A viscosity reducer for drilling fluid suitable for deep wells and preparation method thereof

Through the compounding of amphoteric viscosity-reducing polymers and bifunctional carbon nanotubes, the problem of increased viscosity of drilling fluids in high-temperature and high-salt environments is solved, and the excellent viscosity-reducing performance, temperature resistance, and salt resistance of the drilling fluid are achieved. It is suitable for Drilling in deep wells.

CN118530704BActive Publication Date: 2024-10-25SHENGLI OILFIELD GUBANG PETROLEUM EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411008339.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-25
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

Heavy oil viscosity reducers in existing drilling fluids fail in high-temperature and high-salt environments, resulting in increased viscosity and affecting the fluidity of drilling fluids and the protection of oil and gas layers.

Method used

It uses a compound of amphoteric viscosity-reducing polymer and bifunctional carbon nanotubes, and modifies the carbon nanotubes with highly active amphoteric silane coupling agent and hydrophobic phenyl silane coupling agent to form a product with excellent temperature resistance and salt resistance. Performance viscosity reducer.

Benefits of technology

It has significantly improved the viscosity reduction performance, temperature resistance and salt resistance of the drilling fluid. It can maintain good viscosity reduction rate and anti-filtration performance at a high temperature of 260°C, and is suitable for the complex environment of deep wells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The present invention relates to the technical field of drilling fluids, and in particular to a viscosity reducer for drilling fluids suitable for deep wells and a preparation method thereof. The viscosity reducer for drilling fluids suitable for deep wells is obtained by mixing an amphoteric viscosity reducing polymer and a bifunctional carbon nanotube; the amphoteric viscosity reducing polymer is obtained by polymerization reaction of monomer raw materials, and the monomer raw materials include acrylamide, acrylic acid, sodium p-styrene sulfonate and methacryloylethyl sulfobetaine; the bifunctional carbon nanotubes are obtained by modifying carbon nanotubes with an amphoteric silane coupling agent containing imidazolium cations and a hydrophobic phenyl silane coupling agent. The viscosity reducer for drilling fluid provided by the present invention has excellent temperature resistance and salt resistance, and is suitable for the increasingly complex mining environment in deep wells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of drilling fluid, and in particular to a viscosity reducer for drilling fluid suitable for deep wells and a preparation method thereof. Background Art

[0002] Viscosity reducers are chemical agents that can reduce the viscosity and shear force of drilling fluids and adjust the rheological properties of drilling fluids. As an important type of chemical additive in the oil drilling process, it plays an important role in adjusting the rheological properties of drilling fluids, maintaining the performance of drilling fluids, and protecting oil and gas layers. Although the solid phase control system can remove harmful solid phases in the drilling fluid, effectively adjust the rheological properties of the drilling fluid, and reduce the amount of viscosity reducers, the solid control equipment on site is not ideal, and the role of viscosity reducers is very important.

[0003] With the vertical development of oil exploration, the number of deep wells and ultra-deep wells with temperatures exceeding 200°C is increasing, and the drilling conditions of drilling tools in the formation are becoming more and more complex. During the drilling process, as the drilling depth increases, the temperature in the wellbore increases significantly, and the problem of drilling fluid thickening becomes more and more serious. Viscosity reducers play a very important role in regulating the rheology of drilling fluids. Among the many types of drilling fluid additives, polymer additives have a faster development speed and high adjustability. People can synthesize high-temperature resistant viscosity reducers that meet environmental requirements and adapt to complex wells by selecting monomers with characteristic functional groups.

