Coated glass and preparation method thereof

By forming a double-layer coating structure on the glass, using the first layer with small pores and the third layer around large pores to provide stress support, the problem of water vapor entering porous AR-coated glass is solved, and the stability and performance of the glass are improved.

CN118545919BActive Publication Date: 2024-10-01XINYI PHOTOVOLTAIC (SUZHOU) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411029750.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-01
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

Existing porous AR-coated glass is prone to holes under the influence of the external environment, causing water vapor to enter the glass surface, triggering the glass hydrolysis reaction and affecting performance.

Method used

It adopts a double-layer coating structure, in which the first layer of coating forms dense micropores, and the second layer of coating forms larger pores and smaller pores around them, providing stress support and buffering to prevent water vapor from contacting the glass surface.

Benefits of technology

It effectively prevents water vapor from entering the glass surface, protects the performance parameters of the glass, and improves the stability and performance of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118545919B_ABST
    Figure CN118545919B_ABST
Patent Text Reader

Abstract

The present application provides a coated glass and a preparation method thereof, comprising: a glass substrate; a first porous insulating film layer, covering a side surface of the glass substrate; and a second porous insulating film layer, covering a side surface of the first porous insulating film layer away from the glass substrate, wherein the first porous insulating film layer comprises a plurality of first micropores, and the second porous insulating film layer comprises a plurality of micropore units, each of which comprises a second micropore and a plurality of third micropores surrounding the second micropores; the present application can ensure the performance of the coating through the second micropores, and the third micropores are arranged around the large aperture, at which time the physical structure of the second micropores forms stress support and buffering for the first micropores, and when an external force acts on the second micropores to cause them to break, the presence of the third micropores provides a certain space for unloading the external force compared to a solution without the third micropores, so that the second micropores are not easy to break, thus avoiding contact between water vapor and the glass surface and ensuring the performance parameters of the glass.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of coated glass, and in particular to coated glass and a preparation method thereof. Background Art

[0002] Anti-reflective coating (AR Coating) is a technology that deposits one or more layers of thin film materials with specific optical properties on the surface of optical elements to reduce the reflection loss of light and improve the transmittance and optical performance. The main goal of AR coating is to reduce the reflection of light at the interface, thereby increasing the light intensity passing through the optical element. There are many methods for coating the glass surface, such as sputtering to coat the anti-reflection film. Currently, a single layer of SiO2 coating is generally used. Because the sputtering process can form a porous structure, the performance parameters such as the refractive index and thermal conductivity of the coating are improved. However, under the influence of the external environment, if the surface protection layer of the porous SiO2 film is not strong enough, there is a certain probability that one or more hollow spheres will break, thereby forming 30~50nm holes on the surface of the film, thereby triggering the capillary effect. The surface water vapor will further quickly introduce the contact layer between the film layer and the glass surface, thereby triggering the hydrolysis reaction on the glass surface, affecting the performance parameters of the glass, and there are many shortcomings. Summary of the invention

[0003] The purpose of the present application is to provide a coated glass and a preparation method, aiming to solve the problem that water vapor enters the glass surface due to the current porous AR coating, thereby triggering glass hydrolysis.

[0004] A first aspect of the present application provides a coated glass, including:

[0005] Glass substrate;

[0006] A first porous insulating film layer covering a surface of one side of the glass substrate; and

[0007] A second porous insulating film layer covers a surface of the first porous insulating film layer away from the glass substrate, wherein the first porous insulating film layer includes a plurality of first micropores, and the second porous insulating film layer includes a plurality of micropore units, each of which includes a second micropore and a plurality of third micropores surrounding the second micropore;

[0008] The aperture of the third micropore is smaller than the aperture of the second micropore, and in each micropore unit, the distance between the second micropore and each third micropore is within a first set threshold.

[0009] In an optional embodiment, the pore size of the first micropore is smaller than the pore size of the third micropore.

[0010] In an optional embodiment, the distance between any two adjacent third microholes is smaller than the second set threshold.

[0011] In an optional embodiment, the second porous insulating film layer includes: a first sub-insulating film layer, an indium tin oxide layer and a second sub-insulating film layer which are stacked; the first sub-insulating film layer is close to the first porous insulating film layer; wherein the indium tin oxide layer includes indium tin oxide and silicon dioxide, and the indium tin oxide and silicon dioxide are formed by the same sputtering process.

