Molecular sieve encapsulated heteropolyacid salt composite catalyst, preparation method and application thereof
By encapsulating and modifying the heteropoly acid salt composite catalyst on the silicon germanium molecular sieve ITQ-44, the environmental pollution and catalyst separation problems in the oxidation step in the production of isooctanoic acid are solved, and efficient and low-cost production of isooctanoic acid is achieved, improving the Thermal stability and catalytic efficiency of catalysts.
Patent Information
- Application Number
- CN202411016789.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-07-29
Smart Images

Figure CN118527170B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalysts, and in particular relates to a molecular sieve encapsulated heteropolyacid salt composite catalyst, a preparation method and application thereof. Background Art
[0002] 2-Ethylhexanoic Acid (2-EHA), commonly known as isooctanoic acid, is an important synthetic saturated branched fatty acid. It usually reacts with a variety of metal compounds to form isooctanoic acid metal salts, which are widely used in paint driers, PVC stabilizers, pharmaceutical salt-forming agents, etc. In addition, its ester compounds are also commonly used in the preparation of fungicides, cosmetics, plasticizers, etc.
[0003] The preparation of isooctanoic acid usually adopts isooctyl alcohol oxidation method and butyraldehyde condensation hydrogenation method. The advantages of isooctyl alcohol oxidation method are that raw materials are easily available and the operation is simple, but the disadvantages are that the process flow is long, the three wastes are discharged in a large amount, and the production scale is small. The butyraldehyde condensation hydrogenation method uses n-butyraldehyde as raw material, produces isooctyl aldehyde through condensation dehydration, and then prepares isooctyl acid after hydrogenation, oxidation and other steps. This method is easy to scale production and has high yield. It has become the mainstream process of isooctyl acid production. However, in the oxidation step of this process, the strong oxidants such as KMnO4 commonly used will seriously pollute the ecological environment. Developing a green oxidation synthesis process is a problem that needs to be solved urgently, and the design of the catalyst is the key to solving this problem.
[0004] Patent application CN102701944A, patent US5739352A, patent application CN110773234A, patent application CN109433270A respectively adopt phosphorus molybdenum vanadium heteropoly acid, amine or amine-N-oxide, nano gold carbon nitride, porphyrin biomimetic supported catalyst to produce isooctanoic acid.Wherein, amine or amine-N-oxide, nano gold carbon nitride, porphyrin biomimetic supported catalyst have the problems such as high preparation cost, poor mass transfer effect, long reaction time, and are difficult to industrialization.By comparison, phosphorus molybdenum vanadium heteropoly acid has application potential, but the subject matter of such catalyst is that it belongs to homogeneous catalyst, is difficult to separate from reaction system.Therefore, need to design and develop a kind of multiphase phosphorus molybdenum vanadium heteropoly acid catalyst and related process to realize the green production of isooctanoic acid. Summary of the invention
[0005] The present invention aims at the deficiencies of the above-mentioned prior art and provides a molecular sieve encapsulated heteropolyacid salt composite catalyst, a preparation method and its application. The preparation method proposed in the present invention can make the catalytic active components evenly dispersed in the molecular sieve, and the prepared catalyst has strong thermal stability and high catalytic efficiency, simple process and low cost.
[0006] The specific technical solutions are as follows:
[0007] One of the purposes of the present invention is to provide a molecular sieve encapsulated heteropoly acid salt composite catalyst, comprising a heteropoly acid and a carrier, wherein the heteropoly acid has the following chemical expression: a B b PMo 12-n V n O 40 ;
[0008] In the formula: A is at least one of Ni, Cu, Zn, and Fe; B is at least one of Co, Mn, La, Ce, Sb, and Sn;
[0009] Wherein: a, b, n are molar coefficients, 0.05≤a≤5, 0.02≤b≤2, 0<n≤3;
[0010] The carrier is silicon germanium molecular sieve ITQ-44.
[0011] Furthermore, the carrier is preferably Al-doped silicon germanium molecular sieve ITQ-44.
[0012] Furthermore, the silicon germanium molecular sieve ITQ-44 is preferably treated with ammonium modification.
[0013] Furthermore, the molecular sieve encapsulated heteropoly acid salt catalyst preferably comprises 10 to 30 parts of heteropoly acid and 70 to 90 parts of carrier, in parts by weight.
