A method for preparing samarium-iron alloy powder based on mixed molten salt
By performing mixed molten salt treatment and impurity removal processes under a reducing atmosphere, the problem of uniform mixing difficulties caused by raw material size differences was solved, stable Sm2Fe17 alloy powder preparation was achieved, and sub-micron particles with high stability and dispersion were obtained. .
Patent Information
- Application Number
- CN202410969409.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-19
AI Technical Summary
When preparing Sm2Fe17 magnetic powder by the reduction-diffusion method in the prior art, the size difference of the raw materials makes it difficult to mix uniformly, and the conditions for co-precipitation and hydrogen reduction are complex, making it difficult to control the stability and particle size of the samarium-iron alloy.
Using a preparation method based on mixed molten salt, the iron salt, samarium salt and flux are melted in a reducing atmosphere, and then the reducing agent is added for heat treatment, and impurities are removed through grinding, ultrasonic, and magnetic separation processes to control the relationship between the iron salt and the flux. The molar ratio of the samarium salt and the amount of flux ensure that the raw materials are evenly mixed and impurities are removed.
This method achieves the preparation of uniform and stable Sm2Fe17 alloy powder, avoids the generation of impurities and particle agglomeration, improves the stability and dispersion of the preparation, and obtains Sm2Fe17 alloy powder with submicron-level nearly spherical particles.
Smart Images

Figure CN118527669B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal magnetic materials, and in particular relates to a method for preparing samarium-iron alloy powder based on mixed molten salt. Background Art
[0002] Due to the rapid development of the electrical industry in recent years and the trend of miniaturization and integration of electronic devices, Nd2Fe 14 The widespread application of rare earth permanent magnet materials has led to the depletion of neodymium resources, and the price of rare earth metal neodymium and its compounds has increased year by year; while samarium resources are relatively abundant, and samarium-rich tailings are piled up in large quantities or even directly discharged, causing serious environmental pollution. 17 N3 compared to Nd2Fe 14 B has a higher Curie temperature, magnetocrystalline anisotropy field, better thermal stability, oxidation resistance and corrosion resistance. 17 In addition to its significant economic advantages, N3 permanent magnet materials can also promote the balanced utilization of my country's rare earth resources.
[0003] Sm2Fe 17 The preparation of N3 magnetic powder is usually divided into two steps: Sm2Fe 17 Preparation of master alloy powder and Sm2Fe2O3 obtained by gas-solid nitriding reaction 17 N3 magnetic powder, including Sm2Fe 17 The preparation of master alloy powder is the key to obtain high-performance magnetic powder. 17 The methods mainly include powder metallurgy, melt quenching, mechanical alloying, hydrogenation disproportionation, reduction diffusion, etc. Among them, the reduction diffusion method uses relatively low-priced samarium oxide as the samarium source to replace expensive and difficult-to-store metal samarium, and avoids alloy smelting, homogenization annealing and coarse crushing, etc., which greatly reduces the production cost.
[0004] However, in the prior art, the reduction diffusion method directly mechanically mixes samarium oxide powder, iron powder and a reducing agent. Since the sizes of the three raw materials are quite different, uniform mixing cannot be achieved, which is not conducive to the preparation of a uniform and stable samarium-iron alloy. In addition, the composite hydroxide generated by the co-precipitation of samarium salt and iron salt is thermally decomposed to obtain a mixture of samarium-iron oxides, which is then subjected to hydrogen reduction and reduction diffusion to obtain a samarium-iron alloy. Due to the complex co-precipitation and hydrogen reduction conditions, the samarium-iron molar ratio in the alloy and the stability of particle size control are poor. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a method for preparing samarium-iron alloy powder based on mixed molten salt. The preparation method comprises the following steps: melting iron salt, samarium salt and flux in a reducing atmosphere and then grinding them, then adding a reducing agent for heat treatment and using grinding, ultrasound and magnetic separation processes to remove impurities, thereby obtaining uniform and stable Sm2Fe 17 The alloy powder solves the problem that the prior art cannot evenly mix the raw materials, which is not conducive to preparing a uniform and stable samarium-iron alloy.
