Preparation method of transparent antifreeze hydrogel with adjustable mechanical properties
By mixing acrylic acid monomer and high-polymerization polyvinyl alcohol with acid solution and performing freeze-thaw cycles, combined with salting out and pressure treatment, a hydrogel with high transparency and frost resistance was prepared, solving the existing transparent protection problem The problem of insufficient material structural stability and frost resistance has been achieved by improving the mechanical properties and enhancing the frost resistance.
Patent Information
- Application Number
- CN202411026512.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Existing transparent protective materials have poor structural stability, low transparency, and insufficient frost resistance and dehydration resistance when impact deformation, which limits their impact-resistant transparent protection applications under load environmental conditions.
By mixing a mixture of acrylic acid monomer and high-polymerization polyvinyl alcohol with an acid solution and then subjecting it to freezing and ablation cycles, combined with a salting-out agent and pressure, a hydrogel with high transparency and frost resistance is prepared to form The "hard-soft" two-phase microstructure improves the mechanical properties of the material.
The mechanical properties of the hydrogel can be adjusted, and it has high transparency and excellent frost resistance comparable to organic glass. It can maintain stable transparency and long service time in low temperature environments.
Smart Images

Figure CN118546306B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrogels, and in particular to a method for preparing a transparent, antifreeze hydrogel with adjustable mechanical properties. Background Art
[0002] Polymer transparent protective materials refer to transparent protective materials / structures that have both light-transmitting and image-transmitting functions and excellent mechanical properties, and are mainly used for the protection of various windows and observation areas. At present, polymer transparent protective materials mainly include base materials such as polymethyl methacrylate (PMMA), polycarbonate (PC) or polyurethane (PU), and interlayer adhesive materials such as polyvinyl butyral, polyurethane, silicone, and acrylate. Although polymer materials show better impact resistance, folding resistance, durability, and temperature resistance than traditional inorganic glass, existing transparent materials still lack energy dissipation mechanisms, making it difficult to resist repeated impact damage.
[0003] Hydrogels are a type of polymer material with a three-dimensional grid structure. In the past decade, researchers have conducted in-depth research on the problem of regulating the mechanical properties of hydrogels, and developed high-strength hydrogel systems such as double network hydrogels, nanocomposite hydrogels, topological hydrogels, and molecular microsphere composite hydrogels, achieving simultaneous improvements in strength, modulus, and toughness. By regulating the mechanical properties of hydrogels, they can be used as structural materials in medicine, engineering, and other fields. However, hydrogel materials used for transparent protection still need to meet the following basic requirements: (1) be able to maintain the stability of the material structure during impact deformation, that is, excellent mechanical properties; (2) have a visible light transmittance of more than 90% and clear imaging (high transparency); (3) be reliable under various conditions (for example, freezing or dehydration in cold or hot environments). However, the current hydrogel system still has some disadvantages, including poor structural stability (low mechanical strength and flexibility), poor transparency, and high water content (poor antifreeze and anti-dehydration properties). These factors greatly limit the application of hydrogel materials in impact-resistant transparent protection under load conditions. Therefore, developing a simple hydrogel material with tunable mechanical properties that is transparent and frost-resistant is imperative, but also extremely challenging. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a transparent antifreeze hydrogel with adjustable mechanical properties. The hydrogel prepared by the preparation method is transparent and antifreeze, and has adjustable mechanical properties.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a hydrogel, comprising the following steps:
[0007] After mixing the mixed solution of acrylic acid monomer and polyvinyl alcohol with the acid solution, adding an initiator for initiation, freezing and ablating are performed in sequence, and the freezing and ablating processes are repeated to obtain an acidic hydrogel precursor;
[0008] salting out the acidic hydrogel precursor in a salting-out agent while applying pressure to obtain the hydrogel;
[0009] The polymerization degree of the polyvinyl alcohol in the mixed solution of the acrylic acid monomer and the polyvinyl alcohol is greater than 2000.