[0014] Furthermore, in the chemical expression: 0.1≤a≤4, 0.05≤b≤1.8, 0.5≤n≤2.5.
[0015] More preferably, in the chemical expression: 0.2≤a≤3, 0.1≤b≤1.5, 1≤n≤2.
[0016] Specifically, the heteropoly acid is at least one of the following chemical formulas:
[0017] Cu 1.5 Ce 0.3 PMo 11 VO 40 ;
[0018] Ni 2.5 Sb 0.5 PMo 10 V2O 40 ;
[0019] Fe 0.3 Co 1.5 PMo 11 VO 40 ;
[0020] NiMn 0.2 PMo 11VO 40 ;
[0021] Cu 0.8 La 1.2 PMo 11 VO 40 .
[0022] Specifically, the molecular sieve encapsulated heteropoly acid salt composite catalyst is at least one of the following chemical formulas:
[0023] Cu 1.5 Ce 0.3 PMo 11 VO 40 / Al-ITQ-44;
[0024] Ni 2.5 Sb 0.5 PMo 10 V2O 40 / Al-ITQ-44;
[0025] Fe 0.3 Co 1.5 PMo 11 VO 40 / Al-ITQ-44;
[0026] NiMn 0.2 PMo 11 VO 40 / Al-ITQ-44;
[0027] Cu 0.8 La 1.2 PMo 11 VO 40 / Al-ITQ-44.
[0028] The second object of the present invention is to provide a method for preparing the above molecular sieve encapsulated heteropolyacid salt composite catalyst, comprising the following steps:
[0029] S1. Obtaining a carrier; the carrier is a silicon germanium molecular sieve ITQ-44;
[0030] S2. In situ synthesis of heteropoly acid: reacting a carrier, MoO3, V2O5, phosphoric acid, a compound containing element A and a compound containing element B, and drying to obtain a catalyst powder;
[0031] S3. Calcination: Calcinate the catalyst powder to obtain a catalyst.
[0032] The present invention uses the molecular sieve ITQ-44 with a large cage space (d=1.74nm) structure as a carrier, and encapsulates the heteropoly acid molecules (d=1.1~1.2nm) in the large cage structure of the molecular sieve. The small window aperture can prevent the heteropoly acid molecules from being lost from the molecular sieve, thereby ensuring the number of catalytically active components. Compared with the reported Y-type molecular sieve super cage structure (1.3nm) encapsulating heteropoly acid molecules, the larger cage space of ITQ-44 is conducive to the diffusion of large spatial steric hindrance branched aliphatic organic compounds in the cage, thereby improving its catalytic efficiency. The heteropoly acid molecules can be evenly dispersed in the ITQ-44 molecular sieve by the in-situ synthesis method, avoiding the agglomeration phenomenon of the traditional impregnation method. In addition, the encapsulation method can also greatly increase the specific surface area of the active component heteropoly acid, expose more active sites, and help improve the catalytic activity.
[0033] Further, in step S1: the carrier is Al-doped silicon germanium molecular sieve ITQ-44. The preparation method of the carrier preferably comprises: dissolving colloidal silica and GeO2 into an aqueous solution of benzyltriethylammonium hydroxide, adding Al(OH)3, NH4F and NH4Cl to react, and then calcining.
[0034] The presence of Al ensures the acidity of the molecular sieve, which is conducive to the subsequent ion exchange ammonium modification treatment. The control of Al content is crucial to the stability of heteropolyacids. Compared with the Al removal process required for Y-type molecular sieves, the present invention uses a direct synthesis method to accurately control the Al content in the molecular sieve, simplifies the process flow, and avoids the use of a large number of chemical reagents.
[0035] Specifically, in step S1, the preparation method of the carrier preferably includes: dissolving colloidal silica and GeO2 into a benzyltriethylammonium hydroxide aqueous solution, stirring evenly, adding Al(OH)3, NH4F and NH4Cl, heating and stirring at 60-90°C for 1-10 h to obtain a mixed solution; transferring the mixed solution into a hydrothermal autoclave with a tetrafluoroethylene liner, and crystallizing at 140-200°C for 1-3 days; after cooling to room temperature, filtering the solid product, washing it several times with deionized water and ethanol, and drying it; and calcining it at 300-600°C in an air atmosphere for 2-8 h to obtain Al-doped silicon germanium molecular sieve ITQ-44.
