Preparation method and application of cellulose nanofiber / alkaline lignin ultraviolet-resistant composite film
Through a composite film of cellulose nanofibers and alkaline lignin, combining 1-chloro-2,2,5,5-tetramethyl-4-imidazolinone and anhydrous ethanol, the food packaging film has been solved in light resistance and The problem of insufficient fresh-preservation ability has improved the mechanical properties and antibacterial properties of food packaging films, and significantly enhanced the fresh-preservation ability and safety of foods.
Patent Information
- Application Number
- CN202411008947.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-26
AI Technical Summary
The existing food packaging films have shortcomings in light resistance and fresh preservation capabilities, which are difficult to meet the needs of food transportation, and do not have good mechanical properties and antibacterial properties.
The composite membrane of cellulose nanofibers and alkaline lignin is used to enhance the composite membrane by adding alkaline lignin and green antibacterial agent 1-chloro-2,2,5,5-tetramethyl-4-imidazolinone. Tensile strength and antibacterial properties, and improve drying rate and stability through anhydrous ethanol to form a composite film that is resistant to UV.
It improves the mechanical properties and antibacterial properties of cellulose nanofiber membranes, has good hygroscopicity and ultraviolet shielding properties, and can maintain the chlorine content after ultraviolet irradiation, significantly enhancing the freshness and safety of food.
Smart Images

Figure CN118530488B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of a composite film, and in particular to a preparation method and application of a cellulose nanofiber / alkaline lignin ultraviolet-resistant composite film. Background Art
[0002] During the storage, transportation and sales of food, it is inevitable that it will come into contact with bacteria and other harmful microorganisms, which will lead to the decomposition of nutrients and the spoilage of food. In addition, some harmful microorganisms will metabolize toxic or carcinogenic toxins such as aflatoxin, fumonisin, and T-2 mycin after decomposing food, which will have an adverse effect on human health if ingested. At present, the materials used for food packaging films commonly used in the market are mostly PE or PP materials, but they all have disadvantages such as poor light resistance and wear resistance, which are not conducive to food transportation as packaging films under certain conditions. The mechanical properties of pure cellulose nanofiber film are also difficult to meet the needs of food packaging. At the same time, these packaging films do not have the ability to prevent mold and preserve freshness for a long time. However, as a food transportation material, it must have certain mechanical properties, UV resistance, and preservation ability, so as to play a certain protective role when bumps occur during transportation and encounter strong light exposure. Summary of the invention
[0003] In view of the above technical requirements, the present invention provides a method for preparing a cellulose nanofiber / alkaline lignin UV-resistant composite film, the purpose of which is to improve the mechanical properties of the cellulose nanofiber film so that it meets the requirements of food packaging. The present invention also provides an application of the cellulose nanofiber / alkaline lignin UV-resistant composite film.
[0004] The technical scheme of the present invention is as follows: A method for preparing a cellulose nanofiber / alkaline lignin UV-resistant composite film, comprising the following steps: stirring and defoaming a mixed solution of a cellulose nanofiber aqueous dispersion and an alkaline lignin aqueous solution, and then spreading the mixed solution on a mold and letting it stand to dry to obtain a cellulose nanofiber / alkaline lignin UV-resistant composite film, wherein the alkaline lignin in the mixed solution accounts for 2% to 8% of the total mass of the cellulose nanofibers and the alkaline lignin.
[0005] Furthermore, in the mixed solution, the alkaline lignin accounts for 5% of the total mass of the cellulose nanofibers and the alkaline lignin.
[0006] Furthermore, the mixed solution of the cellulose nanofiber aqueous dispersion and the alkaline lignin aqueous solution is stirred, and then 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone solution is added and mixed and stirred, and after defoaming, it is spread on a mold and left to dry to obtain a cellulose nanofiber / alkaline lignin UV-resistant composite film.
[0007] Furthermore, the solvent of the 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone solution is anhydrous ethanol. The anhydrous ethanol used is miscible with water, which improves the stability of the composite system, the dispersibility of the antibacterial agent, and the drying rate.