[0006] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing samarium-iron alloy powder based on mixed molten salt, characterized in that the preparation method comprises the following steps:
[0007] Step 1, mixed molten salt: iron salt, samarium salt and flux are placed in a crucible, and then the crucible is placed in a tube furnace for melting treatment under a reducing atmosphere to obtain a mixed molten salt; the melting treatment system is: heating to 780°C~900°C at a rate of 2°C / min~5°C / min and then keeping warm for 1h~3h;
[0008] Step 2: Reduction diffusion: Grind the mixed molten salt obtained in step 1 and mix it evenly with the reducing agent, put it into a crucible and place it in a tube furnace, and perform heat treatment under an inert gas atmosphere to form Sm2Fe 17 alloy;
[0009] Step 3: Remove impurities: Sm2Fe formed in step 2 17 The alloy was treated with ammonium chloride-methanol solution for multiple times to remove impurities, and Sm2Fe 17 Alloy powder; the impurity removal treatment is to form Sm2Fe 17 The alloy is sequentially subjected to grinding, ultrasonic and magnetic separation treatments.
[0010] The present invention sets the heating rate to 2°C / min-5°C / min. The lower heating rate can fully melt the raw materials and ensure uniform mixing of the raw materials. The temperature is set to 780°C-900°C and the insulation time is set to 1h-3h, so that the block raw materials obtained after treatment can have higher looseness, and it is avoided that the temperature of the melting treatment is too high and the insulation time is too long, which leads to too high adhesion of the materials. The loose block raw materials can be crushed by grinding with less force and mixed evenly with the reducing agent.
[0011] The present invention adopts ammonium chloride-methanol solution as a medium to react Sm2Fe 17 The alloy is treated to remove impurities to avoid Sm2Fe 17 The alloy contacts with oxygen or water to make Sm2Fe 17 The oxygen content of the alloy increases.
[0012] The above-mentioned method for preparing samarium-iron alloy powder based on mixed molten salt is characterized in that the molar ratio of iron salt to samarium salt in step one is 6.5~7.5:1.
[0013] The present invention can ensure that the molar ratio of iron salt to samarium salt is 6.5-7.5:1. 17 The alloy forms a stable phase and avoids the formation of impurity α-Fe or samarium-rich phase. When the molar ratio of iron salt to samarium salt is lower than 6.5:1, samarium hydrogen or samarium-rich phase is easily generated. When the molar ratio of iron salt to samarium salt is higher than 7.5:1, α-Fe phase is easily generated.
[0014] The above-mentioned method for preparing samarium-iron alloy powder based on mixed molten salt is characterized in that the mass of the flux in step one is 20% to 40% of the total mass of the mixed molten salt, and the flux is calcium chloride and potassium chloride.
[0015] The present invention can enhance the fluidity of the reducing agent in a high-temperature molten state by setting the mass of the flux to 20% to 40% of the mass of the mixed molten salt; when the mass percentage of the flux is lower than 20%, the effect of enhancing the fluidity is not significant; when the mass percentage of the flux is higher than 40%, the diffusion of the Sm element and the Fe element in the reduction diffusion process will be hindered, which is not conducive to the Sm2Fe 17 The alloy is phase-stable.
[0016] The above-mentioned method for preparing samarium-iron alloy powder based on mixed molten salt is characterized in that the crucibles in step one and step two are both stainless steel crucibles with crucible covers.
[0017] The present invention can prevent the material from reacting with the inner wall of the crucible and affecting the preparation process by selecting a crucible made of stainless steel.