[0036] Among them, the molar ratio of Si to Ge is preferably (0.5~5):1, and more preferably (1~2):1.
[0037] Among them, the molar ratio of benzyltriethylammonium hydroxide to (Si+Ge) is preferably 1: (3~6), and more preferably 1: (4~5).
[0038] Among them, the molar ratio of Al(OH)3 to (Si+Ge) is preferably (0.01~0.1):1, and more preferably (0.02~0.05):1.
[0039] Among them, the molar ratio of NH4F to (Si+Ge) is preferably 1: (2~20), and more preferably 1: (6~12).
[0040] The molar ratio of NH4Cl to (Si+Ge) is preferably 1: (2-20), and more preferably 1: (4-8).
[0041] Among them, the preparation method of benzyltriethylammonium hydroxide preferably includes: mixing benzyltriethylammonium bromide and anion exchange resin to convert benzyltriethylammonium bromide into benzyltriethylammonium hydroxide. The preparation conditions are preferably: reaction temperature 20~40℃, reaction time 15 min~4 h. In the above preparation method, the mass ratio of benzyltriethylammonium bromide and anion exchange resin is preferably 1: (1~10), more preferably 1: (2~5). The anion exchange resin is preferably one of D202, 201×7, Amberlite IRA-400, Amberlite IRA-900, Amberlite IRA-910, Lewatit MP-600, Diaion PA-408, SA-10A; Dowex SBR; Purolite A600, Purolite Bromide Plus / 9218, MIEX-Bromide, MIEX-DOC, and MIEX-Gold.
[0042] Further, in step S1: the carrier is subjected to ion exchange modification treatment using a modifier to obtain an ammonium type molecular sieve.
[0043] After the molecular sieve is modified by ion exchange, it can be transformed into an ammonium molecular sieve. The negatively charged heteropoly acid radicals use the positively charged ammonium ions in the molecular sieve as active sites. Under the attraction of the charge, the two can be firmly combined to form heteropoly acid ammonium salts, which greatly improves the thermal stability of the heteropoly acid and ensures the life of the catalyst. At the same time, the addition of ammonium salts transforms the heteropoly acid from a triclinic form to a cubic form. The presence of the cubic form significantly improves the conversion rate and selectivity.
[0044] Furthermore, in step S1: the modifier is at least one of ammonium chloride, ammonium nitrate, ammonium acetate, ammonium sulfate, ammonium bisulfate, ammonium carbonate, ammonium bicarbonate, ammonium bromide, ammonium iodide, and ammonium fluoride.
[0045] Furthermore, in step S1, the modification treatment conditions are preferably: placing silicon germanium molecular sieve ITQ-44 (preferably Al-doped silicon germanium molecular sieve ITQ-44) in a modifier solution, heating and stirring at 40-90° C. for 0.5-6 h, filtering, washing, and drying to obtain an ammonium type molecular sieve.
[0046] The concentration of the modifier solution is preferably 0.5-5 mol / L, more preferably 1-3 mol / L. In the ion exchange modification treatment, the molecular sieve and the modifier solution are preferably used in a ratio of 1 g: (5-50) mL, more preferably 1 g: (10-30) mL.
[0047] Further, in step S2: the compound containing element A and the compound containing element B are at least one of nitrates, carbonates, sulfates, acetates, oxalates, chlorides, hydroxides and oxides of their corresponding elements.
[0048] Further, in step S2: the modified Al-ITQ-44 is placed in a mixed solution containing MoO3, V2O5 and phosphoric acid, refluxed and stirred, a compound containing element A and a compound containing element B are added, and the stirring is continued and the catalyst powder is obtained after drying.
[0049] Specifically, the working conditions of step S2 include: adding MoO3 and V2O5 to deionized water, heating to 80-95°C and stirring for 0.5-2 h to obtain a mixed solution; placing the carrier into the mixed solution, stirring at 80-95°C for 10-30 min, adding phosphoric acid dropwise, reflux stirring at 80-95°C for 2-8 h; adding a compound containing element A and a compound containing element B, continuing stirring, filtering and drying to obtain a catalyst powder.
[0050] Wherein, in step S2: the mass ratio of the carrier to the synthesized heteropolyacid is preferably 1: (3~19).