[0012] In an optional embodiment, the sputtering concentration of the indium tin oxide is less than one percent of the sputtering concentration of the silicon dioxide.

[0013] In an optional embodiment, the second porous insulating film layer includes: indium tin oxide and silicon dioxide, the concentration of the indium tin oxide is less than one five hundredth of the concentration of the silicon dioxide, and the indium tin oxide and the silicon dioxide are formed by the same sputtering process.

[0014] In an optional embodiment, the first porous insulating film layer is rapidly cooled after being formed by sputtering, and the second porous insulating film layer is cooled in multiple stages after being formed by sputtering, each stage firstly being cooled slowly and then being aged for a set time.

[0015] In an optional embodiment, in two adjacent stages, the set duration relative to the latter stage is smaller than the set duration relative to the former stage.

[0016] In an optional embodiment, during each stage of the aging process, a heat source dot matrix plate is used to cover the second porous insulating film layer, wherein the heat source dot matrix plate includes a plurality of electric heating needles arranged in an array, and the diameter of each electric heating needle is less than 3 mm.

[0017] In an optional embodiment, the first porous insulating film layer includes silicon dioxide and a non-polar bonding element, and the non-polar bonding element can form a bonding structure with silicon and oxygen.

[0018] In an optional embodiment, the non-polar bonding element includes Ti element.

[0019] A second aspect of the present application provides a method for preparing coated glass, comprising:

[0020] forming a glass substrate;

[0021] forming a first porous insulating film layer on the glass substrate;

[0022] A second porous insulating film layer is formed on a surface of the first porous insulating film layer away from the glass substrate; the first porous insulating film layer includes a plurality of first micropores, the second porous insulating film layer includes a plurality of micropore units, each micropore unit includes a second micropore and a plurality of third micropores surrounding the second micropore;

[0023] The aperture of the third micropore is smaller than the aperture of the second micropore, and in each micropore unit, the distance between the second micropore and each third micropore is within a first set threshold.

[0024] Compared with the prior art, the embodiments of the present application have the following beneficial effects: by configuring a double-layer coating, the micropores (first micropores) formed by the first layer of coating have a small aperture and are relatively dense, the aperture of the second layer of coating is relatively large, and at the same time, small apertures (third micropores) are formed around the large apertures (second micropores) of the second layer of coating. At this time, the second micropores can ensure the performance of the coating, and the third micropores are arranged around the large apertures. At this time, the physical structure of the second micropores forms stress support and buffering for the first micropores. When an external force acts on the second micropore to cause it to break, the presence of the third micropore provides a certain space for unloading the external force compared to a solution without the third micropore, so that the second micropore is not easy to break, thereby avoiding contact between water vapor and the glass surface and ensuring the performance parameters of the glass. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is one of the structural schematic diagrams of a coated glass provided in an embodiment of the present application.

[0026] Figure 2 This is a second schematic diagram of the structure of a coated glass provided in an embodiment of the present application.

[0027] Figure 3 This is a third structural schematic diagram of a coated glass provided in an embodiment of the present application. DETAILED DESCRIPTION

[0028] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0029] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.

[0030] It should be understood that the orientation or position relationship indicated by terms such as "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0031] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0032] The present application aims to solve the problem that water vapor enters the glass surface due to the current porous AR coating, thereby triggering glass hydrolysis.

[0033] Specifically, in order to facilitate understanding of the present application, the present application embodiment first provides a coated glass, such as Figure 1 and Figure 3 As shown, the glass coating of the present application includes: a glass substrate 1; a first porous insulating film layer 21, covering one side surface of the glass substrate 1; and a second porous insulating film layer 22, covering the side surface of the first porous insulating film layer 21 away from the glass substrate 1, the first porous insulating film layer 21 includes a plurality of first micropores 211, the second porous insulating film layer 22 includes a plurality of micropore units 224, each micropore unit 224 includes a second micropore 2211 and a plurality of third micropores 2212 surrounding the second micropore 2211; wherein the pore size of the third micropore 2212 is smaller than the pore size of the second micropore 2211, and in each micropore unit 224, the distance between the second micropore 2211 and each third micropore 2212 is within a first set threshold.

