A continuous gradient bicrystalline tungsten copper contact material and its preparation method

The continuous gradient bicrystalline tungsten-copper contact material prepared by spray pyrolysis and hydrogen reduction processes solves the problems of high-temperature stability and unreliable bonding at the welding surface of tungsten-copper contact materials, achieving higher resistance to arc erosion and longer service life.

CN118516581BActive Publication Date: 2026-11-10JIANGXI UNIV OF SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410720578.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2026-11-10
Estimated Expiration
2044-06-05

AI Technical Summary

Technical Problem

Existing tungsten copper contact materials lack high-temperature stability and resistance to arc erosion, and the welded surfaces are not firmly bonded, leading to thermal failure due to differences in thermal expansion coefficients.

Method used

Bicrystalline tungsten-copper composite powder was prepared by spray pyrolysis and hydrogen reduction processes. By controlling the oxidation process and pressing molding, a continuous gradient distribution of material composition and porosity was achieved. Copper was used as the pressing binder phase, and oxygen-free copper was melt-infiltrated to form a continuous gradient bicrystalline tungsten-copper contact.

Benefits of technology

It improves the arc erosion resistance of tungsten copper contact materials and the reliability of the welding surface, reduces the probability of separation failure caused by differences in thermal expansion coefficients, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118516581B_ABST
    Figure CN118516581B_ABST
Patent Text Reader

Abstract

This invention discloses a continuous gradient bicrystalline tungsten-copper contact material and its preparation method. The preparation method includes the following steps: mixing ball-milled and dispersed W powder with a copper salt solution containing oxyacid anions to obtain a mixed slurry; subjecting the mixed slurry to spray pyrolysis to obtain tungsten-copper mixed oxide powder; subjecting the tungsten-copper mixed oxide powder to hydrogen reduction to obtain a composite powder of bicrystalline tungsten and copper; pressing the composite powder into a copper-tungsten blank with a continuous gradient distribution of W content; and infiltrating the copper-tungsten blank with oxygen-free copper to obtain the continuous gradient bicrystalline tungsten-copper contact material. The continuous gradient bicrystalline tungsten-copper contact material has a tungsten content of 80–93 wt.% at one end and 50–75 wt.% at the other end. The bicrystalline tungsten-copper contact of this invention combines the good toughness and high-temperature stability of coarse tungsten grains with the excellent arc dispersion capability of fine tungsten grains; simultaneously, the continuous gradient structure effectively solves the interfacial thermal stress problem between the tungsten-copper material at the contact end and the pure copper at the conductive end of the contact product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of tungsten-copper composite materials, specifically to a continuous gradient bicrystalline tungsten-copper contact material and its preparation method. Background Technology

[0002] Tungsten-copper contact materials are widely used in high-voltage circuit breakers, electrical shielding, and other electrical contact applications. Tungsten, possessing excellent high-temperature strength and arc erosion resistance, is the main component of tungsten-copper contact materials, accounting for over 80 wt.%. However, with the rapid development of power grid transmission technology, conventional tungsten-copper contact materials have become less effective, failing to adequately combine high-temperature stability and arc erosion resistance. Furthermore, due to tungsten's poor conductivity, tungsten-copper contact materials often exhibit poor electrical conductivity and are frequently used in combination with pure copper or copper-chromium alloys in practical applications. During contact product manufacturing, the bonding of tungsten-copper with pure copper or copper-chromium alloys employs friction welding or electron beam welding processes. However, the high tungsten content in tungsten-copper contact materials results in a significant difference in thermal expansion coefficient compared to pure copper or copper-chromium alloys, leading to interfacial thermal stress and resulting in a weak bond at the weld surface. At the same time, the mismatch in the coefficients of thermal expansion between tungsten copper contact material and pure copper or copper-chromium alloy can also cause thermal failure of contact products under high-temperature service environments, resulting in the separation of tungsten copper from pure copper or copper-chromium alloy.

[0003] Functionally graded materials (FJTs) are composites of two or more materials, with their composition and structure exhibiting a continuous gradient. These materials optimize the overall performance of components to meet the requirements of repeated normal operation under extreme environments, and are commonly used in high-tech fields such as modern aerospace and nuclear industries. The emergence of this material provides a more reliable solution to the welding problem of tungsten-copper contacts. By constructing a gradient composition, the tungsten-copper contact material maintains its original composition at the electrical contact surface while reducing the tungsten content at the welding surface. This reduces the difference in thermal expansion coefficients between the tungsten-copper contact material and pure copper or copper-chromium alloys, significantly improving the reliability of the bonding surface between the tungsten-copper contact material and pure copper or copper-chromium alloys.