[0051] Wherein, in step S2: after adding the compound containing element A and the compound containing element B, preferably heating and stirring at 60-80° C. for 1-5 h.
[0052] Wherein, in step S2: the drying temperature is preferably 80-120° C., and the drying time is preferably 8-24 h.
[0053] Furthermore, in step S3, the specific conditions of calcination are preferably: calcination at 200-400° C. for 2-24 h.
[0054] Furthermore, in step S3: calcination is preferably performed in an air atmosphere.
[0055] Furthermore, in step S3: the heating rate of calcination is preferably 2-10°C / min.
[0056] The third object of the present invention is to provide the use of the above molecular sieve encapsulated heteropolyacid salt catalyst in catalyzing the oxidation of high-carbon aliphatic aldehydes to high carbonic acid.
[0057] The test results confirm that the molecular sieve encapsulated heteropolyacid salt catalyst of the present invention can improve the reaction conversion rate and selectivity.
[0058] The carbon number of the high-carbon aliphatic aldehyde is ≥ 8. Preferably, the carbon number is 8-12, and more preferably, 8-9.
[0059] Furthermore, the high-carbon aliphatic aldehyde is at least one of 2-ethylhexanal (isooctanal), n-octanal, n-nonanal, and isononanal.
[0060] The beneficial effects of the present invention are as follows:
[0061] (1) The encapsulation strategy adopted by the present invention is to encapsulate the active component heteropoly acid inside the molecular sieve ITQ-44 with a large cage space, which can effectively prevent the loss of the active component. The regular molecular sieve structure ensures the uniform distribution of the heteropoly acid in the molecular sieve and avoids agglomeration.
[0062] (2) The present invention transforms the molecular sieve into an ammonium type molecular sieve through ion exchange modification. The negatively charged heteropoly acid radicals use the positively charged ammonium ions in the molecular sieve as active sites. Under the attraction of the charge, the two are firmly combined to form heteropoly acid ammonium salts, which greatly improves the thermal stability of the heteropoly acid and ensures the life of the catalyst. At the same time, the addition of ammonium salts transforms the heteropoly acid from a triclinic crystal form to a cubic crystal form. The presence of the cubic crystal form significantly improves the conversion rate and selectivity.
[0063] (3) The present invention uses Al-doped silicon germanium molecular sieve ITQ-44 as a carrier. The presence of Al ensures the acidity of the molecular sieve, which is conducive to the subsequent ion exchange ammonium modification treatment. The present invention adopts a direct synthesis method to accurately control the doping amount of Al and avoid excessive Al from destroying the heteropoly acid structure.
[0064] (4) The catalyst of the present invention has strong thermochemical stability. When used in gas-solid phase catalytic reactions, it can meet the requirements of large-scale continuous production. There is no separation problem between the catalyst and the reaction system, which effectively solves the post-treatment problem of liquid-solid system catalysts.
[0065] (5) The catalyst of the present invention has excellent catalytic effect and can significantly improve the reaction conversion rate and selectivity in the reaction of catalyzing the oxidation of high-carbon aliphatic aldehydes to high carbonic acid. BRIEF DESCRIPTION OF THE DRAWINGS
[0066] Figure 1 This is the X-ray diffraction pattern of the catalyst obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0067] The principles and features of the present invention are described below in conjunction with examples, which are only used to explain the present invention and are not used to limit the scope of the present invention. The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial sources. Example 1
[0068] The steps for preparing molecular sieve encapsulated heteropolyacid salt composite catalyst are as follows:
[0069] S1. Get the vector:
[0070] (1) Preparation of benzyltriethylammonium hydroxide: Dissolve 6.8 g of benzyltriethylammonium bromide in 100 mL of deionized water, add 32.275 g of D202 anion exchange resin to the above solution, stir at 30°C for 1 h, filter the solid resin, and obtain a benzyltriethylammonium hydroxide aqueous solution.
[0071] (2) Synthesis of Al-doped silicon-germanium molecular sieve ITQ-44: 5.207 g of colloidal silica (hydrated silica, M=78.1) and 3.488 g of GeO2 were dissolved in the above-mentioned benzyltriethylammonium hydroxide aqueous solution, stirred evenly, and then 0.312 g of Al(OH)3, 0.37 g of NH4F and 0.802 g of NH4Cl were added, and the mixture was heated and stirred at 80°C for 4 h to obtain a mixed solution; the mixed solution was transferred into a hydrothermal autoclave lined with tetrafluoroethylene and crystallized at 180°C for 2 days; after cooling to room temperature, the solid product was filtered, washed several times with deionized water and ethanol, and dried; and calcined at 500°C in air atmosphere for 6 h to obtain Al-doped silicon-germanium molecular sieve ITQ-44, which was labeled as Al-ITQ-44.
