Complete set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material

By forming a multi-layer stress control structure and an aluminum-doped zinc oxide layer on a sapphire single crystal substrate, the problem of compressive stress and thermal expansion stress when the zinc oxide layer grows on the sapphire substrate is solved, and high-quality transparent conductive films are prepared, improving improve the performance and reliability of optoelectronic devices.

CN118516764BActive Publication Date: 2024-10-25GUOJING HECHUANG (QINGDAO) TECH CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410599121.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-15
Publication Date
2024-10-25
Estimated Expiration
2044-05-15

AI Technical Summary

Technical Problem

When existing transparent optoelectronic devices prepare a zinc oxide layer on a sapphire single crystal substrate, problems such as compressive stress, large surface undulations, and high defect density often occur, which affect the conductive performance and light transmittance performance.

Method used

Plasma-enhanced atomic layer deposition and remote plasma-enhanced chemical vapor deposition are used to form a multi-layer stress control structure and annealing treatment to form a porous weakly bonded decoupling layer and an aluminum-doped zinc oxide layer to coordinate the lattice and thermal expansion stress. , to achieve dense, smooth, low-stress, and low-defect density growth of the zinc oxide layer.

Benefits of technology

The sapphire-based zinc oxide transparent material has a dense film layer, smooth surface, low stress, and low defect density, which improves the conductivity and light transmission properties, and improves the performance and reliability of transparent optoelectronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118516764B_ABST
    Figure CN118516764B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of optoelectronic materials, and provides a complete set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film materials, comprising: forming a first zinc oxide layer, a zinc-magnesium oxide layer, a second zinc oxide layer and an aluminum oxide template layer in sequence on the surface of a sapphire substrate by plasma enhanced atomic layer deposition, wherein the lattice constant of the zinc-magnesium oxide layer is smaller than the lattice constant of zinc oxide and the lattice constant of sapphire, and the thermal expansion coefficient of the zinc-magnesium oxide layer is larger than the thermal expansion coefficient of zinc oxide and the thermal expansion coefficient of sapphire; annealing the sapphire substrate formed with the first zinc oxide layer, the zinc-magnesium oxide layer, the second zinc oxide layer and the aluminum oxide template layer, so that pores are formed in the first zinc oxide layer, the zinc-magnesium oxide layer and the second zinc oxide layer; and forming an aluminum-doped zinc oxide layer on the surface of the aluminum oxide template layer by remote plasma enhanced chemical vapor deposition. The growth of a dense, flat, low-stress and low-defect density zinc oxide layer on the sapphire substrate is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of optoelectronic materials, and in particular to a complete set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film materials. Background Art

[0002] Existing transparent optoelectronic devices often use large-sized transparent glass as a substrate, first prepare an oxide transparent conductive thin film material (such as zinc oxide or indium tin oxide) as a lower electrode layer, and then prepare a transparent optoelectronic device structure layer, a transparent conductive upper electrode layer and a passivation protective layer in sequence. Since transparent glass is an amorphous material, the oxide transparent conductive thin film material grown on it can only be prepared into an amorphous layer or polycrystalline layer with high defect density and poor conductivity or light transmittance in most cases due to the lack of a single crystal template layer.

[0003] The inventors found that the size of sapphire single crystals has expanded from the early 2 inches to the current 8 inches, and is expected to expand to more than 18 inches, and the price is getting lower and lower. Therefore, the use of large-size sapphire transparent single crystal substrates to prepare transparent optoelectronic devices has a lower cost advantage. At the same time, aluminum-doped zinc oxide materials have better electronic conductivity and are currently the most ideal transparent electrode materials for transparent optoelectronic devices and transparent display technologies.

[0004] The inventors also found in practice that due to the large lattice mismatch and thermal expansion coefficient difference between zinc oxide and the sapphire single crystal substrate, when zinc oxide is directly prepared and grown on the sapphire single crystal substrate, large compressive stress often accumulates in the film layer, and three-dimensional (3D) island or one-dimensional (1D) columnar growth is prone to occur. The film layer has poor density, large surface undulations, high defect density, and both conductive properties and light transmittance properties are affected.

[0005] In order to coordinate the lattice mismatch stress and the thermal mismatch stress and realize the dense, flat, low-stress and low-defect density growth of the zinc oxide layer on the sapphire single crystal substrate, the present application provides a set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film materials. Summary of the invention

[0006] The present invention provides a complete set of equipment for producing a sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material, which is used to coordinate lattice mismatch stress and thermal mismatch stress to achieve dense, flat, low-stress, and low-defect density growth of a zinc oxide layer on a sapphire single crystal substrate.

[0007] In one aspect, the present invention provides a method for producing a sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material, comprising:

[0008] A first zinc oxide layer, a zinc magnesium oxide layer, a second zinc oxide layer and an aluminum oxide template layer are sequentially formed on the surface of a sapphire substrate by a plasma enhanced atomic layer deposition method, wherein the lattice constant of the zinc magnesium oxide layer is smaller than the lattice constant of zinc oxide and the lattice constant of sapphire, and the thermal expansion coefficient of the zinc magnesium oxide layer is larger than the thermal expansion coefficient of zinc oxide and the thermal expansion coefficient of sapphire;

[0009] Annealing the sapphire substrate having the first zinc oxide layer, the zinc magnesium oxide layer, the second zinc oxide layer and the aluminum oxide template layer formed thereon, so that pores are formed in the first zinc oxide layer, the zinc magnesium oxide layer and the second zinc oxide layer;

[0010] An aluminum-doped zinc oxide layer is formed on the surface of the aluminum oxide template layer of the sapphire substrate after annealing by remote plasma enhanced chemical vapor deposition.