[0034] The present application configures a double-layer coating. The micropores (first micropores 211) formed by the first layer of coating have a small aperture and are relatively dense. The aperture of the second layer of coating is relatively large. At the same time, small apertures (third micropores 2212) are formed around the large apertures (second micropores 2211) of the second layer of coating. At this time, the second micropores 2211 can ensure the performance of the coating, and the third micropores 2212 are arranged around the large apertures. At this time, the physical structure of the second micropores 2211 forms stress support and buffering for the first micropores 211. When external force acts on the second micropores 2211 to cause it to break, due to the existence of the third micropores 2212, a certain space is provided for unloading the external force compared to the solution without the third micropores 2212, so that the second micropores 2211 are not easy to break, thereby avoiding the contact between water vapor and the glass surface and ensuring the performance parameters of the glass.

[0035] In the embodiment of the present application, the insulating film layer can be a SiO2 film layer, which can be formed by evaporation and sputtering. Specifically, Si and SiO2 can be evaporated or bombarded and sputtered onto the surface of the glass substrate 1 by an electron beam or a laser beam to form a SiO2 film layer.

[0036] Specifically, high-purity quartz or single-crystal silicon can be selected as the target material, and SiO2 can be prepared by magnetron sputtering. Through the radio frequency sputtering process, a mixed gas of 99.99% pure oxygen and 99.99% pure argon is introduced as the working gas, and a high-frequency voltage with a power of 300-500W and a frequency of 13.56MHz is applied to the target.

[0037] In the embodiment of the present application, the first porous insulating film layer 21 is arranged close to the glass substrate 1. The first porous insulating film layer 21 is a relatively dense protective film layer, and the pore size of the first micropore 211 thereof is the smallest, which can provide the protective function of isolating the surface of the glass substrate 1 from water vapor. The second porous insulating film layer 22 is relatively arranged on the outside, that is, directly in contact with the air, so that the second micropores 2211 and the third micropores 2212 in the second porous insulating film layer 22 are relatively large, wherein the third micropore 2212 is larger than the first micropore 211, and the third micropore 2212 is arranged around the second micropore 2211 to form a "micropore unit 224". It should be noted that the micropore units 224 of the present application can be evenly distributed in the second porous insulating film layer 22, and the present application does not impose any limitation on this.

[0038] In the micropore unit 224 of the present application, a second micropore 2211 with a larger aperture and a third micropore 2212 with a smaller aperture are included. Due to the presence of the third micropore 2212, when the second micropore 2211 is subjected to external impact force, if the third micropore 2212 does not exist, the second micropore 2211 is squeezed and broken when subjected to force. The capillary effect of the second micropore 2211 allows water vapor to enter the second micropore 2211 due to the breakage, and then penetrate to the surface of the glass substrate 1. In the present application, a plurality of third micropores 2212 with smaller apertures are formed around the second micropore 2211. The third micropore 2212 is first formed by Due to its smaller aperture, it is less susceptible to external impact force. When the second micropore 2211 is subjected to external impact force, due to the "idle" space of the third micropore 2212 formed around it, the third micropore 2212 is equivalent to a "force unloading zone" at this time, and the force of the second micropore 2211 is transmitted to the third micropore 2212, and most of the force is unloaded by squeezing the third micropore 2212. Since the aperture of the third micropore 2212 is smaller, even if it is subjected to external impact force, it will not cause excessive deformation and water vapor will not enter. In this way, through the cooperation of the third micropore 2212, the rigidity of the second micropore 2211 can be prevented from being damaged.

[0039] It should be noted that the film thickness of the first porous insulating film layer 21 of the present application can be lower than the film thickness of the second porous insulating film layer 22. In this way, on the one hand, it can provide the final guarantee for isolating water vapor (only when there is too much water vapor and the external air pressure is too high, this situation may cause some micro-nano level water vapor to adhere to the glass substrate 1 through the second porous insulating film layer 22), and on the other hand, the second porous insulating film layer 22 can provide better glass coating properties such as refractive index.