[0004] For example, Chinese patent document CN201910789782.4 discloses a method for preparing a W-Cu continuous gradient composite material. This method uses W powder of different particle sizes as raw materials, adds binders, dispersants, plasticizers, etc., and mixes them through ball milling to obtain a suspension slurry. The slurry is then settled and dried to obtain a green body. After debinding and sintering, a W skeleton with a continuous gradient pore size is obtained. Finally, Cu is infiltrated at a certain temperature to obtain a W-Cu continuous gradient composite material with continuously varying W and Cu compositions along the cross-section. This preparation method involves many steps and a long cycle, from suspension preparation, W particle settling, furnace debinding, skeleton sintering to final Cu infiltration. Furthermore, the W particles of different sizes are distributed along the gradient direction in the material according to particle size rather than a mixture of multiple particle sizes, which limits the effective improvement of material properties. Summary of the Invention

[0005] In view of some problems existing in the existing tungsten copper contact materials and their preparation methods, the main objective of this invention is to provide an improved continuous gradient bicrystalline tungsten copper contact material and its preparation method.

[0006] To achieve the above-mentioned main objectives, a first aspect of the present invention discloses a method for preparing a continuous gradient bicrystalline tungsten-copper contact material, comprising the following steps:

[0007] (1) Mix the ball-milled and dispersed W powder with a copper salt solution containing oxyacid anions to obtain a mixed slurry;

[0008] (2) The mixed slurry is subjected to spray pyrolysis to obtain tungsten-copper mixed oxide powder;

[0009] (3) The tungsten-copper mixed oxide powder is subjected to hydrogen reduction to obtain a composite powder of bicrystalline tungsten and copper;

[0010] (4) The composite powder is pressed into a copper-tungsten blank with a continuous gradient distribution of W content and porosity, and the copper in the composite powder is used as the pressing binder phase.

[0011] (5) Oxygen-free copper is melt-infiltrated into the copper-containing tungsten billet to obtain a continuous gradient bicrystalline tungsten-copper contact material.

[0012] In this invention, the realization of the bicrystalline tungsten structure is achieved through two stages: spray pyrolysis and hydrogen reduction. During spray pyrolysis, the oxyacid copper salt decomposes to form gaseous oxide, oxygen, and copper oxide. Most of the oxygen, in the form of gaseous oxide, is carried away by the protective atmosphere through the exhaust port. The oxygen then combines with tungsten at high temperatures to form WO2. Simultaneously, under high-temperature conditions, oxygen in the copper oxide migrates to the tungsten, and the tungsten and copper oxide undergo a redox reaction to produce pure copper and WO2. After hydrogen reduction, bicrystalline tungsten powder is obtained. The coarse and fine tungsten powders in the bicrystalline tungsten powder are uniformly mixed (the fine tungsten powder mainly adheres to the surface of the coarse tungsten powder and is uniformly mixed with it). This results in a uniformly mixed distribution of both coarse and fine tungsten grains in the final material, fully leveraging the synergistic effect and comprehensive advantages of both grains.

[0013] In this invention, oxygen from oxyacid copper salts is used as the oxygen source. After being prepared into a mixed slurry, the oxygen element is evenly distributed, resulting in a uniform oxide layer on the powder surface during oxidation, without the formation of oxide segregation. Furthermore, the copper in the oxyacid copper salts, after spray pyrolysis and hydrogen reduction, acts as the binder phase during the pressing process, eliminating the need for additional binders. This reduces the degreasing step in the production process, shortening the production time and lowering production costs. Moreover, the tungsten blanks prepared by traditional tungsten powder pressing have higher purity.

[0014] In this invention, the overall oxygen content in the mixed slurry can be quantified by adjusting the mass ratio of oxyacid copper salt to tungsten powder, thereby enabling quantitative control of the oxidation degree of tungsten particle surface and the fine tungsten powder during subsequent spray pyrolysis. Simultaneously, the formation of a coarse-fine tungsten powder by generating fine tungsten powder in situ on the surface of coarse tungsten powder facilitates the uniform distribution of both types of tungsten particles during subsequent pressing and sintering processes.