[0011] According to a method for producing a sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material provided by the present invention, the size of the sapphire substrate includes 2 inches, 4 inches, 6 inches, 8 inches, 12 inches and 18 inches.

[0012] According to a method for producing a sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material provided by the present invention, annealing the sapphire substrate formed with the first zinc oxide layer, the zinc magnesium oxide layer, the second zinc oxide layer and the aluminum oxide template layer comprises:

[0013] Under the conditions that the working pressure is 1 Torr to 10 Torr and the heating temperature of the sapphire substrate is 750° C. to 1200° C., hydrogen gas with a flow rate of 1 scmm to 10 sccm is introduced to anneal the sapphire substrate for 10 minutes to 30 minutes.

[0014] On the other hand, the present invention also provides a complete set of equipment for producing a sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material, which is used to implement the above-mentioned method for producing a sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material, comprising:

[0015] A storage chamber, used for storing a tray, wherein the tray is used for placing a sapphire substrate;

[0016] an exchange chamber connected to the storage chamber;

[0017] a first deposition chamber connected to the exchange chamber, the first deposition chamber being used to sequentially form a first zinc oxide layer, a zinc magnesium oxide layer, a second zinc oxide layer and an aluminum oxide template layer on the surface of a sapphire substrate by plasma enhanced atomic layer deposition, wherein the lattice constant of the zinc magnesium oxide layer is smaller than the lattice constant of zinc oxide and the lattice constant of sapphire, and the thermal expansion coefficient of the zinc magnesium oxide layer is larger than the thermal expansion coefficient of zinc oxide and the thermal expansion coefficient of sapphire;

[0018] An annealing chamber connected to the exchange chamber, the annealing chamber being used to anneal the sapphire substrate formed with the first zinc oxide layer, the zinc magnesium oxide layer, the second zinc oxide layer and the aluminum oxide template layer;

[0019] A second deposition chamber connected to the exchange chamber, the second deposition chamber being used to form an aluminum-doped zinc oxide layer on the surface of the aluminum oxide template layer of the sapphire substrate after annealing by remote plasma enhanced chemical vapor deposition;

[0020] a robot, disposed in the exchange chamber, and capable of transferring the tray between any two of the storage chamber, the first deposition chamber, the annealing chamber, and the second deposition chamber;

[0021] An opening and closing device, the storage chamber, the first deposition chamber, the annealing chamber and the second deposition chamber are all connected to the exchange chamber through the corresponding opening and closing devices.

[0022] A complete set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film materials provided by the present invention also includes a glove box, which is connected to the storage chamber through the corresponding opening and closing device.

[0023] A complete set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film materials provided by the present invention also includes a nitrogen storage device. The glove box and the storage chamber are both connected to the nitrogen storage device. Before opening the opening and closing device between the glove box and the storage chamber, the nitrogen storage device introduces nitrogen into the glove box and the storage chamber.

[0024] A complete set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film materials provided by the present invention also includes a vacuum pumping device. The storage chamber, the exchange chamber, the first deposition chamber, the annealing chamber and the second deposition chamber are all connected to the vacuum pumping device. Before opening the opening and closing device between any one of the storage chamber, the first deposition chamber, the annealing chamber and the second deposition chamber and the exchange chamber, the vacuum pumping device sucks the gas in the storage chamber, the first deposition chamber, the annealing chamber or the second deposition chamber corresponding to the opening and closing device to be opened.

[0025] According to a complete set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film materials provided by the present invention, the storage chamber, the first deposition chamber, the annealing chamber and the second deposition chamber are arranged in sequence along the circumference of the exchange chamber.

[0026] According to a complete set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film materials provided by the present invention, the tray is provided with at least two sapphire substrates.

[0027] According to a complete set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film materials provided by the present invention, the opening and closing device is configured as a vacuum gate valve.

[0028] The method for producing a sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material provided by the present invention organically combines the plasma enhanced atomic layer deposition method to realize the low-temperature and slow generation of a first zinc oxide layer, a zinc magnesium oxide layer, a second zinc oxide layer and an aluminum oxide template layer, annealing to form a porous weakly bonded decoupling layer, and the remote plasma enhanced chemical vapor deposition method to realize the rapid generation of an aluminum-doped zinc oxide layer, so as to more effectively overcome the large mismatch stress problem of the sapphire-based zinc oxide transparent material, and also enable the sapphire-based zinc oxide transparent material to have the advantages of dense film layer, smooth surface, low stress, low defect density and high crystal quality.