[0004] Patent technology document CN202211409571.1 discloses a heavy oil viscosity reducer composition and preparation method. The heavy oil polymer viscosity reducer is composed of a low molecular weight amphiphilic polymer and a nano hydrophobic modified material. The preparation method of the low molecular weight amphiphilic polymer is to carry out polymerization reaction under deoxygenation conditions with acrylamide hydrophilic monomers, sulfonic acid group-containing temperature-resistant monomers, hydrophobic monomers containing rigid structures, initiators and inhibitors, and the reaction product is obtained after washing, drying and crushing; the nano hydrophobic modified material is a nano material that is hydrophobically modified by a coupling agent, and then an amphiphilic surfactant is added to further improve the dispersibility. The heavy oil viscosity reducer composition formed by the invention can be used for reducing the viscosity of pipeline heavy oil. However, the heavy oil polymer viscosity reducer in the invention contains anionic groups. When the salt content in the heavy oil is too high, the hydration ability of the polymer will be weakened, the molecular chain will curl, and hydrophobic association will occur, and even the clay end faces will be agglomerated to form a network structure, which will increase the viscosity. Summary of the invention

[0005] In view of this, the purpose of the present invention is to propose a viscosity reducer for drilling fluid suitable for deep wells and a preparation method thereof, so as to provide a viscosity reducer for drilling fluid with excellent temperature resistance and salt resistance, so as to be suitable for the increasingly complex mining environment in deep wells.

[0006] Based on the above purpose, the present invention provides a viscosity reducer for drilling fluid suitable for deep wells, characterized in that it is obtained by mixing an amphoteric viscosity reducing polymer and a bifunctional carbon nanotube.

[0007] Furthermore, the weight ratio of the amphoteric viscosity-reducing polymer to the bifunctional carbon nanotube is 20-30:0.5-1.

[0008] Furthermore, the amphoteric viscosity-reducing polymer is prepared by polymerization reaction of monomer raw materials, and the monomer raw materials include acrylamide, acrylic acid, sodium p-styrene sulfonate and methacryloylethyl sulfobetaine.

[0009] Preferably, the weight ratio of acrylamide, acrylic acid, sodium p-styrene sulfonate and methacryloylethyl sulfobetaine is 10-15:2-3:15-25:3-5.

[0010] More preferably, the weight ratio of acrylamide, acrylic acid, sodium p-styrene sulfonate and methacryloylethyl sulfobetaine is 12:2.4:20:4.

[0011] Furthermore, the preparation method of the bifunctional carbon nanotubes is as follows: dispersing carbon nanotubes in anhydrous ethanol, then adjusting the pH to 9-10 with ammonia water, adding amphoteric silane coupling agent and phenyltriethoxysilane, heating to 50-60°C, stirring for 12-14h, centrifuging, washing, and obtaining bifunctional carbon nanotubes.

[0012] Furthermore, the weight ratio of the carbon nanotubes, anhydrous ethanol, amphoteric silane coupling agent and phenyltriethoxysilane is 1:20-30:0.3-0.5:0.1-0.2.

[0013] Preferably, the carbon nanotubes are double-walled carbon nanotubes with a diameter of 20-40 nm and a length of 1-2 μm.

[0014] Preferably, the mass fraction of the ammonia water is 28%.

[0015] Furthermore, the preparation method of the amphoteric silane coupling agent is as follows: triethoxy-3-(2-imidazoline-1-yl)propylsilane and 1,3-propane sultone are added to anhydrous acetone, refluxed for 16-18 hours under a nitrogen atmosphere, and rotary evaporated after the reaction to obtain the amphoteric silane coupling agent.

[0016] Furthermore, the weight ratio of triethoxy-3-(2-imidazoline-1-yl)propylsilane, 1,3-propane sultone and anhydrous acetone is 1:0.48-0.55:20-30.

[0017] Preferably, the specific preparation method of the amphoteric viscosity-reducing polymer is as follows: under a nitrogen atmosphere, the monomer raw material is added to ethyl acetate, the temperature is raised to 60-65°C, and stirred for 20-30 minutes, then an initiator is added, the temperature is raised to 80-90°C, and the reaction is stirred for 8-10 hours, then an inhibitor is added, stirred for 10-20 minutes, rotary evaporated, washed, and dried to obtain an amphoteric viscosity-reducing polymer.

[0018] Preferably, the weight ratio of the monomer raw material, ethyl acetate, initiator and inhibitor is 30-48:150-250:1-2:1.2-1.8.