[0015] According to a specific embodiment of the present invention, in step (1), tungsten powder with a particle size of 3-8 μm is selected for ball milling for 4-6 hours, the ball-to-material ratio is 3-2:1, the ball milling medium is anhydrous ethanol, and after ball milling, vacuum drying is performed to obtain dispersed tungsten powder.

[0016] According to a specific embodiment of the present invention, the concentration of the copper salt solution in step (1) is 1-3 mol / L, the mixing ratio of tungsten powder and copper salt solution is 2-3 kg / L, and the mixture is stirred and mixed evenly to obtain a slurry.

[0017] In the above technical solution, the mixing ratio of tungsten powder and copper salt solution is reasonably controlled so that the surface of tungsten particles can be oxidized without the oxide layer peeling off, so that after subsequent hydrogen reduction, submicron-sized fine tungsten particles can better adhere to the surface of coarse tungsten particles.

[0018] According to one specific embodiment of the present invention, the oxyacid anion copper salt is one or more of copper sulfate, copper nitrate, copper oxalate, copper carbonate, and copper acetate.

[0019] According to a specific embodiment of the present invention, the feed rate of spray pyrolysis in step (2) is 50-180 ml / min, the inlet temperature is 230-260°C, the pyrolysis temperature is 550-750°C, and an inert gas is used as a protective atmosphere.

[0020] According to a specific embodiment of the present invention, the reduction temperature in step (3) is 800-950°C, the reduction time is 2-3 hours, and the thickness of the oxide powder layer is 8-12 mm.

[0021] According to a specific embodiment of the present invention, step (4) involves pressing using a die with a beveled punch, with an average pressing pressure of 2–5 MPa / cm. 2 The angle of inclination of the punch's bevel relative to the pressing and forming surface is controlled between 3° and 8°.

[0022] In the above technical solution, a die with a beveled punch (e.g., a wedge-shaped punch) is used to press and form a tungsten billet. During the pressing process, the height difference between the two ends of the pressing and forming surface of the beveled punch is used to achieve a continuous gradient change in the amount of powder compression deformation, resulting in a tungsten billet with a continuous gradient change in porosity and tungsten content with opposite trends. The overall porosity of the tungsten billet and the difference in porosity between the two ends of the tungsten billet can be controlled by adjusting the inclination angle of the beveled punch and the average compression amount during the pressing process.

[0023] According to a specific embodiment of the present invention, the melting temperature of step (5) is 1250-1400°C, and the melting atmosphere is a mixture of hydrogen and inert gas.

[0024] To achieve the aforementioned main objective, a second aspect of the present invention discloses a continuous gradient bicrystalline tungsten-copper contact material, wherein the tungsten content at one end of the continuous gradient bicrystalline tungsten-copper contact material is 80–93 wt.%, and the tungsten content at the other end is 50–75 wt.%, and the tungsten content exhibits a continuous change from one end to the other without a macroscopic interface layer; the bicrystalline tungsten in the continuous gradient bicrystalline tungsten-copper contact material comprises a mixed distribution of first tungsten grains and second tungsten grains, the first tungsten grains having a larger average size than the second tungsten grains, and the mass ratio of the first tungsten grains to the second tungsten grains being 8–5:1.

[0025] Preferably, the average sizes of the first tungsten grain and the second tungsten grain are 3-7 μm and 200-500 nm, respectively.

[0026] The continuous gradient bicrystalline tungsten-copper contact material of this invention features a mixed distribution of coarse and fine tungsten grains. The coarse tungsten grains exhibit good toughness and high-temperature stability, while the fine tungsten grains demonstrate excellent arc dispersion capability and strength. This bicrystalline tungsten-copper contact material combines both advantages, resulting in more stable contact and a longer service life compared to conventional tungsten-copper contact materials. Simultaneously, the continuous gradient composition addresses the issues of requiring higher tungsten content for superior arc erosion resistance on the contact surface and the need for the welding surface to match the coefficient of thermal expansion of copper or copper-chromium alloys.

