 1, when the technical solution of the present invention is adopted, the optical properties of the obtained product are excellent, wherein the fluorescence intensity is above 1249 and the asymmetry factor is above 0.12;
[0113] It can be seen from Example 1 and Comparative Example 1 that the average particle size of cellulose powder will also affect the performance of the product. When the average particle size of cellulose powder in Comparative Example 1 is too large, the polarization ability of the obtained product is weakened and the asymmetry factor is significantly reduced; it can be seen from Example 1, Examples 4-5 and Comparative Examples 2-3 that the molar ratio of L-lysine, formaldehyde and fluorescent substance in the reaction process will significantly affect the performance of the product. When the molar ratio of the three is not within the range given by the present invention, specifically, when there is too much fluorescent substance in Comparative Example 2, the polarization ability of the obtained product is weakened and the asymmetry factor is significantly reduced; when there is too little fluorescent substance in Comparative Example 3, the obtained product has no fluorescent performance. It can be seen from Example 1 and Comparative Example 4 that when other fluorescent substances are used, the obtained product has no obvious fluorescence; it can be seen from Example 1 and Examples 9-12 that the mass percentage of ethanol in the mixed solution will also affect the comprehensive performance of the product. When the mass percentage of ethanol is not within the preferred range given by the present invention, the polarization ability of the obtained product is weakened and the asymmetry factor is significantly reduced; it can be seen from Example 1 and Comparative Examples 5-6 that when any one of the raw materials is missing, the product has no fluorescent performance and the product of the present invention cannot be prepared.
[0114] In addition, the optical spectrum obtained during the test is shown in the attached figure, from which it can be clearly seen that the optical properties of the product obtained by adopting the technical solution of the present invention are excellent.
[0115] Finally, it should be noted that the above embodiments are intended to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a circularly polarized fluorescent film, characterized in that: The preparation method comprises the following steps: (1) hydrolyzing cellulose powder with an average particle size of 10-100 μm with sulfuric acid to obtain a cellulose nanocrystal suspension; (2) mixing a cellulose nanocrystal suspension, L-lysine, a formaldehyde solution, a fluorescent substance and ethanol to form a mixed solution and reacting the mixture, quenching the reaction after the reaction is completed and centrifuging the mixture, then collecting the precipitate and washing and dialyzing the precipitate; (3) After the dialysis, the suspension is ultrasonicated and placed in a culture dish to dry, thereby obtaining a circularly polarized fluorescent film; The fluorescent substance includes curcumin and / or fluorescein diacetate; The molar ratio of L-lysine, formaldehyde and fluorescent substance is 1:(0.8-1.2):(0.025-0.60).
2. The preparation method according to claim 1, characterized in that: The molar ratio of L-lysine, formaldehyde and fluorescent substance is 1:(0.9-1.1):(0.18-0.40).
3. The preparation method according to claim 1, characterized in that: In the cellulose nanocrystal suspension, the mass percentage of cellulose nanocrystals is 2-4%.
4. The preparation method according to claim 1, characterized in that: In step (2), the mass percentage of ethanol is 20-80% based on the mixed solution.
5. The preparation method according to claim 1, characterized in that: In step (2), the reaction temperature is 20-30°C and the reaction time is 12-24h.
6. The preparation method according to claim 1, characterized in that: The steps of the sulfuric acid hydrolysis are: S1. Mix cellulose powder and sulfuric acid and heat to 40-50°C for hydrolysis for 0.5-3h. After hydrolysis, add water to terminate the reaction and let the reaction solution stand for 20-28h. S2, remove the upper liquid after standing, then collect the precipitate by centrifugation, and place the precipitate in a dialysis bag for 7 days or more until the pH value is stable; S3. The dialyzed solution is then centrifuged and the upper layer solution is collected to obtain a cellulose nanocrystal suspension.
7. The preparation method according to claim 1, characterized in that: In step (2), at least one of the following conditions is met: a. In the formaldehyde solution, the mass percentage of formaldehyde is 35-40%; b. Quench the reaction using anhydrous ethanol 1-2 times the volume of the reaction solution; c. The centrifugal speed is 7000-9000rpm and the centrifugal time is 8-12min; d. Washing is done by using anhydrous ethanol; e. The molecular cutoff of the dialysis bag used for dialysis is 8000D; f. Dialysis duration ≥ 7 days.
8. The preparation method according to claim 1, characterized in that: In step (3), the ultrasonication time is 8-12 min; And / or, the drying temperature is 40-50° C., and the drying time is 24-48 hours.
9. A circularly polarized fluorescent film, characterized in that: The circularly polarized fluorescent film is prepared by the preparation method according to any one of claims 1 to 8.