[0019] Preferably, the initiator is azobisisobutyronitrile.

[0020] Preferably, the polymerization inhibitor is p-hydroxyanisole.

[0021] Furthermore, the temperature resistance of the viscosity reducer for deep well drilling fluid can reach 260°C.

[0022] Furthermore, the present invention also provides a method for preparing a viscosity reducer for deep well drilling fluid, comprising the following steps: uniformly mixing an amphoteric viscosity reducing polymer and a bifunctional carbon nanotube to obtain a viscosity reducer for deep well drilling fluid.

[0023] Beneficial effects of the present invention:

[0024] The present invention adopts bifunctional carbon nanotubes and amphoteric viscosity reducing polymers to prepare a viscosity reducing agent for drilling fluid suitable for deep wells, wherein the bifunctional carbon nanotubes are obtained by modifying carbon nanotubes with a highly active amphoteric silane coupling agent containing imidazolium cations and a hydrophobic phenyl silane coupling agent, and can be effectively compounded with the amphoteric viscosity reducing polymer to synergistically improve the viscosity reducing performance and the temperature resistance and salt resistance.

[0025] The invention adopts methacryloylethyl sulfobetaine and sodium p-styrene sulfonate with certain steric hindrance to synthesize an amphoteric viscosity-reducing polymer. The sulfobetaine group can form an ionic bond with an amphoteric silane coupling agent on the surface of a carbon nanotube, thereby improving the dispersion of the carbon nanotube. In addition, the sodium p-styrene sulfonate has certain steric hindrance with the phenyl group and the imidazole group on the carbon nanotube, which is helpful to adjust the spatial structure. The hydrophobicity of the phenyl group is helpful to release free water in the clay, thereby further improving the viscosity-reducing performance and the temperature resistance and salt resistance. DETAILED DESCRIPTION

[0026] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0027] The carbon nanotubes in the specific implementation manner of the present invention were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. with the item number C121257.

[0028] Example 1

[0029] (1) Add 1 g of triethoxy-3-(2-imidazoline-1-yl)propylsilane and 0.48 g of 1,3-propanesultone to 20 g of anhydrous acetone, and reflux for 16 h under a nitrogen atmosphere. After the reaction is completed, rotary evaporation is performed to obtain an amphoteric silane coupling agent;

[0030] (2) Disperse 1 g of carbon nanotubes in 20 g of anhydrous ethanol, adjust the pH to 9.2 with 28% ammonia water, add 0.3 g of amphoteric silane coupling agent and 0.1 g of phenyltriethoxysilane, heat to 50 °C, stir for 12 h, centrifuge, and wash to obtain bifunctional carbon nanotubes;

[0031] (3) Under nitrogen atmosphere, add 10 g acrylamide, 2 g acrylic acid, 15 g sodium p-styrene sulfonate and 3 g methacryloylethyl sulfobetaine to 150 g ethyl acetate, heat to 60°C, stir for 20 min, then add 1-2 g azobisisobutyronitrile, heat to 80°C, stir for 8 h, then add 1.2 g p-hydroxyanisole, stir for 10 min, rotary evaporate, wash, and dry to obtain an amphoteric viscosity-reducing polymer;

[0032] (4) 20 g of the amphoteric viscosity reducing polymer and 0.5 g of the bifunctional carbon nanotubes are uniformly mixed to obtain a viscosity reducing agent for drilling fluid suitable for deep wells.