[0040] In the embodiment of the present application, in each micropore unit 224, the distance between the second micropore 2211 and the relatively farthest third micropore 2212 is within the distance of the set threshold. Specifically, during the manufacturing process of the coated glass of the present application, since the first porous insulating film layer 21 and the second porous insulating film layer 22 are formed by a sputtering process, they are not formed according to the arrangement pattern of the micropore unit 224 when formed, that is, the micropore unit 224 of the present application belongs to a "virtual definition". Specifically, when dividing the third micropore 2212, it can be configured according to the distance between the third micropore 2212 and the second micropore 2211, that is, the third micropore 2212 with a distance less than the set threshold is configured to the corresponding second micropore 2211 to form a micropore unit 224. In this way, each micropore unit 224 can be configured. When the micropore unit 224 configured based on the distance is subjected to force on the second micropore 2211, the third micropore 2212 corresponding to the same micropore unit 224 is first affected by the force due to its closer distance, thereby completing the unloading of the force first.

[0041] The present application is described in detail below through a microstructure schematic diagram.

[0042] In an optional embodiment, the aperture of the first micropore 211 is smaller than the aperture of the third micropore 2212. In this embodiment, the aperture of the first micropore 211 is further smaller than the third micropore 2212, and the first porous insulating film layer 21 forms a dense SiO2 film layer, thereby providing the final guarantee to prevent water vapor from entering.

[0043] In the embodiment of the present application, the first micropore 211 of micro-nano level can be formed by magnetron sputtering process, for example, the diameter of the first micropore 211 is within 100um (micrometer level), and the present application does not limit this. The aperture of the second micropore 2211 is larger than the aperture of the first micropore 211, for example, 300um, and the diameter of the second micropore 2211 is preferably within the range of 500um. In the sputtering process, it can be controlled by controlling the concentration of Si element and sputtering time and other parameters, and the present application does not limit this.

[0044] In an optional embodiment, the distance between any two adjacent third micropores 2212 is less than the second set threshold. For example, the distance between any two third micropores 2212 is within 50um, or within 30um, that is, preferably, the distance between any two third micropores 2212 is less than the diameter of the second micropore 2211, and more preferably, the diameter of the first micropore 211 is less than the diameter of the third micropore 2212, that is, at this time, the first micropore 211 can be formed into a nanometer level by an evaporation process, for example, within 100nm, and the present application does not limit this.

[0045] It should be noted that, in theory, the sputtering process of the first porous insulating film layer 21 can be achieved by increasing the Si element concentration and the sputtering time. However, if the Si element concentration and the sputtering time are increased, the thickness of the film layer will be greatly increased during the actual process. The present application creatively adopts a low-concentration multiple rapid staggered sputtering process. Specifically, multiple (generally 2-3) sputtering initial points are pre-configured, and then sputtering is started on the glass substrate at each initial point with a lower Si element concentration. Due to multiple sputtering, the coverage rate of the Si element per unit area is increased. In specific experiments, the lower Si element concentration can be less than one-quarter of the concentration required for a single sputtering to achieve the corresponding target coverage rate, and the total sputtering time is only increased by 2 times (the single sputtering speed of the original process is lower than the sputtering speed after this optimization). Therefore, the thickness of the first porous insulating film layer 21 can be significantly reduced through this process optimization.

[0046] The second porous insulating film layer 22 is much more difficult to manufacture than the first porous insulating film layer 21. Specifically, the prior art has not yet produced pores of different sizes in the same film layer. The present application can arrange a "sputtering mask" with hollows of different sizes above the glass substrate 1 during sputtering. The solid part of the sputtering mask corresponds to the second micropores 2211 and the third micropores 2212 formed by sputtering on the glass substrate 1. Therefore, by configuring the size of the solid part, the second micropores 2211 and the third micropores 2212 can be formed during sputtering.

[0047] In an optional embodiment, if Figure 2 As shown, the second porous insulating film layer 22 includes: a first sub-insulating film layer 221, an indium tin oxide layer 222 and a second sub-insulating film layer 223 which are stacked; the first sub-insulating film layer 221 is close to the first porous insulating film layer 21; wherein the indium tin oxide layer 222 includes indium tin oxide 2213 and silicon dioxide, and the indium tin oxide 2213 and silicon dioxide are formed by the same sputtering process.