[0029] The complete set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film materials provided by the present invention can implement the method for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film materials provided by the present invention, and therefore includes all the above-mentioned advantages of the method for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film materials. In addition, the production equipment is combined through multiple chambers, so that many parts of the equipment can be shared, which greatly reduces the equipment construction and production costs. In addition, under a high vacuum environment, the tray can be transferred and exchanged between various functional chambers through a manipulator, which can not only greatly shorten the heating and cooling time and improve the material preparation efficiency, but also avoid the introduction of unintentional doping impurities and particulate matter, and ensure that the purity, quality and photoelectric performance of the prepared materials are stable and have a high yield. The assembly line preparation can realize mass production and has high production capacity, which is easier to promote industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 It is a schematic structural diagram of a complete set of equipment for producing a sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material provided by an embodiment of the present invention;

[0032] Figure 2 It is a schematic diagram of the structure after a first zinc oxide layer, a zinc magnesium oxide layer, a second zinc oxide layer and an aluminum oxide template layer are sequentially formed on the surface of sapphire provided by an embodiment of the present invention;

[0033] Figure 3It is a schematic structural diagram of a sapphire-based aluminum-doped zinc oxide transparent material prepared based on a sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material production method provided by an embodiment of the present invention.

[0034] Reference numerals:

[0035] 100. Sapphire-based aluminum-doped zinc oxide transparent material; 101. First zinc oxide layer; 102. Zinc-magnesium oxide layer; 103. Second zinc oxide layer; 104. Aluminum oxide template layer; 105. Al-doped zinc oxide layer; 106. Sapphire substrate; 200. Sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material production equipment; 201. Storage room; 202. Exchange room; 203. First deposition chamber; 204. Annealing chamber; 205. Second deposition chamber; 206. Robot; 207. Opening and closing device; 208. Glove box; 209. Tray. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Combine the following Figure 1-Figure 2 The present invention describes a method for producing a sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material provided in an embodiment of the present invention.

[0038] Specifically, the production method comprises:

[0039] In the first step, a first zinc oxide layer 101, a zinc magnesium oxide layer 102, a second zinc oxide layer 103 and an aluminum oxide template layer 104 are sequentially formed on the surface of a sapphire substrate 106 by plasma enhanced atomic layer deposition. The lattice constant of the zinc magnesium oxide layer 102 is smaller than the lattice constant of zinc oxide and the lattice constant of sapphire, and the thermal expansion coefficient of the zinc magnesium oxide layer 102 is larger than the thermal expansion coefficient of zinc oxide and the thermal expansion coefficient of sapphire.

[0040] Specifically, the sapphire substrate 106 is a double-sided polished transparent single crystal substrate. A first zinc oxide layer 101, a zinc magnesium oxide layer 102, a second zinc oxide layer 103 and an aluminum oxide template layer 104 are sequentially deposited on the surface of the sapphire substrate 106, and the first zinc oxide layer 101, the zinc magnesium oxide layer 102, the second zinc oxide layer 103 and the aluminum oxide template layer 104 form a multilayer stress regulation structure. By regulating the magnesium component in zinc magnesium oxide (ZnMgO), the lattice constant of the zinc magnesium oxide layer 102 can be made smaller than the lattice constant of zinc oxide and the lattice constant of sapphire, and the thermal expansion coefficient of the zinc magnesium oxide layer 102 is greater than the thermal expansion coefficient of zinc oxide and the thermal expansion coefficient of sapphire.

[0041] The relatively mature plasma enhanced atomic layer deposition method is used to realize low-temperature ultra-thin preparation of the first zinc oxide layer 101, the zinc magnesium oxide layer 102, the second zinc oxide layer 103 and the aluminum oxide template layer 104, which can obtain ultra-thin layer materials with uniform and controllable components, dense film layers and smooth surfaces.

[0042] Furthermore, zinc oxide has a hexagonal wurtzite crystal structure with lattice constants a=0.3249nm, c=0.5204nm, and a-axis thermal expansion coefficient of 6.5×10 -6 K -1 (300K), the c-axis thermal expansion coefficient is 3.0×10 -6 K -1 (300K). Magnesium oxide has a cubic sodium chloride crystal structure, with a lattice constant a=0.4216nm and an a-axis thermal expansion coefficient of 10.5×10 -6 K -1 (300K); the lattice constant of the magnesium oxide crystal plane (0.2981nm) is smaller than that of the c-plane sapphire and zinc oxide, while the thermal expansion coefficient is larger than that of sapphire and zinc oxide. By adjusting the magnesium component in the zinc magnesium oxide, the lattice constant of the zinc magnesium oxide layer 102 can be adjusted to be smaller than that of sapphire and zinc oxide, and then the lattice mismatch stress is first transferred to the zinc magnesium oxide layer 102 for release, that is, the sapphire substrate 106 and the aluminum-doped zinc oxide layer 105 apply tensile stress to the zinc magnesium oxide layer 102 from top to bottom at the same time; the thermal expansion coefficient of the zinc magnesium oxide layer 102 can also be adjusted to be smaller than the thermal expansion coefficient of sapphire (7.5×10 -6 K -1 (300K)) and zinc oxide have large thermal expansion coefficients (6.5×10 -6 K -1 (300K)), and then the thermal mismatch stress can also be transferred to the zinc-magnesium-oxide layer 102 for release, that is, the sapphire substrate 106 and the aluminum-doped zinc oxide layer 105 apply tensile stress to the zinc-magnesium-oxide layer 102 from top and bottom at the same time.