[0033] Example 2

[0034] (1) Add 1 g of triethoxy-3-(2-imidazoline-1-yl)propylsilane and 0.55 g of 1,3-propanesultone to 30 g of anhydrous acetone, and reflux for 18 h under a nitrogen atmosphere. After the reaction is completed, rotary evaporation is performed to obtain an amphoteric silane coupling agent;

[0035] (2) Disperse 1 g of carbon nanotubes in 25 g of anhydrous ethanol, adjust the pH to 9.6 with 28% ammonia water, add 0.4 g of amphoteric silane coupling agent and 0.15 g of phenyltriethoxysilane, heat to 55 °C, stir for 12 h, centrifuge, and wash to obtain bifunctional carbon nanotubes;

[0036] (3) Under nitrogen atmosphere, add 12 g acrylamide, 2.4 g acrylic acid, 20 g sodium p-styrene sulfonate and 4 g methacryloylethyl sulfobetaine to 200 g ethyl acetate, heat to 60°C, stir for 20 min, then add 1.5 g azobisisobutyronitrile, heat to 85°C, stir for 8 h, then add 1.5 g p-hydroxyanisole, stir for 10 min, rotary evaporate, wash, and dry to obtain an amphoteric viscosity-reducing polymer;

[0037] (4) 25 g of an amphoteric viscosity reducing polymer and 0.75 g of a bifunctional carbon nanotube are uniformly mixed to obtain a viscosity reducing agent for drilling fluid suitable for deep wells.

[0038] Example 3

[0039] (1) Add 1 g of triethoxy-3-(2-imidazoline-1-yl)propylsilane and 0.55 g of 1,3-propanesultone to 30 g of anhydrous acetone, and reflux for 18 h under a nitrogen atmosphere. After the reaction is completed, rotary evaporation is performed to obtain an amphoteric silane coupling agent;

[0040] (2) Disperse 1 g of carbon nanotubes in 30 g of anhydrous ethanol, then adjust the pH to 9.3 with 28% ammonia water, add 0.5 g of amphoteric silane coupling agent and 0.2 g of phenyltriethoxysilane, heat to 60 °C, stir for 14 h, centrifuge, and wash to obtain bifunctional carbon nanotubes;

[0041] (3) Under nitrogen atmosphere, 15 g acrylamide, 3 g acrylic acid, 25 g sodium p-styrene sulfonate and 3-5 g methacryloylethyl sulfobetaine were added to 250 g ethyl acetate, the temperature was raised to 65°C, and the mixture was stirred for 30 min. Then, 2 g azobisisobutyronitrile was added, the temperature was raised to 90°C, and the mixture was stirred for 10 h. Then, 1.8 g p-hydroxyanisole was added, the mixture was stirred for 20 min, and the mixture was rotary evaporated, washed, and dried to obtain an amphoteric viscosity-reducing polymer.

[0042] (4) 30 g of the amphoteric viscosity reducing polymer and 1 g of the bifunctional carbon nanotubes are uniformly mixed to obtain a viscosity reducing agent for drilling fluid suitable for deep wells.

[0043] Comparative Example 1:

[0044] The difference between Comparative Example 1 and Example 2 is that the amphoteric silane coupling agent in step (2) is replaced by phenyltriethoxysilane, and the remaining steps are the same as Example 2, which will not be described in detail here.

[0045] Comparative Example 2:

[0046] The difference between Comparative Example 2 and Example 2 is that the phenyltriethoxysilane in step (2) is replaced by an amphoteric silane coupling agent, and the remaining steps are the same as Example 2 and are not described in detail here.

[0047] Comparative Example 3:

[0048] (1) Under nitrogen atmosphere, 12 g acrylamide, 2.4 g acrylic acid, 20 g sodium p-styrene sulfonate and 4 g methacryloylethyl sulfobetaine were added to 200 g ethyl acetate, the temperature was raised to 60°C, and the mixture was stirred for 20 min. Then, 1.5 g azobisisobutyronitrile was added, the temperature was raised to 85°C, and the mixture was stirred for 8 h. Then, 1.5 g p-hydroxyanisole was added, the mixture was stirred for 10 min, and the mixture was rotary evaporated, washed, and dried to obtain an amphoteric viscosity-reducing polymer.

[0049] (2) 25 g of an amphoteric viscosity reducing polymer and 0.75 g of carbon nanotubes were uniformly mixed to obtain a viscosity reducing agent for drilling fluid.