[0048] In this embodiment, in order to further improve the performance of the coated glass, the second porous insulating film layer 22 can be configured as an insulating-partially insulating-insulating sandwich structure. Since the outermost layer is all insulating, an overall insulating structure is formed.

[0049] After the indium tin oxide layer 222 is added, since the indium tin oxide layer 222 includes indium tin oxide 2213, the indium tin oxide 2213 itself is transparent and will not affect the light transmission performance of the coated glass. In addition, since the indium tin oxide 2213 is also formed by sputtering, the indium tin oxide 2213 is uniformly mixed in the silicon dioxide layer. At this time, the indium tin oxide 2213 existing as a heterogeneous substance can significantly improve the firmness of the second porous insulating film layer 22 because it is a metal oxide. When the second micropore 2211 is subjected to external force, the indium tin oxide 2213 can play a better supporting role.

[0050] In the specific preparation, different sputtering heads can be used for simultaneous sputtering, and mask sputtering can also be performed under the above-mentioned sputtering mask. In this way, the indium tin oxide 2213 can be evenly distributed in the indium tin oxide layer 222, thereby improving the overall supporting performance without affecting the formation of the second micropores 2211 and the third micropores 2212.

[0051] In an optional embodiment, the sputtering concentration of the indium tin oxide 2213 is less than 1% of the sputtering concentration of the silicon dioxide. Since the indium tin oxide 2213 itself exists as a heterogeneous material for supporting and adjusting performance, the sputtering concentration of the indium tin oxide 2213 is controlled to be less than 1% of the sputtering concentration of the silicon dioxide, and the content of the indium tin oxide 2213 in the second porous insulating film layer 22 finally formed is less than 1% of the content of the silicon dioxide, which is not described in detail in this application.

[0052] In an optional embodiment, the second porous insulating film layer 22 includes: indium tin oxide 2213 and silicon dioxide, the concentration of the indium tin oxide 2213 is less than one five hundredth of the concentration of the silicon dioxide, and the indium tin oxide 2213 and the silicon dioxide are formed by the same sputtering process.

[0053] In this embodiment, the second porous insulating film layer 22 can be integrally configured with the indium tin oxide 2213. In this way, there is no need to configure a sandwich structure, which can save process. Due to the existence of the first porous insulating film layer 21, it can be ensured that the second porous insulating film layer 22 will not contact the glass substrate 1, thereby also avoiding the influence of the indium tin oxide 2213 on the glass substrate 1.

[0054] It should be noted that, in this embodiment, since the second porous insulating film layer 22 is entirely configured with indium tin oxide 2213, its sputtering concentration can be less than one five hundredth of the silicon dioxide concentration, so that the aforementioned technical efficacy can be guaranteed.

[0055] The present application further creatively discovered that in order to avoid the second micropores from rupturing, internal stress can be used to alleviate the problem. In an optional embodiment, the first porous insulating film layer is rapidly cooled after being sputtered, and the second porous insulating film layer is cooled in multiple stages after being sputtered. Each stage is first cooled slowly and then aged for a set period of time. Rapid cooling will cause internal stress to increase. The reason why the second micropores are prone to rupture is that, on the one hand, the external force cannot be relieved and buffered. On the other hand, even if there is no external force, the second micropores are formed by a sputtering process, which will cause internal stress to be generated during the cooling process, so that the second micropores are continuously in a state of internal stress. Therefore, the second micropores are prone to rupture even if there is no external force. The inventors of the present application found that the fundamental reason for the rupture of the second micropores is not only the external force but also the internal stress. Based on this, the preferred embodiment of the present application can reduce the magnitude of internal stress by temperature control during the cooling process of the second porous insulating film layer. Specifically, the generation of internal stress is caused by instantaneous temperature difference, that is, sudden cooling at a high position will cause an increase in internal stress. Based on this, the present application can reduce the cooling rate and the instantaneous cooling temperature difference through multiple slow cooling, thereby reducing the generation of internal stress. Furthermore, the present application sets the aging time, so that the stress is further eliminated through aging after each slow cooling, thereby reducing the internal stress.

[0056] Furthermore, in an optional embodiment, in two adjacent stages, the set duration relative to the latter stage is shorter than the set duration relative to the former stage. In this embodiment, since the temperature drops fastest and the temperature difference is the largest at the beginning of cooling, the stress formed at this time is greater, and the stress can be eliminated through a longer period of aging, so that the subsequent aging time is continuously reduced.