[0008] Furthermore, the mass ratio of anhydrous ethanol in the 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone solution to the total of the mixed solution and anhydrous ethanol is 5 wt% to 30 wt%.
[0009] Furthermore, the mass ratio of anhydrous ethanol in the 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone solution to the total of the mixed solution and anhydrous ethanol is 15 wt% to 30 wt%.
[0010] Furthermore, the concentration of 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone in the 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone solution is not less than 0.5 wt%.
[0011] Furthermore, the defoaming is carried out in an ultrasonic cleaning machine at an ultrasonic power of 120 W and an ultrasonic frequency of 40 KHz for 5 to 30 min.
[0012] Furthermore, the static drying is carried out at room temperature of 20 to 25°C.
[0013] Another technical solution of the present invention is the application of a cellulose nanofiber / alkaline lignin composite antibacterial film, wherein the cellulose nanofiber / alkaline lignin UV-resistant composite film obtained by the aforementioned preparation method of the cellulose nanofiber / alkaline lignin UV-resistant composite film is directly wrapped on the surface of food.
[0014] The advantages of the present invention compared with the prior art are:
[0015] The present invention adopts two natural polymer materials, cellulose nanofiber and alkaline lignin, to make a composite film. By adding a small amount of alkaline lignin, the tensile strength of the composite film is enhanced while maintaining a certain elongation at break. The composite film has certain safety, transparency and good hygroscopicity during use and can be used for food transportation packaging.
[0016] Furthermore, the green antibacterial agent N-halamine compound 1-chloro-2, 2, 5, 5-tetramethyl-4-imidazolidinone was introduced into the composite system of cellulose nanofibers and alkaline lignin. The composite film can inactivate all Staphylococcus aureus and Escherichia coli within a contact time of 30 minutes, showing excellent antibacterial properties. In the composite system of cellulose nanofibers and alkaline lignin, alkaline lignin has excellent ultraviolet shielding properties, so that the chlorine content retention rate of the composite film after 24 hours of ultraviolet irradiation is about 74%, which has outstanding stability and ultraviolet resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a graph showing the tensile strength test results of each cellulose nanofiber / alkaline lignin UV-resistant composite film of Example 1.
[0018] Figure 2 This is a graph showing the elongation at break test results of each cellulose nanofiber / alkaline lignin UV-resistant composite film of Example 1.
[0019] Figure 3 This is a graph showing the stability test results of the CNF / AL suspension mixed solution after adding different amounts of anhydrous ethanol in Example 1.
[0020] Figure 4 This is a test chart of the chlorine content of the cellulose nanofiber / alkaline lignin UV-resistant composite film obtained in Example 2.
[0021] Figure 5 This is a scanning electron microscope image of the cellulose nanofiber / alkaline lignin UV-resistant composite film obtained in Example 2.
[0022] Figure 6 This is a graph showing the antibacterial performance test results of the cellulose nanofiber / alkaline lignin UV-resistant composite film obtained in Example 3 against Staphylococcus aureus.
[0023] Figure 7 This is a graph showing the test results of the antibacterial performance of the cellulose nanofiber / alkaline lignin UV-resistant composite film obtained in Example 3 against Escherichia coli.
[0024] Figure 8 This is a graph showing the chlorine content of the cellulose nanofiber / alkaline lignin UV-resistant composite film obtained in Example 3 after being stored away from light.
[0025] Fig. 9 This is a graph showing the chlorine content of the cellulose nanofiber / alkaline lignin UV-resistant composite film obtained in Example 4 after being irradiated with a UV lamp.
[0026] Fig.10 This is a graph showing the freshness test results of Example 4. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with the embodiments, but are not intended to limit the present invention.
[0028] Cellulose nanofibers (SEUMCNF02, 3.6% aqueous dispersion, 1-5 um in length, 10-20 nm in diameter, Tianjin Wood Elf Biotechnology Co., Ltd.), alkaline lignin (L832292, Shanghai McLean Biochemical Technology Co., Ltd.).