[0010] Preferably, the polyvinyl alcohol comprises high-polymerization degree polyvinyl alcohol or ultra-high-polymerization degree polyvinyl alcohol;
[0011] The number average molecular weight of the high polymerization degree polyvinyl alcohol is 170,000 to 220,000;
[0012] The number average molecular weight of the ultra-high polymerization degree polyvinyl alcohol is 250,000 to 300,000;
[0013] The alcoholysis degree of the polyvinyl alcohol is 87% to 89%.
[0014] Preferably, the mass ratio of acrylic acid monomer to polyvinyl alcohol in the mixed solution of acrylic acid monomer and polyvinyl alcohol is 1:(1-100);
[0015] The mass ratio of the total mass of the acrylic acid monomer and the polyvinyl alcohol in the mixed solution of the acrylic acid monomer and the polyvinyl alcohol to the solvent is 1:(1-9).
[0016] Preferably, the acid solution includes hydrochloric acid, nitric acid or sulfuric acid;
[0017] The concentration of hydrogen ions in the mixed solution obtained after the mixing is 10 -7 ~2mol / L.
[0018] Preferably, the initiator comprises a photoinitiator, a thermal initiator or a radiation initiator.
[0019] Preferably, the salting-out agent is a saturated salting-out agent solution at 20-60°C;
[0020] The salt in the saturated salting-out agent solution includes one or more of sodium sulfate, magnesium sulfate, ammonium sulfate, sodium chloride, lithium chloride, calcium chloride, sodium phosphate, ammonium nitrate and lithium nitrate.
[0021] Preferably, the salting-out time is 0 min to 6 h.
[0022] Preferably, the pressure is 10 1 ~10 3 Pa pressure;
[0023] The water content of the hydrogel obtained after the pressure application is completed is 1% to 50%.
[0024] The present invention also provides a hydrogel prepared by the preparation method described in the above technical solution.
[0025] The present invention also provides application of the hydrogel described in the above technical solution in the field of transparent protective materials.
[0026] The present invention provides a method for preparing a hydrogel, comprising the following steps: mixing a mixture of acrylic acid monomer and polyvinyl alcohol with an acid solution, adding an initiator for initiation, sequentially freezing and ablating, and cycling the freezing and ablating process to obtain an acidic hydrogel precursor; applying pressure while salting out the acidic hydrogel precursor in a salting-out agent to obtain the hydrogel; the degree of polymerization of the polyvinyl alcohol in the mixture of acrylic acid monomer and polyvinyl alcohol is >2000. The present invention uses polyvinyl alcohol with a high degree of polymerization as the main chain of the graft copolymer, and the longer the polymer chain, the stronger the tensile performance of the soft phase structure, which can improve the toughness of the material; after mixing with the acid solution, the number of hydrogen bonds between hydroxyl and carboxyl, carboxyl and carboxyl, and hydroxyl and hydroxyl can be increased to improve the mechanical properties. At the same time, under the action of salting out, the binding energy between water molecules and the salting-out agent is lower, resulting in the PAA dissolved phase being a soft phase to form a "hard-soft" two-phase microstructure. At the same time, the hydrogel with adjustable mechanical properties prepared by the above method has high transparency and excellent antifreeze properties comparable to organic glass. Since the salting-out agent in the hydrogel has high saltiness, the hydrogel prepared by the present invention has good antifreeze ability, can maintain stable transparency and a long service time at low temperatures. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 3 are stress-strain curves of the hydrogels described in Example 3 and Comparative Example 1;
[0028] Figure 2 is the transmittance of the hydrogel in Example 3 in the visible light range at room temperature and after being refrigerated at -20°C for 30 hours;
[0029] Figure 3 These are stress-strain curves of the PVA / PAA-NaCl HCl hydrogel prepared in Example 2 and the PVA / PAA HCl hydrogel prepared in Comparative Example 2. DETAILED DESCRIPTION
[0030] The present invention provides a method for preparing a hydrogel, comprising the following steps:
[0031] After mixing the mixed solution of acrylic acid monomer and polyvinyl alcohol with the acid solution, adding an initiator for initiation, freezing and ablating are performed in sequence, and the freezing and ablating processes are repeated to obtain an acidic hydrogel precursor;
[0032] salting out the acidic hydrogel precursor in a salting-out agent while applying pressure to obtain the hydrogel;
[0033] The polymerization degree of the polyvinyl alcohol in the mixed solution of the acrylic acid monomer and the polyvinyl alcohol is greater than 2000.