[0057] It should be noted that, during the aging process at each stage, a heat source dot matrix plate can be used to cover the second porous insulating film layer, wherein the heat source dot matrix plate includes a plurality of electric heating needles arranged in an array, and the diameter of each electric heating needle is less than 3 mm. In this way, the second porous insulating film layer is "slightly" heated by the heat source, thereby providing a reaction force opposite to the positive stress formed by the current cooling during the aging process, thereby partially offsetting the positive stress, reducing the magnitude of the positive stress, and facilitating further stress reduction. In addition, the dot matrix heat source can provide a more uniform and stable heat source in the second porous insulating film layer, avoiding the uneven heat distribution caused by a single point heat source.

[0058] In an optional embodiment, the first porous insulating film layer includes silicon dioxide and a non-polar bonding element, and the non-polar bonding element can form a bonding structure with silicon and oxygen.

[0059] In an optional embodiment, the non-polar bonding element includes Ti element. Ti element can reduce the polarity of silicon dioxide, thereby increasing the hydrophobic property.

[0060] A second aspect of the present application provides a method for preparing coated glass, comprising:

[0061] S1: forming a glass substrate;

[0062] S2: forming a first porous insulating film layer on the glass substrate;

[0063] S3: forming a second porous insulating film layer on a surface of the first porous insulating film layer away from the glass substrate; the first porous insulating film layer includes a plurality of first micropores, the second porous insulating film layer includes a plurality of micropore units, each micropore unit includes a second micropore and a plurality of third micropores surrounding the second micropore;

[0064] The aperture of the third micropore is smaller than the aperture of the second micropore, and in each micropore unit, the distance between the second micropore and each third micropore is within a first set threshold.

[0065] The present application configures a double-layer coating. The micropores (first micropores 211) formed by the first layer of coating have a small aperture and are relatively dense. The aperture of the second layer of coating is relatively large. At the same time, small apertures (third micropores 2212) are formed around the large apertures (second micropores 2211) of the second layer of coating. At this time, the second micropores 2211 can ensure the performance of the coating, and the third micropores 2212 are arranged around the large apertures. At this time, the physical structure of the second micropores 2211 forms stress support and buffering for the first micropores 211. When external force acts on the second micropores 2211 to cause it to break, due to the existence of the third micropores 2212, a certain space is provided for unloading the external force compared to the solution without the third micropores 2212, so that the second micropores 2211 are not easy to break, thereby avoiding the contact between water vapor and the glass surface and ensuring the performance parameters of the glass.

[0066] In the embodiment of the present application, the insulating film layer can be a SiO2 film layer, which can be formed by evaporation and sputtering. Specifically, Si and SiO2 can be evaporated or bombarded and sputtered onto the surface of the glass substrate 1 by an electron beam or a laser beam to form a SiO2 film layer.

[0067] Specifically, high-purity quartz or single-crystal silicon can be selected as the target material, and SiO2 can be prepared by magnetron sputtering. Through the radio frequency sputtering process, a mixed gas of 99.99% pure oxygen and 99.99% pure argon is introduced as the working gas, and a high-frequency voltage with a power of 300-500W and a frequency of 13.56MHz is applied to the target.

[0068] In the embodiment of the present application, the first micropore 211 of micro-nano level can be formed by magnetron sputtering process, for example, the diameter of the first micropore 211 is within 100um (micrometer level), and the present application does not limit this. The aperture of the second micropore 2211 is larger than the aperture of the first micropore 211, for example, 300um, and the diameter of the second micropore 2211 is preferably within the range of 500um. In the sputtering process, it can be controlled by controlling the concentration of Si element and sputtering time and other parameters, and the present application does not limit this.

[0069] It should be noted that, in theory, the sputtering process of the first porous insulating film layer 21 can be achieved by increasing the Si element concentration and the sputtering time. However, if the Si element concentration and the sputtering time are increased, the thickness of the film layer will be greatly increased during the actual process. The present application creatively adopts a low-concentration multiple rapid staggered sputtering process. Specifically, multiple (generally 2-3) sputtering initial points are pre-configured, and then sputtering is started on the glass substrate at each initial point with a lower Si element concentration. Due to multiple sputtering, the coverage rate of the Si element per unit area is increased. In specific experiments, the lower Si element concentration can be less than one-quarter of the concentration required for a single sputtering to achieve the corresponding target coverage rate, and the total sputtering time is only increased by 2 times (the single sputtering speed of the original process is lower than the sputtering speed after this optimization). Therefore, the thickness of the first porous insulating film layer 21 can be significantly reduced through this process optimization.