[0029] Example 1
[0030] The method for preparing a cellulose nanofiber / alkaline lignin UV-resistant composite film comprises the following steps:
[0031] Cellulose nanofiber (CNF) and alkaline lignin (AL) were used to prepare cellulose nanofiber aqueous dispersion with a mass fraction of 2.6% and alkaline lignin aqueous solution, respectively, and mixed in different proportions (the mass ratio of alkaline lignin aqueous solution to the solution was 0%, 2%, 5%, 8%, 10%, and 12%, respectively). After magnetic stirring at room temperature for 2 h, the mixture was transferred to an ultrasonic oscillation bath and degassed at an ultrasonic power of 120 W and an ultrasonic frequency of 40 kHz for 30 min. The CNF / AL suspended mixed solution was evenly poured into a clean polytetrafluoroethylene mold and spread flat. After standing and drying (room temperature 20-25°C), a cellulose nanofiber / alkaline lignin UV-resistant composite film was obtained.
[0032] The mechanical properties of each cellulose nanofiber / alkaline lignin UV-resistant composite film obtained in this example were tested to determine the tensile strength and elongation at break.
[0033] The tensile strength (σ) and elongation at break (δ) were tested using an electronic tensile tester. Before the experiment, the thickness of the film was measured at 5 randomly selected points on each sample using a digital micrometer and the average value was taken. The experimental sample was cut into a rectangular film (20 mm × 50 mm), stretched at a speed of 20 mm / min, tested three times, and the average value was taken. The calculation method of tensile strength (σ) and elongation at break (δ) is as follows:
[0034] ,
[0035] ,
[0036] Among them: F b It is the maximum force that the sample bears when it is broken, N (Newton); S o is the cross-sectional area of the specimen (mm 2 ); is the elongated length (mm); L0 is the original length (mm).
[0037] Test results such as Figure 1 and Figure 2 As shown in the figure, the tensile strength of the cellulose nanofiber / alkaline lignin UV-resistant composite film is greater than that of the pure cellulose nanofiber film (22 MPa), indicating that the addition of an appropriate amount of alkaline cellulose can improve the toughness of the cellulose nanofibers. When the alkaline cellulose addition amount is 5 wt%, the cellulose nanofiber / alkaline lignin UV-resistant composite film has the largest tensile strength and the highest elongation at break. Excessive addition of alkaline cellulose may affect the arrangement of the cellulose nanofiber macromolecular chains, thereby reducing its mechanical properties.
[0038] The stability of the CNF / AL suspension mixed solution was tested. Different amounts of anhydrous ethanol were added to the CNF / AL suspension mixed solution (the alkaline lignin aqueous solution accounted for 5% of the solution mass ratio) to investigate the effect of the amount of ethanol added on the storage state of the CNF / AL mixed solution. The mass ratio of the amount of anhydrous ethanol added to the total mass of the CNF / AL suspension mixed solution and anhydrous ethanol was 0, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, and 30 wt%. The results are shown in Figure 2. Figure 3 As shown in the figure, after 30 days of static storage, the appearance of the dispersion did not change significantly, the dispersion was good, and no precipitation was generated. Considering the solubility of the subsequent antibacterial agent in ethanol and the uniform dispersion in the film, an addition amount of more than 15 wt% is more appropriate, and 15 wt% of anhydrous ethanol is used in the subsequent examples.
[0039] Example 2
[0040] Cellulose nanofiber (CNF) and alkaline lignin (AL) were used to prepare 1.3% cellulose nanofiber aqueous dispersion and alkaline lignin aqueous solution, respectively, wherein the alkaline lignin aqueous solution accounted for 5% of the solution mass ratio, and after magnetic stirring for 2 h at room temperature, 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone (MC) solution with anhydrous ethanol as solvent was added, wherein the concentrations of 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone in the 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone solution were 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.5 wt%, 0.7 wt%, and 1.0 wt%, respectively. The amount of anhydrous ethanol was calculated according to the mass ratio of anhydrous ethanol added to the total mass of CNF / AL suspension mixed solution and anhydrous ethanol, which was 15wt%. 1-Chloro-2,2,5,5-tetramethyl-4-imidazolidinone solution was added to the CNF / AL suspension mixed solution and placed on a magnetic stirrer for 2 h to mix evenly. The mixture was then transferred to an ultrasonic oscillation bath and degassed for 30 min at an ultrasonic power of 120 W and an ultrasonic frequency of 40 kHz. The mixed solution was evenly poured into a clean polytetrafluoroethylene mold and spread flat. After standing and drying (room temperature 20-25°C), a cellulose nanofiber / alkaline lignin UV-resistant composite film was obtained.