[0027] The continuous gradient bicrystalline tungsten-copper contact material of this invention, through the design of a gradient composition structure, can further increase the tungsten content of the contact surface without considering the coefficient of thermal expansion, resulting in stronger resistance to arc erosion. Reducing the tungsten content at the welding surface can minimize the difference in the coefficient of thermal expansion between the tungsten-copper contact end and the pure copper or copper-chromium alloy end, significantly reducing the probability of separation failure of the tungsten-copper contact end and the pure copper or copper-chromium alloy conductive end due to the difference in the coefficient of thermal expansion during subsequent welding and service.

[0028] To more clearly illustrate the purpose, technical solution, and advantages of the present invention, the present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. Attached Figure Description

[0029] Figure 1 This is a schematic diagram of a tungsten billet pressing die with a 4° inclined punch.

[0030] Figure 2 The image shows the morphology of copper-containing bicrystalline tungsten composite powder prepared by spray pyrolysis and hydrogen reduction.

[0031] Figure 3 This is a cross-sectional SEM image of a bicrystalline tungsten copper contact material with a gradient composition change from 65 wt.% to 85 wt.%. Detailed Implementation

[0032] Many specific details are set forth in the following description in conjunction with embodiments and comparative examples in order to provide a full understanding of the invention. However, it should be understood that the following detailed description is for illustrative purposes only and does not limit the scope of protection of the invention.

[0033] The continuous gradient bicrystalline tungsten-copper contact material disclosed in this invention has a continuous gradient structure in the direction perpendicular to the pressing surface. One end of the material has a tungsten content of 80–93 wt.%, and the other end has a tungsten content of 50–75 wt.%, with the remainder being copper and impurities. The impurity content does not exceed 0.2 wt.%, achieving a continuous gradient change in material composition without the formation of a macroscopic interface layer. The bicrystalline tungsten is composed of dual-sized tungsten grains, including a first tungsten grain of 3–7 μm and a second tungsten grain of 200–500 nm, with a mass ratio of 8:1 to 5:1 between the first and second tungsten grains.

[0034] The continuous gradient bicrystalline tungsten-copper contact material disclosed in this invention is prepared by melting oxygen-free copper into a tungsten blank with a continuous gradient composition. The raw material used for pressing the tungsten blank is a tungsten-copper composite powder with a bicrystalline tungsten structure obtained by spray pyrolysis and hydrogen reduction of tungsten powder and oxyacid copper salt. The specific preparation process includes the following steps:

[0035] (1) Tungsten powder is ball-milled and dispersed, and then mixed with a copper salt solution containing oxyanions to obtain a slurry. Preferably, the particle size of the tungsten powder is 3-8 μm, the ball milling time is 4-6 h, the ball-to-powder ratio is 3-2:1, the ball milling medium is anhydrous ethanol, and the dispersed tungsten powder is obtained by vacuum drying after ball milling.

[0036] The copper salts containing oxyanions include, but are not limited to, one or more of copper sulfate, copper nitrate, copper oxalate, copper carbonate, and copper acetate. Preferably, the concentration of the copper salt solution (using water as the solvent) is 1–3 mol / L, the ratio of tungsten powder to copper salt solution is 2–3 kg / L, and the mixture is stirred evenly using magnetic stirring to obtain a slurry.

[0037] (2) The slurry mixture obtained in step (1) is subjected to spray pyrolysis to obtain tungsten-copper mixed oxide powder. Preferably, the feed rate of the spray pyrolysis process is 50-180 ml / min, the inlet gas temperature is 230-260°C, the pyrolysis temperature is 550-750°C, and an inert gas such as argon or nitrogen is used as the protective atmosphere.

[0038] (3) The tungsten-copper mixed oxide powder obtained in step (2) is subjected to hydrogen reduction to obtain a composite powder of bicrystalline tungsten and copper. Preferably, the reduction temperature is 800-950℃, the reduction atmosphere is hydrogen atmosphere, the oxide powder layer thickness is 8-12mm, and the reduction time is 2-3h.

[0039] (4) The composite powder of bicrystalline tungsten and copper is pressed into a copper-containing tungsten billet with a continuous gradient distribution of W content and porosity. Copper in the composite powder is used as the pressing binder phase, while the W content and porosity in the tungsten billet have opposite continuous gradient distributions.