[0072] (3) 5 g of the above Al-ITQ-44 was placed in 50 mL of ammonium nitrate solution (2 mol / L), heated and stirred at 80 °C for 2 h, filtered, washed with deionized water, and dried at 100 °C for 10 h to obtain ammonium Al-ITQ-44.
[0073] S2. In-situ synthesis of heteropoly acid: 0.887 g MoO3 and 0.051 g V2O5 were placed in 100 mL deionized water, heated to 90°C and stirred for 0.5 h to obtain a mixed solution; 4 g ammonium Al-ITQ-44 was placed in the above mixed solution, stirred at 90°C for 15 min, 0.055 g phosphoric acid was added dropwise, and refluxed at 90°C with stirring for 4 h to obtain a suspension; 20 mL of a water mixture containing 0.203 g copper nitrate trihydrate and 0.092 g ammonium cerium nitrate was added dropwise to the above suspension, stirred at 70°C for 3 h, filtered, and dried at 100°C for 12 h to obtain a catalyst powder.
[0074] S3. The catalyst powder was heated to 380°C in an air atmosphere at a heating rate of 10°C / min and calcined for 6 h to obtain a molecular sieve encapsulated heteropolyacid salt catalyst.
[0075] The composition of the catalyst obtained is Cu 1.5 Ce 0.3 PMo 11 VO 40 / Al-ITQ-44, its X-ray diffraction pattern is shown in Figure 1 . Example 2
[0076] Referring to Example 1, the difference from Example 1 is that step S2 is as follows: 0.835 g MoO3 and 0.105 g V2O5 are added to 100 mL deionized water, heated to 90° C. and stirred for 0.5 h to obtain a mixed solution; 4 g ammonium type Al-ITQ-44 is added to the mixed solution, stirred at 90° C. for 15 min, 0.057 g phosphoric acid is added dropwise, and refluxed at 90° C. for 4 h to obtain a suspension; 5 mL of a 0.1 M hydrochloric acid solution containing 0.422 g nickel nitrate hexahydrate and 0.066 g antimony trichloride is added dropwise to the suspension, stirred at 70° C. for 4 h, filtered, and dried at 100° C. for 12 h to obtain a catalyst powder.
[0077] The remaining technical features are the same as those of Example 1.
[0078] The composition of the obtained catalyst is Ni 2.5 Sb 0.5 PMo 10 V2O 40 / Al-ITQ-44. Example 3
[0079] Referring to Example 1, the difference from Example 1 is that step S2 is: 0.887 g MoO3 and 0.051 g V2O5 are added to 100 mL deionized water, heated to 90°C and stirred for 0.5 h to obtain a mixed solution; 4 g ammonium type Al-ITQ-44 is added to the mixed solution, stirred at 90°C for 15 min, 0.055 g phosphoric acid is added dropwise, and refluxed at 90°C for 4 h to obtain a suspension; 20 mL of a water mixture containing 0.068 g ferric nitrate nonahydrate and 0.2 g cobalt dichloride hexahydrate is added dropwise to the suspension, stirred at 70°C for 3 h, filtered, and dried at 100°C for 12 h to obtain a catalyst powder.
[0080] The remaining technical features are the same as those of Example 1.
[0081] The composition of the catalyst obtained is Fe 0.3 Co1.5 PMo 11 VO 40 / Al-ITQ-44. Example 4
[0082] Referring to Example 1, the difference from Example 1 is that step S2 is: 0.887 g MoO3 and 0.051 g V2O5 are added to 100 mL deionized water, heated to 90°C and stirred for 30 min to obtain a mixed solution; 4 g ammonium type Al-ITQ-44 is added to the above mixed solution, stirred at 90°C for 15 min, 0.055 g phosphoric acid is added dropwise, and refluxed at 90°C for 4 h to obtain a suspension; 20 mL of a water mixture containing 0.133 g nickel chloride hexahydrate and 0.03 g manganese acetate dihydrate is added dropwise to the above suspension, stirred at 70°C for 3 h, filtered, and dried at 100°C for 12 h to obtain a catalyst powder.