[0041] The cellulose nanofiber / alkaline lignin UV-resistant composite films obtained in this example were tested for effective chlorine content using the following test method:
[0042] Cut the circular sample film (d = 3.5 cm) into pieces, place it in 10 mL of deionized water, add 0.5 g of potassium iodide powder, stir with a magnetic stirrer for about 30 min until the aqueous solution turns yellow, then add 5 mL of a low starch content aqueous solution with a total mass fraction of about 1%, stir continuously until the aqueous solution turns purple-black, and titrate with 0.001 N sodium thiosulfate aqueous solution until the purple-black gradually becomes transparent. Each sample is measured three times and the average value is taken. The formula for calculating the oxidized chlorine content is as follows:
[0043] ,
[0044] in: (atoms / cm²) is the chlorine content on the film surface, N is the sodium thiosulfate concentration (equiv / L), V is the volume of the sodium thiosulfate solution consumed (L), and S is the area of the film sample (cm²).
[0045] Test results such as Figure 4 As shown in Figure 2, the test results show that when the concentration of 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone solution is 0.5 wt%, the chlorine content of the cellulose nanofiber / alkaline lignin UV-resistant composite film is 9.19×1017 atoms / cm 2 According to literature reports, the chlorine content of composite membranes containing N-halamine antimicrobial agents is higher than 6.28×10 17 atoms / cm 2 When the logarithm value was about 6.07, Escherichia coli and Staphylococcus aureus were completely inactivated within 5 minutes.
[0046] The cellulose nanofiber / alkaline lignin UV-resistant composite film sample obtained when the concentration of 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone in Example 2 was 0.7 wt % was tested by scanning electron microscopy. Figure 5 As shown, there is no obvious change in the surface texture of the composite film, and the fibers are relatively clear, indicating that the cellulose nanofibers have good compatibility with alkaline lignin. At the same time, 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone is successfully doped into the CNF / AL system.
[0047] Example 3
[0048] Cellulose nanofibers (CNF) and alkaline lignin (AL) were used to prepare cellulose nanofiber aqueous dispersions with a mass fraction of 2.6% and alkaline lignin aqueous solutions, respectively, wherein the alkaline lignin aqueous solution accounted for 5% of the solution mass ratio, and after magnetic stirring for 2 h at room temperature, 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone (MC) solution with anhydrous ethanol as solvent was added, wherein the concentration of 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone in the 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone solution was 0.5 wt%. The amount of anhydrous ethanol was calculated according to the mass ratio of anhydrous ethanol added to the total mass of CNF / AL suspension mixed solution and anhydrous ethanol, which was 15 wt%. 1-Chloro-2,2,5,5-tetramethyl-4-imidazolidinone solution was added to the CNF / AL suspension mixed solution and placed on a magnetic stirrer for 2 h to mix evenly. The mixture was then transferred to an ultrasonic oscillation bath and degassed for 30 min at an ultrasonic power of 120 W and an ultrasonic frequency of 40 kHz. The mixed solution was evenly poured into a clean polytetrafluoroethylene mold and spread flat. After standing and drying (room temperature 20-25°C), a cellulose nanofiber / alkaline lignin UV-resistant composite film was obtained.