[0040] In this invention, compression molding can be performed using methods such as... Figure 1 The pressing die shown has a lower punch that is a beveled punch (wedge-shaped punch) and an upper punch that is a flat punch. The beveled punch's inclination angle is preferably controlled between 3° and 8°, for example, 4° as shown in the figure. The pressing surface (e.g., the horizontal plane shown in the figure) is perpendicular to the pressing direction. The copper-tungsten ingot obtained by pressing exhibits a continuous gradient distribution of W content and porosity, with the W content continuously increasing from end y1 to end y2, while the porosity continuously decreases from end y1 to end y2. The average pressing pressure is preferably 2–5 MPa / cm². 2 .

[0041] As Figure 1 In one variation of the illustrated embodiment, the lower punch can be a flat punch and the upper punch can be a sloping punch; or, both the lower punch and the upper punch can be sloping punches, in which case the sloping directions of the lower punch and the upper punch are opposite or, although the sloping directions are the same, they have different inclination angles.

[0042] (5) A continuous gradient bicrystalline tungsten-copper contact material is obtained by melting and infiltrating oxygen-free copper into a copper-containing tungsten billet in a molybdenum wire pusher furnace. Preferably, the melting and infiltrating temperature is 1250-1400℃, and the melting and infiltrating atmosphere is a mixture of hydrogen and inert gas with a mixing ratio of 1:2-5. The inert gas can be one or more of argon and nitrogen.

[0043] The following is a detailed description with reference to the embodiments.

[0044] Example 1

[0045] In the continuous gradient bicrystalline tungsten-copper contact material of Example 1, the tungsten content exhibits a gradient composition change from approximately 65 wt.% to approximately 85 wt.% from one end of the material to the opposite end. The bicrystalline tungsten comprises a first tungsten grain with an average size of approximately 7 μm and a second tungsten grain with an average size of approximately 300 nm, with a mass ratio of the first tungsten grain to the second tungsten grain of 5:1. Its preparation method includes the following steps:

[0046] (1) Tungsten powder with an average particle size of 8 μm was ball-milled for 4 hours at a ball-to-particle ratio of 3:1. Anhydrous ethanol was used as the milling medium. After ball milling, the powder was vacuum-dried to obtain dispersed tungsten powder. Copper sulfate was prepared into a solution with a concentration controlled at 2 mol / L. Tungsten powder was then added to the copper salt solution at a ratio of 2 kg / L and mixed evenly with magnetic stirring to obtain a slurry.

[0047] (2) The above mixed slurry was subjected to spray pyrolysis at a feed rate of 100 ml / min, an inlet gas temperature of 230°C, and a pyrolysis temperature of 700°C. Argon was used as the protective atmosphere. After the spray pyrolysis was completed, tungsten copper mixed oxide powder was obtained.

[0048] (3) The above-mentioned tungsten-copper mixed oxide powder was subjected to hydrogen reduction at a reduction temperature of 900℃, a hydrogen atmosphere, a material layer thickness of 10mm, and a reduction time of 3h. After reduction, a composite powder of bicrystalline tungsten and copper was obtained.

[0049] (4) A slanted punch die is used to press the composite powder of bicrystalline tungsten and copper into shape, and the average pressing pressure is controlled at 3 MPa / cm during the pressing process. 2 The tilt angle of the inclined punch is controlled at 4°. Copper in the composite powder is used as the pressing binder. After pressing, a tungsten billet with a tungsten content ranging from 65wt.% to 85wt.% is obtained.

[0050] (5) The copper-containing tungsten billet is infiltrated with oxygen-free copper in a molybdenum wire pusher furnace at a melting temperature of 1300℃. The melting atmosphere is a mixture of hydrogen and argon in a ratio of 1:3. After cooling, a continuous gradient bicrystalline tungsten-copper contact material is obtained.

[0051] Figure 2 The image shown is a morphology diagram of the bicrystalline tungsten-copper composite powder obtained after hydrogen reduction in Example 1. It can be clearly seen that the fine tungsten particles grown during the reduction process are attached to the surface of the coarse tungsten particles. The powder with this structural feature prepared by in-situ generation can ensure the uniform mixing and distribution of the two types of tungsten particles during subsequent pressing and sintering processes.

[0052] A portion of the middle section of the continuous gradient bicrystalline tungsten copper contact material sample obtained after pressing and melt infiltration in Example 1 was subjected to SEM characterization. The results are as follows: Figure 3 As shown, the coarse and fine tungsten particles are evenly mixed and distributed, which can effectively disperse the electric arc, improve the arc erosion resistance of the tungsten copper contact, and extend its service life.