[0018] The above-mentioned method for preparing samarium-iron alloy powder based on mixed molten salt is characterized in that the reducing atmosphere in step one is a mixed gas composed of argon and hydrogen, the volume of hydrogen accounts for 5%~10% of the total volume of the mixed gas, and the flow rate of the mixed gas is 0.1L / min~0.3L / min.
[0019] The present invention introduces a mixed gas of argon and hydrogen during the melting process to provide a moderate reducing atmosphere to prevent the raw materials from being oxidized at high temperatures, and sets the volume proportion of hydrogen to 5% to 10% and the flow rate to 0.1L / min to 0.3L / min to avoid raw material loss caused by excessive proportion of hydrogen or excessive flow rate of the mixed gas.
[0020] The above-mentioned method for preparing samarium-iron alloy powder based on mixed molten salt is characterized in that the mass of the reducing agent in step 2 is 100% to 300% of the total mass of the mixed molten salt in step 1, and the reducing agent is calcium hydride.
[0021] The present invention can make the reduction diffusion reaction sufficient by setting the mass of the reducing agent to 100% to 300% of the total mass of the mixed molten salt; when the mass of the reducing agent is less than 100% of the total mass of the mixed molten salt, the reduction of the iron salt or samarium salt will be insufficient, affecting the Sm2Fe 17 The alloy is stable in phase; when the mass of the reducing agent is higher than 300% of the total mass of the mixed molten salt, it will cause Sm2Fe 17 The alloy product is stuck together and has too much residual calcium, which is not conducive to impurity removal.
[0022] The above-mentioned method for preparing samarium-iron alloy powder based on mixed molten salt is characterized in that the inert gas in step 2 is argon or nitrogen, and the flow rate of the inert gas is 0.1L / min~0.3L / min.
[0023] The present invention sets the inert gas flow rate to 0.1L / min-0.3L / min, which can not only provide the flowing inert atmosphere required for the reduction diffusion reaction, but also avoid the loss of raw materials caused by excessive gas flow rate.
[0024] The above-mentioned method for preparing samarium-iron alloy powder based on mixed molten salt is characterized in that the heat treatment system in step 2 is: heating to 850°C~1050°C at a rate of 2°C / min~5°C / min, and keeping warm for 1h~3h.
[0025] The present invention can ensure sufficient reduction diffusion reaction and Sm2Fe by setting the heating rate at 2°C / min~5°C / min and the temperature at 850°C~1050°C. 17 The alloy is phase-stabilized to avoid the formation of impurity phases or particle agglomeration caused by excessive sintering.
[0026] The above-mentioned method for preparing samarium-iron alloy powder based on mixed molten salt is characterized in that the molar concentration of the ammonium chloride-methanol solution in step three is 0.3 mol / L~0.6 mol / L.
[0027] Compared with the prior art, the present invention has the following advantages:
[0028] 1. The present invention controls the heating rate and temperature during the melting treatment of iron salt, samarium salt and flux, so that the block raw material obtained after the treatment has a higher looseness, avoids ball milling and crushing of the mixed molten salt, and mixes it evenly with the reducing agent through grinding treatment, which is conducive to the preparation of Sm2Fe 17alloy; by using ammonium chloride-methanol solution as the medium, and using grinding, ultrasonic and magnetic separation processes to 17 The alloy is subjected to multiple impurity removal treatments to effectively remove Sm2Fe 17 Impurities in alloy products, reducing Sm2Fe 17 Oxygen content of alloy powder.
[0029] 2. The present invention controls the molar ratio of iron salt and samarium salt to make Sm2Fe 17 The alloy is stable in phase and the formation of impurity α-Fe or samarium-rich phase is avoided. The raw materials are directly melted to avoid the loss of raw materials during the mixing process. At the same time, a stainless steel crucible with a crucible cover is used as a reaction container, which can effectively reduce the volatilization of Sm elements and ensure the prepared Sm2Fe 17 The molar ratio of samarium to iron in the alloy is stable.