[0049] The antibacterial performance of this embodiment was tested by using Staphylococcus aureus (ATCC6538) and Escherichia coli (ATCC43895) as experimental strains. 25 uL of bacterial suspension was dropped onto a 2.54 cm 2At the center of the composite film, another film was covered on top of the suspension to ensure full contact. After the contact time reached 5, 10, and 30 min, the sample was transferred to a centrifuge tube containing sterile sodium thiosulfate / PBS solution and vortexed for 2 min to quench the oxidized chlorine residue. On this basis, the quenched solution was diluted in different multiples (10-1000 times) and dropped into the pre-prepared agar plate. After the plate was incubated at 37°C for 24 h, the number of colonies on the plate was recorded, and the inhibition rate was calculated according to the following formula:
[0050] ,
[0051] Where: R represents the bactericidal activity value, A is the average colony survival number of the control sample after 0 hours of inoculation with bacteria, B is the average colony survival number of the control sample after 24 hours of inoculation, and C is the average colony survival number of the antibacterial sample after 24 hours of inoculation.
[0052] Pure cellulose nanofiber film (CNF) and cellulose nanofiber / alkaline lignin UV-resistant composite film (alkaline cellulose addition amount is 5 wt %) (CNF / AL) obtained in Example 1 were used for comparison. This example is CNF / AL-MC. The results are as follows Figure 6 and Figure 7 As shown in the figure, pure CNF and CNF / AL showed a certain inhibitory effect on the two strains. This is because CNF / AL has strong water absorption, which can make bacteria adhere to the membrane surface. After adding MC, the prepared CNF / AL-MC membrane can inactivate 0.85 log and 1.28 log of Staphylococcus aureus and Escherichia coli within 5 minutes. With the increase of contact time, the reduction of bacteria also increases. When the contact time is 30 minutes, all inoculated bacteria are completely killed. The possible reason is that MC in CNF / AL-MC membrane can transfer the effective chlorine to the bacterial surface, thereby inactivating the microorganisms.
[0053] The cellulose nanofiber / alkaline lignin UV-resistant composite film obtained in Example 3 was stored for a period of time under light-proof conditions to test the change in chlorine content. The results are as follows: Figure 8 After one week of storage, the chlorine content increased from 9.38×10 17 atoms / cm 2 Down to 9.10×10 17 atoms / cm 2 This may be because the N-Cl bond on the film surface can react with microorganisms and moisture in the air to form NH bonds, resulting in a reduction in the active chlorine content on the film surface. As the storage time increases, the chlorine content decreases slowly and fluctuates slightly, indicating that the antibacterial performance is relatively stable during light-proof storage.
[0054] Example 4
[0055] Cellulose nanofibers (CNF) and alkaline lignin (AL) were used to prepare cellulose nanofiber aqueous dispersions with a mass fraction of 2.6% and alkaline lignin aqueous solutions, respectively, wherein the alkaline lignin aqueous solution accounted for 5% of the solution mass ratio, and after magnetic stirring for 2 h at room temperature, 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone (MC) solution with anhydrous ethanol as solvent was added, wherein the concentration of 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone in the 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone solution was 1.0 wt%. The amount of anhydrous ethanol was calculated according to the mass ratio of anhydrous ethanol added to the total mass of CNF / AL suspension mixed solution and anhydrous ethanol, which was 15 wt%. 1-Chloro-2,2,5,5-tetramethyl-4-imidazolidinone solution was added to the CNF / AL suspension mixed solution and placed on a magnetic stirrer for 2 h to mix evenly. The mixture was then transferred to an ultrasonic oscillation bath and degassed for 30 min at an ultrasonic power of 120 W and an ultrasonic frequency of 40 kHz. The mixed solution was evenly poured into a clean polytetrafluoroethylene mold and spread flat. After standing and drying (room temperature 20-25°C), a cellulose nanofiber / alkaline lignin UV-resistant composite film was obtained.
[0056] Ultraviolet light photolysis can cause permanent loss (decomposition of macromolecular structure) and temporary loss (cleavage of N-Cl) of N-chloramine sites. The cellulose nanofiber / alkaline lignin UV-resistant composite film obtained in Example 4 was placed in a UV light box for different periods of irradiation to test the change in chlorine content. Fig. 9 As shown in the figure, chlorine oxide only lost 2.90% in 1 h, indicating that short-term ultraviolet irradiation has little effect on the chlorine content of the film; as the irradiation time gradually increases (2-4 h), the loss also gradually increases, mainly because the increase in irradiation time causes the decomposition and cracking of the N-Cl chemical bond, but due to the excellent ultraviolet shielding performance of AL, the downward trend of chlorine content gradually slows down after 4 h of irradiation. Until the irradiation time is 24 h, the chlorine content is still maintained at 73.84%. The cellulose nanofiber / alkaline lignin ultraviolet-resistant composite film of the present invention has excellent ultraviolet resistance.