[0050] Comparative Example 4:

[0051] (1) Under nitrogen atmosphere, 12 g acrylamide, 2.4 g acrylic acid, 20 g sodium p-styrene sulfonate and 4 g methacryloylethyl sulfobetaine were added to 200 g ethyl acetate, the temperature was raised to 60°C, and the mixture was stirred for 20 min. Then, 1.5 g azobisisobutyronitrile was added, the temperature was raised to 85°C, and the mixture was stirred for 8 h. Then, 1.5 g p-hydroxyanisole was added, the mixture was stirred for 10 min, and the mixture was rotary evaporated, washed, and dried to obtain an amphoteric viscosity-reducing polymer.

[0052] (2) Directly use amphoteric viscosity reducing polymers as viscosity reducing agents for drilling fluids.

[0053] Test example:

[0054] (1) Sample preparation:

[0055] Preparation of fresh water slurry: Add 400 mL of tap water into a cup, add 2 g of anhydrous sodium carbonate to fully dissolve, then slowly add 40 g of bentonite, stir at high speed for 2 hours, and then place it in a closed environment at 25°C to hydrate for later use;

[0056] Preparation of freshwater slurry with high salt content: add 400mL of tap water into a cup, add 2g of anhydrous sodium carbonate, 2g of sodium chloride and 4g of calcium chloride to fully dissolve, then slowly add 40g of bentonite, stir at high speed for 2h, and then let it stand in a closed environment at 25℃ for hydration, and set aside;

[0057] Preparation of drilling fluid samples: Take 400 mL of the two base slurries mentioned above, add 2 g of the viscosity reducer prepared in the embodiment and the comparative example to the two base slurries respectively, and stir for 20 minutes to obtain the corresponding drilling fluids.

[0058] (2) Performance testing:

[0059] Rheological parameters: measured in accordance with the industry standard SY / T5621-93 "Evaluation Procedure for Viscosity Reducers for Water-Based Drilling Fluids", the measuring temperature is 25°C, and the apparent viscosity and plastic viscosity of the drilling fluid are calculated. The test results are shown in Table 1;

[0060] Filtrate reduction: The filtrate reduction of the drilling fluid was measured using a drilling fluid loss meter. The measurement temperature was 25°C. The test results are shown in Table 1.

[0061] Viscosity reduction rate: The six-speed rotary viscometer was used to test the viscosity reduction rate of the drilling fluid and the drilling fluid after high-temperature tumbling and aging. The results are shown in Table 1. The viscosity reduction rate test formula is as follows:

[0062]

[0063] Among them, The reading of the base slurry without viscosity reducing agent treatment under the six-speed rotation viscometer; It is the reading of the base slurry after being treated with viscosity reducer under a six-speed rotation viscometer.

[0064] Table 1 Performance test data

[0065]

[0066] Data Analysis:

[0067] It can be seen from Examples 1-3 that the viscosity reducer for drilling fluid suitable for deep wells prepared by the present invention has excellent viscosity reducing performance. At room temperature, the viscosity reduction rates of fresh water-based slurry and high salt content fresh water-based slurry can reach 81.5% and 78.3%, respectively. Most importantly, at 260°C, the viscosity reduction rates of fresh water-based slurry and high salt content fresh water-based slurry can still reach 65.3% and 89.1%, respectively, indicating that it has excellent salt resistance and temperature resistance. In addition, the viscosity reduction rate also has good anti-filtration performance, which can meet the complex bottom environment of deep wells.

[0068] From Example 2 and Comparative Examples 1-4, it can be seen that the dual functionalization of carbon nanotubes with amphoteric silane coupling agents and phenyltriethoxysilane can effectively improve the viscosity reduction performance and temperature resistance and salt resistance. This may be because the dual functionalized carbon nanotubes can be more effectively compounded with amphoteric viscosity-reducing polymers, synergistically dismantling the spatial network structure formed by clay, and at the same time, the tubular structure can help release the encapsulated free water, reduce the flow friction resistance between clay particles, thereby reducing the viscosity of the drilling fluid, enhancing the fluidity of the drilling fluid, and thus improving the viscosity reduction performance. In addition, the thermal conductivity of carbon nanotubes and the charge regulation on the surface of carbon nanotubes help to further improve their salt resistance and heat resistance.