[0053] Example 2

[0054] In the continuous gradient bicrystalline tungsten-copper contact material of Example 2, the tungsten content exhibits a gradient composition change from approximately 75 wt.% to approximately 93 wt.% from one end of the material to the opposite end. The bicrystalline tungsten comprises a first tungsten grain with an average size of approximately 5 μm and a second tungsten grain with an average size of approximately 500 nm, with a mass ratio of the first tungsten grain to the second tungsten grain of 7:1. Its preparation method includes the following steps:

[0055] (1) Tungsten powder with an average particle size of 6 μm was ball-milled for 4 hours at a ball-to-particle ratio of 3:1. Anhydrous ethanol was used as the milling medium. After ball milling, the powder was vacuum-dried to obtain dispersed tungsten powder. Copper sulfate was prepared into a solution with a concentration controlled at 2 mol / L. Tungsten powder was then added to the copper salt solution at a ratio of 3 kg / L and mixed evenly using magnetic stirring to obtain a slurry.

[0056] (2) The above mixed slurry was sprayed and pyrolyzed to obtain tungsten copper mixed oxide powder. During the spray pyrolysis process, the feed rate was 80 ml / min, the inlet gas temperature was 250℃, the pyrolysis temperature was 600℃, and argon was used as the protective atmosphere.

[0057] (3) The above-mentioned tungsten-copper mixed oxide powder was subjected to hydrogen reduction to obtain a composite powder of bicrystalline tungsten and copper. The reduction temperature was 850℃, the reduction atmosphere was hydrogen atmosphere, the material layer thickness was 8mm, and the reduction time was 2h.

[0058] (4) A slanted punch die is used to press the composite powder of bicrystalline tungsten and copper into shape, with an average pressing pressure of 5 MPa / cm. 2 The tilt angle of the inclined punch is controlled at 7°. Copper in the composite powder is used as the pressing binder. After pressing, a tungsten billet with a tungsten content ranging from 75wt.% to 93wt.% is obtained.

[0059] (5) Copper-containing tungsten billets were melt-infiltrated in a molybdenum wire pusher furnace at a melting temperature of 1400℃. The melting atmosphere was a mixture of hydrogen and nitrogen in a 1:5 ratio. After cooling, a continuous gradient bicrystalline tungsten-copper contact material was obtained.

[0060] Example 3

[0061] In the continuous gradient bicrystalline tungsten-copper contact material of Example 3, the tungsten content exhibits a gradient composition change from approximately 50 wt.% to approximately 80 wt.% from one end of the material to the opposite end. The bicrystalline tungsten comprises a first tungsten grain with an average size of approximately 3 μm and a second tungsten grain with an average size of approximately 200 nm, with a mass ratio of the first tungsten grain to the second tungsten grain of 5:1. Its preparation method includes the following steps:

[0062] (1) Tungsten powder with an average particle size of 4 μm was ball-milled for 4 hours at a ball-to-particle ratio of 2:1. Anhydrous ethanol was used as the milling medium. After ball milling, the powder was vacuum-dried to obtain dispersed tungsten powder. Copper sulfate was prepared into a solution with a concentration of 1 mol / L. Tungsten powder was then added to the copper salt solution at a ratio of 2 kg / L and mixed evenly with magnetic stirring to obtain a slurry.

[0063] (2) The above-mentioned mixed slurry was subjected to spray pyrolysis at a feed rate of 80 ml / min, an inlet gas temperature of 260℃, and a pyrolysis temperature of 550℃. Argon was used as the protective atmosphere. After the spray pyrolysis was completed, tungsten copper mixed oxide powder was obtained.

[0064] (3) The above-mentioned tungsten-copper mixed oxide powder was subjected to hydrogen reduction at a reduction temperature of 850°C and a hydrogen atmosphere. The material layer thickness was 12 mm and the reduction time was 2 h. After reduction, a composite powder of bicrystalline tungsten and copper was obtained.

[0065] (4) A slanted punch die is used to press the composite powder of bicrystalline tungsten and copper into shape, and the average pressing pressure is controlled at 3 MPa / cm during the pressing process. 2 The tilt angle of the inclined punch is controlled at 5°. Copper in the composite powder is used as the pressing binder. After pressing, a tungsten billet with a tungsten content ranging from 50wt.% to 80wt.% is obtained.