[0057] The cellulose nanofiber / alkaline lignin UV-resistant composite film (CNF / AL-MC) of this example was used as a comparison, and the pure cellulose nanofiber film (CNF) and the cellulose nanofiber / alkaline lignin UV-resistant composite film (alkaline cellulose addition amount is 5 wt %) (CNF / AL) obtained in Example 1 were used as a control group for the freshness preservation test. Each sample was wrapped with steamed buns and stored at 30°C and RH 50% for 6 days. The appearance was observed. The results are as follows: Fig.10The results show that the film without MC addition is prone to mold growth, while no mold growth was observed on the steamed bread packaged with the composite film of this example. The enhanced steamed bread preservation effect is attributed to the broad-spectrum antibacterial properties of MC, and the composite film containing MC has been shown to effectively inhibit bacteria, yeast and mold. Compared with CNF / AL, the composite film containing MC is more suitable for packaging steamed bread samples.
Claims
1. A method for preparing a cellulose nanofiber / alkaline lignin UV-resistant composite film, characterized in that: The following steps are involved: A mixed solution of a cellulose nanofiber aqueous dispersion and an alkaline lignin aqueous solution is stirred and defoamed, and then spread on a mold and left to dry to obtain a cellulose nanofiber / alkaline lignin UV-resistant composite film, wherein the alkaline lignin in the mixed solution accounts for 5% of the total mass of the cellulose nanofibers and the alkaline lignin.
2. The method for preparing the cellulose nanofiber / alkaline lignin UV-resistant composite film according to claim 1, characterized in that: The mixed solution of the cellulose nanofiber aqueous dispersion and the alkaline lignin aqueous solution is stirred, 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone solution is added, and the mixture is stirred and mixed again. After defoaming, the mixture is spread on a mold and left to dry to obtain a cellulose nanofiber / alkaline lignin UV-resistant composite film.
3. The method for preparing the cellulose nanofiber / alkaline lignin UV-resistant composite film according to claim 2, characterized in that: The solvent of the 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone solution is anhydrous ethanol.
4. The method for preparing the cellulose nanofiber / alkaline lignin UV-resistant composite film according to claim 3, characterized in that: The mass ratio of the anhydrous ethanol in the 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone solution to the total of the mixed solution and the anhydrous ethanol is 5 wt % to 30 wt %.
5. The method for preparing the cellulose nanofiber / alkaline lignin UV-resistant composite film according to claim 3, characterized in that: The mass ratio of the anhydrous ethanol in the 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone solution to the total of the mixed solution and the anhydrous ethanol is 15 wt % to 30 wt %.
6. The method for preparing the cellulose nanofiber / alkaline lignin UV-resistant composite film according to claim 5, characterized in that: The concentration of 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone in the 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone solution is not less than 0.5 wt %.
7. The method for preparing the cellulose nanofiber / alkaline lignin UV-resistant composite film according to claim 1 or 2, characterized in that: The defoaming is carried out in an ultrasonic cleaning machine at an ultrasonic power of 120 W and an ultrasonic frequency of 40 KHz for 5 to 30 minutes.
8. The method for preparing the cellulose nanofiber / alkaline lignin UV-resistant composite film according to claim 1 or 2, characterized in that: The static drying is carried out at room temperature of 20 to 25°C.
9. Application of a cellulose nanofiber / alkaline lignin UV-resistant composite film, characterized in that: The cellulose nanofiber / alkaline lignin ultraviolet resistant composite film obtained by the preparation method of the cellulose nanofiber / alkaline lignin ultraviolet resistant composite film according to any one of claims 2 to 6 is directly wrapped on the surface of food.