[0070] The second porous insulating film layer 22 is much more difficult to manufacture than the first porous insulating film layer 21. Specifically, the prior art has not yet produced pores of different sizes in the same film layer. The present application can arrange a "sputtering mask" with hollows of different sizes above the glass substrate 1 during sputtering. The solid part of the sputtering mask corresponds to the second micropores 2211 and the third micropores 2212 formed by sputtering on the glass substrate 1. Therefore, by configuring the size of the solid part, the second micropores 2211 and the third micropores 2212 can be formed during sputtering.

[0071] Optionally, during the specific preparation, different sputtering heads can be used for simultaneous sputtering, and mask sputtering can also be performed under the above-mentioned sputtering mask. In this way, the indium tin oxide 2213 can be evenly distributed in the indium tin oxide layer 222, thereby improving the overall supporting performance without affecting the formation of the second micropores 2211 and the third micropores 2212.

[0072] The present application further creatively discovered that in order to avoid the second micropores from rupturing, internal stress can be used to alleviate the problem. In an optional embodiment, the first porous insulating film layer is rapidly cooled after being sputtered, and the second porous insulating film layer is cooled in multiple stages after being sputtered. Each stage is first cooled slowly and then aged for a set period of time. Rapid cooling will cause internal stress to increase. The reason why the second micropores are prone to rupture is that, on the one hand, the external force cannot be relieved and buffered. On the other hand, even if there is no external force, the second micropores are formed by a sputtering process, which will cause internal stress to be generated during the cooling process, so that the second micropores are continuously in a state of internal stress. Therefore, the second micropores are prone to rupture even if there is no external force. The inventors of the present application found that the fundamental reason for the rupture of the second micropores is not only the external force but also the internal stress. Based on this, the preferred embodiment of the present application can reduce the magnitude of internal stress by temperature control during the cooling process of the second porous insulating film layer. Specifically, the generation of internal stress is caused by instantaneous temperature difference, that is, sudden cooling at a high position will cause an increase in internal stress. Based on this, the present application can reduce the cooling rate and the instantaneous cooling temperature difference through multiple slow cooling, thereby reducing the generation of internal stress. Furthermore, the present application sets the aging time, so that the stress is further eliminated through aging after each slow cooling, thereby reducing the internal stress.

[0073] Furthermore, in an optional embodiment, in two adjacent stages, the set duration relative to the latter stage is shorter than the set duration relative to the former stage. In this embodiment, since the temperature drops fastest and the temperature difference is the largest at the beginning of cooling, the stress formed at this time is greater, and the stress can be eliminated through a longer period of aging, so that the subsequent aging time is continuously reduced.

[0074] It should be noted that, during the aging process at each stage, a heat source dot matrix plate can be used to cover the second porous insulating film layer, wherein the heat source dot matrix plate includes a plurality of electric heating needles arranged in an array, and the diameter of each electric heating needle is less than 3 mm. In this way, the second porous insulating film layer is "slightly" heated by the heat source, thereby providing a reaction force opposite to the positive stress formed by the current cooling during the aging process, thereby partially offsetting the positive stress, reducing the magnitude of the positive stress, and facilitating further stress reduction. In addition, the dot matrix heat source can provide a more uniform and stable heat source in the second porous insulating film layer, avoiding the uneven heat distribution caused by a single point heat source.

[0075] Those skilled in the art can clearly understand that for the convenience and simplicity of description, only the division of the above-mentioned functional units and modules is used as an example for illustration. In actual applications, the above-mentioned functions can be distributed and completed by different functional units and modules as needed, that is, the internal structure of the device can be divided into different functional units or modules to complete all or part of the functions described above. The functional units and modules in the embodiments can be integrated into a processing unit, or each unit can exist physically separately, or two or more units can be integrated into one unit. In addition, the specific names of the functional units and modules are only for the convenience of distinguishing each other, and are not used to limit the scope of protection of this application. The specific working process of the units and modules in the above-mentioned system can refer to the corresponding process in the aforementioned method embodiment, which will not be repeated here.