[0030] 3. The present invention adjusts the amount of flux to enhance the fluidity of the reducing agent in a high-temperature molten state, so that the reduction diffusion reaction can be fully carried out. Then, by adjusting the amount of reducing agent and the reduction diffusion time, the particle agglomeration caused by excessive sintering of the samarium iron alloy can be avoided, and submicron Sm2Fe 17 alloy powder.
[0031] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The Sm2Fe obtained in Example 1 17 XRD patterns of alloy powders.
[0033] Figure 2 The Sm2Fe obtained in Example 1 17 SEM image of alloy powder. DETAILED DESCRIPTION
[0034] Example 1
[0035] The method for preparing samarium-iron alloy based on mixed molten salt in this embodiment comprises the following steps:
[0036] Step 1, mixed molten salt: 37.84g of ferric chloride hexahydrate, 5.13g of anhydrous samarium chloride, 9.21g of potassium chloride, and 9.21g of calcium chloride are placed in a stainless steel crucible with a lid and placed in a tube furnace, a mixed gas with a flow rate of 0.15L / min is introduced, and the temperature is increased to 800°C at a rate of 3°C / min and kept for 2h to obtain a mixed molten salt; the mixed gas is composed of 8% by volume of hydrogen and 92% by volume of argon;
[0037] Step 2: Reduction diffusion: Grind the mixed molten salt obtained in step 1 and mix it evenly with 122.78g of calcium hydride, put it into a stainless steel crucible with a lid, and place it in a tube furnace. Add argon gas at a flow rate of 0.15L / min, heat it to 950℃ at a rate of 3℃ / min and keep it for 1.5h to form Sm2Fe 17 alloy;
[0038] Step 3: Remove impurities: Sm2Fe formed in step 2 17 The alloy was treated with 0.45 mol / L ammonium chloride-methanol solution for three times to remove impurities, and then dried to obtain Sm2Fe 17 Alloy powder; the impurity removal treatment is for Sm2Fe 17 The alloy is then ground, ultrasonically and magnetically separated.
[0039] The Sm2Fe prepared in this embodiment 17 The alloy powder was subjected to XRD analysis, such as Figure 1 As shown, the Sm2Fe 17 The alloy powder phase composition is single phase Sm2Fe 17 ; Sm2Fe prepared in this embodiment 17 The alloy powder was photographed using a scanning electron microscope. Figure 2 As shown, the Sm2Fe 17 The alloy powder is submicron-sized nearly spherical particles with a smooth surface and good dispersibility.
[0040] Example 2
[0041] The method for preparing samarium-iron alloy based on mixed molten salt in this embodiment comprises the following steps:
[0042] Step 1, mixed molten salt: 35.14g of ferric chloride hexahydrate, 5.13g of anhydrous samarium chloride, 5.04g of potassium chloride, and 5.04g of calcium chloride are placed in a stainless steel crucible with a lid and placed in a tube furnace, a mixed gas with a flow rate of 0.3L / min is introduced, and the temperature is increased to 780°C at a rate of 2°C / min and kept for 3h to obtain a mixed molten salt; the mixed gas is composed of 5% by volume of hydrogen and 95% by volume of argon;
[0043] Step 2: Reduction diffusion: Grind the mixed molten salt obtained in step 1 and mix it evenly with 50.35g of calcium hydride, put it into a stainless steel crucible with a lid, and place it in a tube furnace. Add argon gas at a flow rate of 0.1L / min, heat it to 850℃ at a rate of 2℃ / min and keep it for 3h to form Sm2Fe 17 alloy;
[0044] Step 3: Remove impurities: Sm2Fe formed in step 2 17The alloy was treated with 0.3 mol / L ammonium chloride-methanol solution for four times to remove impurities, and then dried to obtain Sm2Fe 17 Alloy powder; the impurity removal treatment is for Sm2Fe 17 The alloy is then ground, ultrasonically and magnetically separated.