[0043] In the second step, the sapphire substrate 106 formed with the first zinc oxide layer 101, the zinc magnesium oxide layer 102, the second zinc oxide layer 103 and the aluminum oxide template layer 104 is annealed to form pores in the first zinc oxide layer 101, the zinc magnesium oxide layer 102 and the second zinc oxide layer 103.

[0044] Specifically, the sapphire substrate 106 with a multilayer stress control structure formed on the surface is annealed, and the first zinc oxide layer 101 and the second zinc oxide layer 103 are self-decomposed to form a porous ultra-thin zinc oxide weakly bonded decoupling layer with controllable pore density, pore size and pore distribution by adjusting the high-temperature annealing temperature and annealing time, and the zinc-magnesium-oxygen layer 102 is decomposed into a porous ultra-thin zinc-magnesium-oxygen stress covariant layer with controllable pore density, pore size and pore distribution. Among them, the first zinc oxide layer 101 and the second zinc oxide layer 103 with high zinc component concentration have low pore density and large pore size after high-temperature annealing, and weak bonding and decoupling effects are more obvious, thereby forming a porous ultra-thin zinc oxide weakly bonded decoupling layer. The zinc-magnesium-oxygen layer 102 with a low zinc component concentration has a high pore density and a small pore size after high-temperature annealing, and the effect of coordinating the transfer of lattice mismatch stress and thermal mismatch stress is enhanced, thereby forming a porous ultra-thin zinc-magnesium-oxygen stress covariant layer.

[0045] Annealing further improves the crystal quality of the top aluminum oxide template layer 104 to form an ultra-thin aluminum oxide single crystal template layer, which is more conducive to the preparation and growth of a thicker aluminum-doped zinc oxide layer 105 with high crystal quality thereon.

[0046] The third step is to form an aluminum-doped zinc oxide layer 105 on the surface of the aluminum oxide template layer 104 of the annealed sapphire substrate 106 by remote plasma enhanced chemical vapor deposition.

[0047] Specifically, the aluminum-doped zinc oxide layer 105 is an aluminum-doped zinc oxide transparent conductive single crystal thin film. Finally, the sapphire-based aluminum-doped zinc oxide transparent material 100 is obtained, which can be used to improve the performance and reliability of transparent optoelectronic devices, including but not limited to transparent light-emitting devices, transparent inorganic LED devices, transparent organic OLED devices, transparent fluorescent display screen components, organic-inorganic composite photovoltaic devices, organic-inorganic composite photodetection devices, organic flexible sensor devices, etc.

[0048] In addition, the remote plasma enhanced chemical vapor deposition method can rapidly prepare single crystal thin films, thereby improving the production efficiency of the sapphire-based aluminum-doped zinc oxide transparent material 100 .

[0049] In this embodiment, by making the lattice constant of the zinc-magnesium-oxide layer 102 smaller than the lattice constant of zinc oxide and the lattice constant of sapphire, the thermal expansion coefficient of the zinc-magnesium-oxide layer 102 is larger than the thermal expansion coefficient of zinc oxide and the thermal expansion coefficient of sapphire, so that the sapphire substrate 106 and the aluminum-doped zinc oxide layer 105 apply tensile stress to the zinc-magnesium-oxide layer 102 from the top and bottom at the same time, thereby releasing the stress of both the sapphire substrate 106 and the aluminum-doped zinc oxide layer 105, and combining with the two layers of porous ultra-thin zinc oxide weak bonding decoupling layers formed by annealing to block the line dislocation from extending upward, compared with conventional buffer layer, low-temperature buffer layer and high-temperature buffer layer substrate preparation technology and patterned substrate technology, it can more effectively coordinate large mismatch stress, and it is easier to achieve the preparation and growth of high-crystalline quality single crystals with dense sapphire-based zinc oxide transparent conductive material film layers, smooth surface, low stress and low defect density.

[0050] Compared with amorphous or polycrystalline zinc oxide transparent conductive thin film materials prepared on conventional amorphous glass substrates, the sapphire-based aluminum-doped zinc oxide transparent material 100 designed with a multi-layer stress regulation structure has higher crystallization quality, a smoother surface and a denser film layer, and thus has better conductivity and light transmittance, and is more conducive to significantly improving the performance and reliability of transparent optoelectronic devices.

[0051] Compared with existing flexible substrate preparation technologies, such as sacrificial layer bonding technology, ion implantation buried layer technology and few-layer two-dimensional material technology, which have weak bonding decoupling effects and are difficult to control, the multilayer stress regulation structure used in the present invention is formed by plasma enhanced atomic layer deposition and annealing process. Both plasma enhanced atomic layer deposition and annealing process are mature preparation processes and have greater application and promotion value.