[0076] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described or recorded in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0077] The units described as separate components may or may not be physically separated, and the components shown as units may or may not be physical units, that is, they may be located in one place or distributed on multiple units. Some or all of the units may be selected according to actual needs to achieve the purpose of the present embodiment.

[0078] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.

Claims

1. A coated glass, characterized in that: include: Glass substrate; A first porous insulating film layer, covering a surface of one side of the glass substrate; as well as A second porous insulating film layer covers a surface of the first porous insulating film layer away from the glass substrate, wherein the first porous insulating film layer includes a plurality of first micropores, and the second porous insulating film layer includes a plurality of micropore units, each of which includes a second micropore and a plurality of third micropores surrounding the second micropore; The aperture of the third micropore is smaller than the aperture of the second micropore, and in each micropore unit, the distance between the second micropore and each third micropore is within a first set threshold.

2. The coated glass according to claim 1, characterized in that: The pore size of the first micropore is smaller than the pore size of the third micropore.

3. The coated glass according to claim 2, characterized in that: The distance between any two adjacent third micro-holes is smaller than the second set threshold.

4. The coated glass according to claim 1, characterized in that: The second porous insulating film layer includes: a first sub-insulating film layer, an indium tin oxide layer and a second sub-insulating film layer which are stacked; the first sub-insulating film layer is close to the first porous insulating film layer; wherein the indium tin oxide layer includes indium tin oxide and silicon dioxide, and the indium tin oxide and silicon dioxide are formed by the same sputtering process.

5. The coated glass according to claim 4, characterized in that: The sputtering concentration of the indium tin oxide is less than one percent of the sputtering concentration of the silicon dioxide.

6. The coated glass according to claim 1, characterized in that: The second porous insulating film layer includes: indium tin oxide and silicon dioxide, the concentration of the indium tin oxide is less than one-five hundredth of the concentration of the silicon dioxide, and the indium tin oxide and the silicon dioxide are formed by the same sputtering process.

7. The coated glass according to claim 1, characterized in that: The first porous insulating film layer is rapidly cooled after being formed by sputtering, and the second porous insulating film layer is cooled in multiple stages after being formed by sputtering, each stage firstly being cooled slowly and then being aged for a set time.

8. The coated glass according to claim 7, characterized in that: In two adjacent stages, the set duration relative to the latter stage is shorter than the set duration relative to the former stage.

9. The coated glass according to claim 7, characterized in that: During the aging process at each stage, a heat source matrix plate is used to cover the second porous insulating film layer, wherein the heat source matrix plate comprises a plurality of electric heating needles arranged in an array, and the diameter of each electric heating needle is less than 3 mm.

10. The coated glass according to claim 1, characterized in that: The first porous insulating film layer includes silicon dioxide and a non-polar bonding element, and the non-polar bonding element can form a bonding structure with silicon and oxygen.

11. The coated glass according to claim 10, characterized in that: The non-polar bonding element includes Ti element.

12. A method for preparing coated glass, characterized in that: include: forming a glass substrate; forming a first porous insulating film layer on the glass substrate; A second porous insulating film layer is formed on a surface of the first porous insulating film layer away from the glass substrate; the first porous insulating film layer includes a plurality of first micropores, the second porous insulating film layer includes a plurality of micropore units, each micropore unit includes a second micropore and a plurality of third micropores surrounding the second micropore; The aperture of the third micropore is smaller than the aperture of the second micropore, and in each micropore unit, the distance between the second micropore and each third micropore is within a first set threshold.

Citation Information

Patent Citations

  • Dual-function film coated glass capable of realizing anti-dazzle performance and visible light antireflection and preparation method of glass

    CN103921487A

  • Anti-reflection coating liquid suitable for double-layer coating as well as preparation method and application thereof

    CN113337208A

  • Coated glass for photovoltaic module and preparation method thereof

    CN114436543A

  • Solar battery component coated cover board glass

    CN201549516U

  • SiO2 antireflective film for solar photovoltaic glass

    CN202943944U