[0083] The remaining technical features are the same as those of Example 1.
[0084] The composition of the obtained catalyst is NiMn 0.2 PMo 11 VO 40 / Al-ITQ-44. Example 5
[0085] Referring to Example 1, the difference from Example 1 is that step S2 is: 0.887 g MoO3 and 0.051 g V2O5 are added to 100 mL deionized water, heated to 90°C and stirred for 30 min to obtain a mixed solution; 4 g ammonium type Al-ITQ-44 is added to the mixed solution, stirred at 90°C for 15 min, 0.055 g phosphoric acid is added dropwise, and refluxed at 90°C for 4 h to obtain a suspension; 20 mL of a water mixture containing 0.09 g copper acetate monohydrate and 0.291 g lanthanum nitrate hexahydrate is added dropwise to the suspension, stirred at 70°C for 3 h, filtered, and dried at 100°C for 12 h to obtain a catalyst powder.
[0086] The remaining technical features are the same as those of Example 1.
[0087] The composition of the catalyst obtained is Cu 0.8 La 1.2 PMo 11 VO 40 / Al-ITQ-44. Comparative Example 1
[0088] Referring to Example 1, the difference from Example 1 is that steps S2 and S3 are not included; that is, the in-situ synthesis of heteropolyacid and subsequent calcination are not performed.
[0089] The remaining technical features are the same as those of Example 1. Comparative Example 2
[0090] Referring to Example 1, the difference from Example 1 is that (3) in step S1 is not included; that is, Al-ITQ-44 is not subjected to ammonium modification treatment.
[0091] The remaining technical features are the same as those of Example 1. Comparative Example 3
[0092] Referring to Example 1, the difference from Example 1 is that step S2 is: 0.887 g MoO3 and 0.051 g V2O5 are placed in 100 mL deionized water, heated to 90°C and stirred for 30 min to obtain a mixed solution; 4 g ammonium Al-ITQ-44 is placed in the mixed solution, stirred at 90°C for 15 min, 0.055 g phosphoric acid is added dropwise, refluxed at 90°C and stirred for 7 h, filtered, and dried at 100°C for 12 h to obtain a catalyst powder. That is, no compound containing element A and no compound containing element B are added.
[0093] The remaining technical features are the same as those of Example 1.
[0094] Test 1
[0095] The catalysts obtained in Examples 1 to 5 and Comparative Examples 1 to 3 were evaluated for activity using a micro fixed bed reactor. The catalyst was crushed into 20-40 mesh particles, 10 mL of the catalyst was loaded into the reactor, and 5 mL of quartz sand was added to the top and bottom of the reactor. The reactor was heated at a space velocity of 1000 h / min. -1 Under the conditions of 240°C, a mixed gas containing 3.5% 2-ethylhexanal, 46.5% air, 25% nitrogen and 25% water vapor by volume was introduced for reaction. After 100 h of reaction, samples were taken and quantitative analysis was performed by gas chromatography using the internal standard method. The results are shown in Table 1.
[0096] Table 1 Evaluation results of the reaction performance of catalysts for the oxidation of 2-ethylhexanal to 2-ethylhexanic acid
[0097] Experiment number 2-Ethylhexanal conversion rate / % Selectivity of 2-ethylhexanoic acid / % Example 1 97.6 92.3 Example 2 98.2 90.9 Example 3 99.1 87.1 Example 4 98.5 89.4 Example 5 97.8 91.3 Comparative Example 1 64.2 57.8 Comparative Example 2 85.5 83.4 Comparative Example 3 95.5 76.4
[0098] As can be seen from Table 1, compared with Comparative Example 1, heteropoly acid was added in Example 1, and the 2-ethylhexanal conversion rate and isooctanoic acid selectivity of the obtained catalyst were significantly improved; compared with Comparative Example 2, the molecular sieve was modified in Example 1, and the 2-ethylhexanal conversion rate and isooctanoic acid selectivity of the obtained catalyst were significantly improved. Compared with Comparative Example 3, A and B elements were added in Example 1, and the 2-ethylhexanal conversion rate and isooctanoic acid selectivity of the obtained catalyst were better.