[0045] Example 3
[0046] The method for preparing samarium-iron alloy based on mixed molten salt in this embodiment comprises the following steps:
[0047] Step 1, mixed molten salt: 40.55g of ferric chloride hexahydrate, 5.13g of anhydrous samarium chloride, 15.23g of potassium chloride, and 15.23g of calcium chloride are placed in a stainless steel crucible with a lid and placed in a tube furnace, a mixed gas with a flow rate of 0.1L / min is introduced, and the temperature is increased to 900°C at a rate of 5°C / min and kept for 1h to obtain a mixed molten salt; the mixed gas is composed of 10% by volume of hydrogen and 90% by volume of argon;
[0048] Step 2: Reduction diffusion: Grind the mixed molten salt obtained in step 1 and mix it evenly with 228.42g of calcium hydride, put it into a stainless steel crucible with a lid, and place it in a tube furnace. A nitrogen gas with a flow rate of 0.3L / min is introduced, and the temperature is raised to 1050℃ at a rate of 5℃ / min and kept for 1h to form Sm2Fe 17 alloy;
[0049] Step 3: Remove impurities: Sm2Fe formed in step 2 17 The alloy was treated with 0.6 mol / L ammonium chloride-methanol solution for 5 times to remove impurities, and then dried to obtain Sm2Fe 17 Alloy powder; the impurity removal treatment is for Sm2Fe 17 The alloy is then ground, ultrasonically and magnetically separated.
[0050] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing samarium-iron alloy powder based on mixed molten salt, characterized in that: The preparation method comprises the following steps: Step 1, mixed molten salt: iron salt, samarium salt and flux are placed in a crucible, and then the crucible is placed in a tube furnace, and a melting treatment is performed under a reducing atmosphere to obtain a mixed molten salt; the melting treatment system is: heating to 780°C~900°C at a rate of 2°C / min~5°C / min and then keeping warm for 1h~3h, the molar ratio of the iron salt to the samarium salt is 6.5~7.5:1, the mass of the flux is 20%~40% of the total mass of the mixed molten salt, and the flux is calcium chloride and potassium chloride; Step 2: Reduction diffusion: Grind the mixed molten salt obtained in step 1 and mix it evenly with the reducing agent, put it into a crucible and place it in a tube furnace, and perform heat treatment under an inert gas atmosphere to form Sm2Fe 17 alloy; the reducing agent is calcium hydride, and the heat treatment system is: heating to 850°C~1050°C at a rate of 2°C / min~5°C / min, and keeping warm for 1h~3h; Step 3: Remove impurities: Sm2Fe formed in step 2 17 The alloy was treated with ammonium chloride-methanol solution for multiple times to remove impurities, and then dried to obtain submicron-sized Sm2Fe 17 Alloy powder; the impurity removal treatment is to form Sm2Fe 17 The alloy is sequentially subjected to grinding, ultrasonic and magnetic separation treatments.
2. The method for preparing samarium-iron alloy powder based on mixed molten salt according to claim 1, characterized in that: The crucibles in step 1 and step 2 are both stainless steel crucibles with crucible covers.
3. The method for preparing samarium-iron alloy powder based on mixed molten salt according to claim 1, characterized in that: The reducing atmosphere in step 1 is a mixed gas composed of argon and hydrogen, the volume of hydrogen accounts for 5% to 10% of the total volume of the mixed gas, and the flow rate of the mixed gas is 0.1 L / min to 0.3 L / min.
4. The method for preparing samarium-iron alloy powder based on mixed molten salt according to claim 1, characterized in that: The mass of the reducing agent in step 2 is 100% to 300% of the total mass of the mixed molten salt in step 1.
5. The method for preparing samarium-iron alloy powder based on mixed molten salt according to claim 1, characterized in that: In step 2, the inert gas is argon or nitrogen, and the flow rate of the inert gas is 0.1 L / min~0.3 L / min.