[0066] (5) Copper-containing tungsten billets are infiltrated with oxygen-free copper in a molybdenum wire pusher furnace at a melting temperature of 1250℃. The melting atmosphere is a mixture of hydrogen and argon in a ratio of 1:5. After cooling, a continuous gradient bicrystalline tungsten-copper contact material is obtained.

[0067] Although the present invention has been described above through embodiments, it should be understood that any equivalent changes made by those skilled in the art in accordance with the present invention without departing from the scope of the present invention should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a continuous gradient bicrystalline tungsten copper contact material, comprising the following steps: (1) Mix the ball-milled and dispersed W powder with a copper salt solution containing oxyacid anions to obtain a mixed slurry; (2) The mixed slurry is subjected to spray pyrolysis to obtain tungsten-copper mixed oxide powder; (3) The tungsten-copper mixed oxide powder is subjected to hydrogen reduction to obtain a composite powder of bicrystalline tungsten and copper; (4) The composite powder is pressed into a copper-tungsten blank with a continuous gradient distribution of W content and porosity, and the copper in the composite powder is used as the pressing binder phase. (5) Oxygen-free copper is melt-infiltrated into the copper-containing tungsten billet to obtain a continuous gradient bicrystalline tungsten-copper contact material.

2. The preparation method according to claim 1, wherein, Step (1) Select tungsten powder with a particle size of 3~8 μm and ball mill it for 4~6 h. The ball-to-material ratio is 3~2:

1. The ball milling medium is anhydrous ethanol. After ball milling, vacuum dry it to obtain dispersed tungsten powder.

3. The preparation method according to claim 1, wherein, In step (1), the concentration of the copper salt solution is 1~3 mol / L, and the mixing ratio of tungsten powder to copper salt solution is 2~3 kg / L. The mixture is stirred and mixed evenly to obtain a slurry.

4. The preparation method according to claim 1, wherein, The oxyacid anion copper salt is one or more of copper sulfate, copper nitrate, copper oxalate, copper carbonate, and copper acetate.

5. The preparation method according to claim 1, wherein, In step (2), the feed rate for spray pyrolysis is 50-180 ml / min, the inlet temperature is 230-260 ℃, the pyrolysis temperature is 550-750 ℃, and an inert gas is used as the protective atmosphere.

6. The preparation method according to claim 1, wherein, The reduction temperature in step (3) is 800~950 ℃, and the reduction time is 2~3h; the thickness of the oxide powder layer is 8~12mm.

7. The preparation method according to claim 1, wherein, Step (4) uses a die with a beveled punch for pressing, with an average pressing pressure of 2~5 MPa / cm. 2 The angle of inclination of the punch's bevel relative to the pressing and forming surface is controlled between 3° and 8°.

8. The preparation method according to claim 3, wherein, The melting temperature in step (5) is 1250~1400 ℃, and the melting atmosphere is a mixture of hydrogen and inert gas.

9. A continuous gradient bicrystalline tungsten-copper contact material obtained by the preparation method according to any one of claims 1-8, wherein, The tungsten content at one end of the continuous gradient bicrystalline tungsten-copper contact material is 80-93 wt.%, and the tungsten content at the other end is 50-75 wt.%. The tungsten content exhibits a continuous change from one end to the other without a macroscopic interface layer. The bicrystalline tungsten in the continuous gradient bicrystalline tungsten-copper contact material comprises a mixed distribution of first tungsten grains and second tungsten grains. The first tungsten grains have a larger average size than the second tungsten grains, and the mass ratio of the first tungsten grains to the second tungsten grains is 8-5:

1.

10. The continuous gradient bicrystalline tungsten-copper contact material according to claim 9, wherein, The average sizes of the first tungsten grain and the second tungsten grain are 3~7 μm and 200~500 nm, respectively.

Citation Information

Patent Citations

  • Preparation method of W-Cu continuous gradient composite

    CN110434343A

  • Method for preparing tungsten-copper continuous gradient material based on SLM technology

    CN114734056A

  • Tungsten-copper alloy with double-peak structure and preparation method of tungsten-copper alloy

    CN117340261A