[0052] In summary, the method for producing a sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material provided in the embodiment of the present invention organically combines the plasma enhanced atomic layer deposition method to realize the low-temperature and slow generation of the first zinc oxide layer 101, the zinc magnesium oxide layer 102, the second zinc oxide layer 103 and the aluminum oxide template layer 104, annealing to form a porous weakly bonded decoupling layer, and the remote plasma enhanced chemical vapor deposition method to realize the rapid generation of the aluminum-doped zinc oxide layer 105, which can more effectively overcome the large mismatch stress problem of sapphire-based zinc oxide transparent materials, and can also make the sapphire-based zinc oxide transparent materials have the advantages of dense film layer, smooth surface, low stress, low defect density and high crystal quality, thereby realizing the efficient, high yield and high crystal quality preparation of sapphire-based aluminum-doped zinc oxide transparent materials 100.

[0053] In some embodiments provided by the present invention, the size of the sapphire substrate 106 includes 2 inches, 4 inches, 6 inches, 8 inches, 12 inches and 18 inches.

[0054] In some embodiments provided by the present invention, annealing the sapphire substrate 106 formed with the first zinc oxide layer 101, the zinc magnesium oxide layer 102, the second zinc oxide layer 103 and the aluminum oxide template layer 104 includes:

[0055] Under the conditions of a working pressure of 1 Torr to 10 Torr and a heating temperature of the sapphire substrate 106 of 750° C. to 1200° C., hydrogen gas with a flow rate of 1 scmm to 10 sccm is introduced to anneal the sapphire substrate 106 for 10 minutes to 30 minutes.

[0056] In this way, some zinc and oxygen components in the first zinc oxide layer 101, zinc magnesium oxide layer 102, and second zinc oxide layer 103 in the multilayer stress regulation structure can be heated and decomposed, so that the first zinc oxide layer 101 and the second zinc oxide layer 103 form a porous ultra-thin zinc oxide weakly bonded decoupling layer with low pore density and large pores, and the zinc magnesium oxide layer 102 forms a porous ultra-thin zinc magnesium oxide stress covariant layer with high pore density and small pores. The aluminum oxide layer forms an ultra-thin aluminum oxide single crystal template layer with improved crystal quality.

[0057] In addition, during the annealing process, hydrogen atoms can diffuse into the material and interact with impurities or foreign matter in the material, thereby removing these impurities or foreign matter, eliminating crystal defects, and improving the purity and structural integrity of the material. The diffused hydrogen atoms also help improve the thermal conductivity and electrical properties of the single crystal material.

[0058] In some embodiments provided by the present invention, forming the first zinc oxide layer 101 includes:

[0059] i) First, nitrogen is used as a carrier gas to carry the precursor source gas of diethyl zinc, with a gas flow rate of 2scmm to 5sccm, and the duration is 0.5s to 1s. Then, argon gas is introduced for purging, with a gas flow rate of 5scmm to 10sccm, and the duration is 5s to 10s. ii) Turn on the 13.58MHz RF power supply, apply 60W to 90W power, and introduce oxygen source gas, with a gas flow rate of 2scmm to 5sccm, and the duration is 2s to 5s. Turn off the RF power supply, and then purge argon gas with a gas flow rate of 5scmm to 10sccm for 5s to 10s. Repeat the two processes i) and ii) 20 to 30 times. For example, the thickness of the first zinc oxide layer 101 formed is 10nm.

[0060] In some embodiments provided by the present invention, forming the zinc-magnesium-oxide layer 102 includes:

[0061] i) First, nitrogen gas with a gas flow rate of 6 scmm to 12 sccm carries the precursor source gas of diethyl zinc and nitrogen gas with a gas flow rate of 2 scmm to 4 sccm carries the precursor source gas of bismuth magnesium for 2s to 3s, and the molar ratio of the two metal organic source gases is 3:1, and then argon gas with a gas flow rate of 5 scmm to 10 sccm is passed for 5s to 10s. ii) Turn on the 13.58MHz frequency RF power supply, apply 60W to 90W power, and pass the oxygen source gas with a gas flow rate of 2 scmm to 5 sccm for 2s to 5s. Turn off the RF power supply, and then pass argon gas with a gas flow rate of 5 scmm to 10 sccm for 5s to 10s. Repeat the two processes i) and ii) 40 to 60 times. For example, the thickness of the formed zinc magnesium oxide layer 102 is 20nm.

[0062] In some embodiments provided by the present invention, forming the second zinc oxide layer 103 includes:

[0063] i) First, nitrogen is used as a carrier gas to carry the precursor source gas of diethyl zinc, with a gas flow rate of 2scmm to 5sccm, and the duration is 0.5s to 1s. Then, argon gas is introduced for purging, with a gas flow rate of 5scmm to 10sccm, and the duration is 5s to 10s. ii) Turn on the 13.58MHz RF power supply, apply 60W to 90W power, and introduce oxygen source gas, with a gas flow rate of 2scmm to 5sccm, and the duration is 2s to 5s. Turn off the RF power supply, and then purge argon gas with a gas flow rate of 5scmm to 10sccm for 5s to 10s. Repeat the two processes i) and ii) 20 to 30 times. For example, the thickness of the second zinc oxide layer 103 formed is 10nm.