[0069] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

Claims

1. A viscosity reducer for drilling fluid suitable for deep wells, characterized in that: The invention is obtained by mixing an amphoteric viscosity-reducing polymer and a bifunctional carbon nanotube; the weight ratio of the amphoteric viscosity-reducing polymer to the bifunctional carbon nanotube is 20-30:0.5-1; The amphoteric viscosity-reducing polymer is prepared by polymerization reaction of monomer raw materials, wherein the monomer raw materials include acrylamide, acrylic acid, sodium p-styrene sulfonate and methacryloylethyl sulfobetaine; The weight ratio of acrylamide, acrylic acid, sodium p-styrene sulfonate and methacryloylethyl sulfobetaine is 10-15:2-3:15-25:3-5; The preparation method of the bifunctional carbon nanotubes is as follows: dispersing carbon nanotubes in anhydrous ethanol, adjusting the pH to 9-10 with aqueous ammonia, adding amphoteric silane coupling agent and phenyltriethoxysilane, heating to 50-60° C., stirring for 12-14 hours, centrifuging, washing, and obtaining bifunctional carbon nanotubes; The weight ratio of the carbon nanotubes, anhydrous ethanol, amphoteric silane coupling agent and phenyltriethoxysilane is 1:20-30:0.3-0.5:0.1-0.2; The preparation method of the amphoteric silane coupling agent is as follows: triethoxy-3-(2-imidazoline-1-yl)propylsilane and 1,3-propane sultone are added to anhydrous acetone, and refluxed for 16-18 hours under a nitrogen atmosphere, and after the reaction is completed, rotary evaporation is performed to obtain the amphoteric silane coupling agent; The weight ratio of the triethoxy-3-(2-imidazoline-1-yl)propylsilane, 1,3-propane sultone and anhydrous acetone is 1:0.48-0.55:20-30.

2. The viscosity reducer for drilling fluid suitable for deep wells according to claim 1, characterized in that: The specific preparation method of the amphoteric viscosity-reducing polymer is as follows: under a nitrogen atmosphere, the monomer raw material is added to ethyl acetate, the temperature is raised to 60-65° C., and stirred for 20-30 minutes, then an initiator is added, the temperature is raised to 80-90° C., and the reaction is stirred for 8-10 hours, then an inhibitor is added, stirred for 10-20 minutes, rotary evaporated, washed, and dried to obtain the amphoteric viscosity-reducing polymer.

3. The viscosity reducer for drilling fluid suitable for deep wells according to claim 2, characterized in that: The weight ratio of the monomer raw material, ethyl acetate, initiator and inhibitor is 30-48:150-250:1-2:1.2-1.

8.

4. The viscosity reducer for drilling fluid suitable for deep wells according to claim 2, characterized in that: The initiator is azobisisobutyronitrile.

5. The viscosity reducer for drilling fluid suitable for deep wells according to claim 2, characterized in that: The polymerization inhibitor is p-hydroxyanisole.

6. The viscosity reducer for drilling fluid suitable for deep wells according to claim 1, characterized in that: The carbon nanotubes are double-walled carbon nanotubes with a diameter of 20-40 nm and a length of 1-2 μm.

7. The viscosity reducer for drilling fluid suitable for deep wells according to claim 1, characterized in that: The mass fraction of the ammonia water is 28%.

8. The viscosity reducer for drilling fluid suitable for deep wells according to claim 1, characterized in that: The temperature resistance of the viscosity reducer for deep well drilling fluid can reach 260°C.

9. A method for preparing a viscosity reducer for deep well drilling fluid according to any one of claims 1 to 8, characterized in that: The following steps are involved: The viscosity reducing agent for drilling fluid suitable for deep wells is obtained by uniformly mixing the amphoteric viscosity reducing polymer and the bifunctional carbon nanotube.