[0099] Test 2
[0100] The molecular sieve encapsulated heteropoly acid salt catalyst obtained in Example 1 was used to evaluate its catalytic performance for selective oxidation of other high-carbon aliphatic aldehydes to corresponding high-carbon fatty acids to investigate its scope of application, and the results are shown in Table 2. The preparation method of n-octanoic acid, n-nonanoic acid, and isononanoic acid refers to Test 1, and 2-ethylhexanal is replaced by the reactants in Table 2 in equal molar amounts.
[0101] Table 2 Oxidation performance of other high-carbon aliphatic aldehydes catalyzed by amination supported heteropolyacid catalysts
[0102] Reactants Conversion rate / % Selectivity / % Octanal 95.5 93.6 n-nonanal 97.2 88.3 Isononanal 96.7 85.9
[0103] As can be seen from Table 2, the catalyst of the present invention is suitable for catalyzing the oxidation of other high-carbon aliphatic aldehydes to high carbonic acid, with high conversion rate and selectivity.
[0104] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A molecular sieve encapsulated heteropoly acid salt composite catalyst, comprising a heteropoly acid and a carrier, characterized in that: The heteropoly acid has the following chemical expression: a B b PMo 12-n V n O 40 ; In the formula: A is at least one of Ni, Cu, Zn, and Fe; B is at least one of Co, Mn, La, Ce, Sb, and Sn; Wherein: a, b, n are molar coefficients, 0.05≤a≤5, 0.02≤b≤2, 0<n≤3; The carrier is Al-doped silicon germanium molecular sieve ITQ-44; The preparation method of the molecular sieve encapsulated heteropolyacid salt composite catalyst comprises the following steps: S1. Obtaining a carrier; the carrier is an Al-doped silicon germanium molecular sieve ITQ-44; the carrier is subjected to ion exchange modification using a modifier to obtain an ammonium type molecular sieve; S2. In situ synthesis of heteropoly acid: reacting a carrier, MoO3, V2O5, phosphoric acid, a compound containing element A and a compound containing element B, and drying to obtain a catalyst powder; S3. Calcination: Calcinate the catalyst powder to obtain a catalyst.
2. The molecular sieve encapsulated heteropoly acid salt composite catalyst according to claim 1, characterized in that: In the formula: 0.1≤a≤4, 0.05≤b≤1.8, 0.5≤n≤2.
5.
3. The molecular sieve encapsulated heteropoly acid salt composite catalyst according to claim 2, characterized in that: The heteropoly acid is at least one of the following chemical formulas: With 1.5 What 0.3 PMo 11 VO 40 ; In 2.5 Sb 0.5 PM 10 V2O 40 ; Feb 0.3 Co 1.5 PMo 11 VO 40 ; NiMn 0.2 PMo 11 VO 40 , With 0.8 to 1.2 PMo 11 VO 40 。 4. A method for preparing a molecular sieve encapsulated heteropolyacid salt composite catalyst as claimed in any one of claims 1 to 3, characterized in that: The steps include: S1. Obtaining a carrier; the carrier is an Al-doped silicon germanium molecular sieve ITQ-44; the carrier is subjected to ion exchange modification using a modifier to obtain an ammonium type molecular sieve; S2. In situ synthesis of heteropoly acid: reacting a carrier, MoO3, V2O5, phosphoric acid, a compound containing element A and a compound containing element B, and drying to obtain a catalyst powder; S3. Calcination: Calcinate the catalyst powder to obtain a catalyst.
5. The preparation method according to claim 4, characterized in that: In step S1: the preparation method of the carrier comprises: dissolving colloidal silica and GeO2 into an aqueous solution of benzyltriethylammonium hydroxide, adding Al(OH)3, NH4F and NH4Cl to react, and then calcining.
6. The preparation method according to claim 4, characterized in that: In step S1: the modifier is at least one of ammonium chloride, ammonium nitrate, ammonium acetate, ammonium sulfate, ammonium bisulfate, ammonium carbonate, ammonium bicarbonate, ammonium bromide, ammonium iodide, and ammonium fluoride.
7. Use of the molecular sieve encapsulated heteropolyacid salt composite catalyst as claimed in any one of claims 1 to 3 in catalyzing the oxidation of high-carbon aliphatic aldehydes to high carbonic acid.