[0064] In some embodiments provided by the present invention, forming the aluminum oxide template layer 104 includes:

[0065] i) First, nitrogen gas with a gas flow rate of 5scmm to 10sccm is passed to carry the precursor source gas of triethylaluminum for 1s to 5s, and then argon gas with a gas flow rate of 5scmm to 10sccm is passed to purge for 5s to 10s. ii) RF power with a frequency of 13.58MHz is turned on, a power of 60W to 90W is applied, oxygen source gas with a gas flow rate of 2scmm to 5sccm is passed for 2s to 5s, the RF power is turned off, and argon gas with a gas flow rate of 5scmm to 10sccm is passed to purge for 5s to 10s. Repeat the two processes of i) and ii) 20 to 30 times.

[0066] In some embodiments provided by the present invention, forming the aluminum-doped zinc oxide layer 105 includes:

[0067] Under the condition of pressure of 0.1 Torr to 0.5 Torr, the substrate is heated to a temperature of 600° C. to 800° C. Argon gas with a gas flow rate of 10 scmm to 20 sccm is used to carry the precursor source gas of diethyl zinc and triethyl aluminum, and the molar ratio of the two is 1500:1. At the same time, oxygen source gas with a gas flow rate of 100 scmm to 300 sccm is introduced, and a remote inductively coupled plasma source (ICP) is turned on with a power of 700 W to 1000 W, and the preparation growth is carried out for 10 to 60 minutes.

[0068] The present invention also provides a sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material production complete set of equipment 200, which can be used to implement the above-mentioned sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material production method. The equipment includes a storage chamber 201, an exchange chamber 202, a first deposition chamber 203, an annealing chamber 204, a second deposition chamber 205, a robot 206 and an opening and closing device 207.

[0069] The storage chamber 201 is used to store the tray 209 , and the tray 209 is used to place the sapphire substrate 106 .

[0070] The exchange chamber 202 is connected to the storage chamber 201 .

[0071] The first deposition chamber 203 is connected to the exchange chamber 202, and is used to sequentially form a first zinc oxide layer 101, a zinc magnesium oxide layer 102, a second zinc oxide layer 103, and an aluminum oxide template layer 104 on the surface of the sapphire substrate 106 by plasma enhanced atomic layer deposition, that is, the first deposition chamber 203 is configured to implement plasma enhanced atomic layer deposition. The lattice constant of the zinc magnesium oxide layer is smaller than the lattice constant of zinc oxide and the lattice constant of sapphire, and the thermal expansion coefficient of the zinc magnesium oxide layer is greater than the thermal expansion coefficient of zinc oxide and the thermal expansion coefficient of sapphire.

[0072] The annealing chamber 204 is connected to the exchange chamber 202 and is used to anneal the sapphire substrate 106 formed with the first zinc oxide layer 101, the zinc magnesium oxide layer 102, the second zinc oxide layer 103 and the aluminum oxide template layer 104, that is, the annealing chamber 204 is used to implement an annealing process.

[0073] The second deposition chamber 205 is connected to the exchange chamber 202. The second deposition chamber 205 is used to form an aluminum-doped zinc oxide layer 105 on the surface of the aluminum oxide template layer 104 of the annealed sapphire substrate 106 through remote plasma enhanced chemical vapor deposition, that is, the second deposition chamber 205 is used to implement remote plasma enhanced chemical vapor deposition.

[0074] The robot arm 206 is disposed in the exchange chamber 202 , and can transfer the tray 209 between any two of the storage chamber 201 , the first deposition chamber 203 , the annealing chamber 204 , and the second deposition chamber 205 .

[0075] The storage chamber 201, the first deposition chamber 203, the annealing chamber 204 and the second deposition chamber 205 are all connected to the exchange chamber 202 through corresponding opening and closing devices 207. The opening and closing devices 207 are configured as vacuum gate valves.

[0076] Specifically, the sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material production equipment 200 includes:

[0077] Step 1: Place a plurality of trays 209 containing double-sided polished transparent single crystal sapphire substrates 106 in the storage chamber 201 .

[0078] Step 2: The tray 209 carrying the sapphire substrate 106 to be processed in the storage chamber 201 is transferred to the first deposition chamber 203 by the robot 206. A first zinc oxide layer 101, a zinc magnesium oxide layer 102, a second zinc oxide layer 103 and an aluminum oxide template layer 104 are sequentially formed on the surface of the sapphire substrate 106 by plasma enhanced atomic layer deposition, that is, a multi-layer stress regulation structure is formed.

[0079] Step 3: First, the tray 209 prepared with the multi-layer stress control structure is transferred to the annealing chamber by the robot 206, and then another tray 209 carrying the sapphire substrate 106 to be processed is transferred from the storage chamber 201 to the first deposition chamber 203. In the annealing chamber 204, under a hydrogen atmosphere, the sapphire substrate 106 formed with the first zinc oxide layer 101, the zinc magnesium oxide layer 102, the second zinc oxide layer 103 and the aluminum oxide template layer 104 is subjected to high-temperature high-vacuum annealing to form a multi-layer stress control structure including a porous ultra-thin zinc oxide weakly bonded decoupling layer, a porous ultra-thin zinc magnesium oxide stress covariant layer and an ultra-thin aluminum oxide single crystal template layer. At the same time, the preparation of the multi-layer stress control structure is repeated in the first deposition chamber 203.

[0080] Step 4: First, the tray 209 in the annealing chamber 204 is transferred to the second deposition chamber 205 by the robot 206, and then the tray 209 in the first deposition chamber 203 is transferred to the annealing chamber 204 in sequence, and the other tray 209 is transferred from the storage chamber 201 to the first deposition chamber 203. In the second deposition chamber 205, an aluminum-doped zinc oxide layer 105 is formed on the surface of the aluminum oxide template layer 104 of the annealed sapphire substrate 106 by remote plasma enhanced chemical vapor deposition. At the same time, high-temperature and high-vacuum annealing treatment under hydrogen atmosphere is repeated in the annealing chamber 204, and preparation of a multi-layer stress regulation structure is repeated in the first deposition chamber 203.

[0081] Step 5: First, the tray 209 in the second deposition chamber 205 is transferred to the storage chamber 201 for cooling by the robot 206. Then, the tray 209 in the annealing chamber 204 is transferred to the second deposition chamber 205, the tray 209 in the first deposition chamber 203 is transferred to the annealing chamber 204, and another tray 209 is transferred from the storage chamber 201 to the first deposition chamber 203.

[0082] Repeat steps 1 to 5 to achieve assembly line-style efficient mass production.

[0083] The sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material production complete set of equipment 200 provided in the embodiment of the present invention can implement the sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material production method provided by the present invention, and therefore simultaneously includes all the above-mentioned advantages of the sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material production method. In addition, the production equipment is combined through multiple chambers, so that many parts of the equipment can be shared, which greatly reduces the equipment construction and production costs. In addition, under a high vacuum environment, the tray 209 can be transferred and exchanged between various functional chambers through the manipulator 206, which can not only greatly shorten the heating and cooling time to improve the material preparation efficiency, but also avoid the introduction of unintentional doping impurities and particulate matter, and ensure that the purity, quality and photoelectric performance of the prepared material are stable and have a high yield. The assembly line preparation can realize mass production and has high production capacity, which is easier to promote industrialization.

[0084] In some embodiments provided in the embodiments of the present invention, the sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material production equipment 200 further includes a glove box 208. The glove box 208 is connected to the storage chamber 201 through a corresponding opening and closing device 207. Through the glove box 208, it is convenient to take out the prepared sapphire-based aluminum-doped zinc oxide transparent material 100 from the storage chamber 201 through the glove box 208, or to place the sapphire substrate 106 to be prepared in the storage chamber 201.

[0085] In some embodiments provided in the embodiments of the present invention, the sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material production equipment 200 further includes a nitrogen storage device. The glove box 208 and the storage chamber 201 are both connected to the nitrogen storage device, and before the opening and closing device 207 between the glove box 208 and the storage chamber 201 is opened, the nitrogen storage device passes nitrogen into the glove box 208 and the storage chamber 201.

[0086] In this embodiment, before transferring or exchanging the tray 209 between the storage chamber 201 and the glove box 208, the storage chamber 201 is first filled with nitrogen to a pressure close to that of the nitrogen in the glove box 208, and then the opening and closing device 207 is opened. After the transfer or exchange of the tray 209 is completed, the opening and closing device 207 is closed. In this way, sampling or taking samples under a nitrogen protective atmosphere can avoid introducing impurities into the equipment and the prepared materials, thereby affecting the material quality.

[0087] In some embodiments provided in the embodiments of the present invention, the sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material production equipment 200 also includes a vacuum pumping device.

[0088] The storage chamber 201, the exchange chamber 202, the first deposition chamber 203, the annealing chamber 204 and the second deposition chamber 205 are all connected to the vacuum equipment. Before opening the opening and closing device 207 between any one of the storage chamber 201, the first deposition chamber 203, the annealing chamber 204 and the second deposition chamber 205 and the exchange chamber 202, the vacuum equipment is used to suck the gas in the storage chamber 201, the first deposition chamber 203, the annealing chamber 204 or the second deposition chamber 205 corresponding to the opening and closing device 207 to be opened.

[0089] In this embodiment, before the exchange chamber 202 and each chamber transfer or exchange the tray 209, it is necessary to first evacuate to a similar vacuum degree, then open the corresponding vacuum gate valve, complete the transfer or exchange of the substrate tray 209, and then close the vacuum gate valves between each other to avoid introducing impurities into the prepared materials. Similarly, when the glove box 208 and the storage chamber 201 complete the transfer or exchange of the tray 209, close the opening and closing device 207 between the glove box 208 and the storage chamber 201, and then evacuate the storage chamber 201 to avoid introducing impurities into the prepared materials.

[0090] In some embodiments provided in the embodiments of the present invention, the storage chamber 201, the first deposition chamber 203, the annealing chamber 204 and the second deposition chamber 205 are arranged in sequence along the circumference of the exchange chamber 202. Such an arrangement facilitates the robot 206 to transfer the tray 209 between the storage chamber 201, the first deposition chamber 203, the annealing chamber 204 and the second deposition chamber 205.

[0091] In some embodiments provided in the embodiments of the present invention, the tray 209 is provided with at least two sapphire substrates 106. Such a configuration can improve the production efficiency of the sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material production equipment 200.

[0092] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for producing a sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material, characterized in that: include: A first zinc oxide layer, a zinc magnesium oxide layer, a second zinc oxide layer and an aluminum oxide template layer are sequentially formed on the surface of a sapphire substrate by a plasma enhanced atomic layer deposition method, wherein the lattice constant of the zinc magnesium oxide layer is smaller than the lattice constant of zinc oxide and the lattice constant of sapphire, and the thermal expansion coefficient of the zinc magnesium oxide layer is larger than the thermal expansion coefficient of zinc oxide and the thermal expansion coefficient of sapphire; Annealing the sapphire substrate having the first zinc oxide layer, the zinc magnesium oxide layer, the second zinc oxide layer and the aluminum oxide template layer formed thereon, so that pores are formed in the first zinc oxide layer, the zinc magnesium oxide layer and the second zinc oxide layer; An aluminum-doped zinc oxide layer is formed on the surface of the aluminum oxide template layer of the sapphire substrate after annealing by remote plasma enhanced chemical vapor deposition.

2. The method for producing a sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material according to claim 1, characterized in that: The sizes of the sapphire substrate include 2 inches, 4 inches, 6 inches, 8 inches, 12 inches and 18 inches.

3. The method for producing a sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material according to claim 1, characterized in that: Annealing the sapphire substrate having the first zinc oxide layer, the zinc magnesium oxide layer, the second zinc oxide layer and the aluminum oxide template layer formed thereon, comprising: Under the conditions that the working pressure is 1 Torr to 10 Torr and the heating temperature of the sapphire substrate is 750° C. to 1200° C., hydrogen gas with a flow rate of 1 scmm to 10 sccm is introduced to anneal the sapphire substrate for 10 minutes to 30 minutes.

4. A complete set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material, characterized in that: include: A storage chamber, used for storing a tray, wherein the tray is used for placing a sapphire substrate; an exchange chamber connected to the storage chamber; a first deposition chamber connected to the exchange chamber, the first deposition chamber being used to sequentially form a first zinc oxide layer, a zinc magnesium oxide layer, a second zinc oxide layer and an aluminum oxide template layer on the surface of a sapphire substrate by plasma enhanced atomic layer deposition, wherein the lattice constant of the zinc magnesium oxide layer is smaller than the lattice constant of zinc oxide and the lattice constant of sapphire, and the thermal expansion coefficient of the zinc magnesium oxide layer is larger than the thermal expansion coefficient of zinc oxide and the thermal expansion coefficient of sapphire; An annealing chamber connected to the exchange chamber, the annealing chamber being used to anneal the sapphire substrate formed with the first zinc oxide layer, the zinc magnesium oxide layer, the second zinc oxide layer and the aluminum oxide template layer; A second deposition chamber connected to the exchange chamber, the second deposition chamber being used to form an aluminum-doped zinc oxide layer on the surface of the aluminum oxide template layer of the sapphire substrate after annealing by remote plasma enhanced chemical vapor deposition; a robot, disposed in the exchange chamber, and capable of transferring the tray between any two of the storage chamber, the first deposition chamber, the annealing chamber, and the second deposition chamber; An opening and closing device, the storage chamber, the first deposition chamber, the annealing chamber and the second deposition chamber are all connected to the exchange chamber through the corresponding opening and closing devices.

5. The complete set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material according to claim 4, characterized in that: It also includes a glove box, which is connected to the storage chamber through the corresponding opening and closing device.

6. The complete set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material according to claim 5, characterized in that: It also includes a nitrogen storage device, and the glove box and the storage chamber are both connected to the nitrogen storage device. Before opening the opening and closing device between the glove box and the storage chamber, the nitrogen storage device introduces nitrogen into the glove box and the storage chamber.

7. The complete set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material according to claim 4, characterized in that: It also includes a vacuum pumping device, and the storage chamber, the exchange chamber, the first deposition chamber, the annealing chamber and the second deposition chamber are all connected to the vacuum pumping device. Before opening the opening and closing device between any one of the storage chamber, the first deposition chamber, the annealing chamber and the second deposition chamber and the exchange chamber, the vacuum pumping device sucks the gas in the storage chamber, the first deposition chamber, the annealing chamber or the second deposition chamber corresponding to the opening and closing device to be opened.

8. The complete set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material according to claim 4, characterized in that: The storage chamber, the first deposition chamber, the annealing chamber, and the second deposition chamber are sequentially arranged along the circumference of the exchange chamber.

9. The complete set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material according to claim 4, characterized in that: The tray is provided with at least two sapphire substrates.

10. The complete set of equipment for producing sapphire-based aluminum-doped zinc oxide transparent conductive single crystal thin film material according to claim 4, characterized in that: The opening and closing device is configured as a vacuum gate valve.

Citation Information

Patent Citations

  • Methods for depositing a high-k dielectric material using chemical vapor deposition process

    CN101298663A

  • Automated batch production thin film deposition systems and methods of using the same

    CN113474485A

  • Preparation method of aluminum-doped zinc oxide film

    CN115652277A

  • Method for adding aluminum to zinc oxide transparent conductive film

    JP2005068544A