[0034] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.
[0035] The invention mixes a mixed solution of acrylic acid monomer and polyvinyl alcohol with an acid solution, adds an initiator for initiation, and then sequentially freezes and ablates, and cycles the freezing and ablating processes to obtain an acidic hydrogel precursor.
[0036] In the present invention, the preparation of the mixed solution of the acrylic acid monomer and polyvinyl alcohol is preferably carried out under water bath conditions, after mixing polyvinyl alcohol and a solvent, adding the acrylic acid monomer. In the present invention, the temperature of the water bath is preferably 65-130°C, more preferably 90-100°C, and most preferably 95°C. In the present invention, the solvent is preferably water, more preferably deionized water. The present invention does not have any special restrictions on the mixing process, and a process well known to those skilled in the art is adopted to ensure that the polyvinyl alcohol is completely dissolved in the solvent. The present invention does not have any special restrictions on the addition of the acrylic acid monomer, and a process well known to those skilled in the art is adopted.
[0037] In the present invention, the mass ratio of the acrylic acid monomer to the polyvinyl alcohol in the mixed solution of the acrylic acid monomer and the polyvinyl alcohol is preferably 1:(1-100), more preferably 1:(20-80), and most preferably 1:(40-60). In the present invention, the mass ratio of the total mass of the acrylic acid monomer and the polyvinyl alcohol to the solvent in the mixed solution of the acrylic acid monomer and the polyvinyl alcohol is preferably 1:(1-9), more preferably 1:(2-8), and most preferably 1:(3-6).
[0038] In the present invention, the polyvinyl alcohol preferably includes high-polymerization degree polyvinyl alcohol or ultra-high-polymerization degree polyvinyl alcohol; the number average molecular weight of the high-polymerization degree polyvinyl alcohol is preferably 170,000 to 220,000; the number average molecular weight of the ultra-high-polymerization degree polyvinyl alcohol is preferably 250,000 to 300,000; the alcoholysis degree of the polyvinyl alcohol is preferably 87% to 89%.
[0039] In the present invention, the acid solution preferably includes hydrochloric acid, nitric acid or sulfuric acid; the mass concentration of the hydrochloric acid is preferably 37%; the mass concentration of the nitric acid is preferably 65%; the mass concentration of the sulfuric acid is preferably 95%; the concentration of hydrogen ions in the mixed solution obtained after mixing is preferably 10 -7 ~2mol / L, more preferably 0.5~1.5mol / L, most preferably 0.8~1.2mol / L.
[0040] The present invention does not have any special limitation on the mixing process, and the mixing process may be carried out using a process well known to those skilled in the art.
[0041] In the present invention, the initiator preferably includes a photoinitiator, a thermal initiator or a radiation initiator, and more preferably includes α-ketoglutaric acid, ammonium persulfate, potassium persulfate, sodium persulfate, 2-hydroxy-2-methyl-1-phenylpropanone, methyl benzoylformate or an alkyl iodonium salt.
[0042] After the addition of the initiator is completed, the present invention also preferably includes dissolution and defoaming at room temperature; the defoaming is preferably pouring the dissolved solution into a glass mold, vacuuming at room temperature for defoaming or standing at room temperature for defoaming; the standing time at room temperature is preferably 12 hours.
[0043] In the present invention, the mass percentage of the initiator to the acrylic monomer is preferably 0.001-1 wt %, more preferably 0.01-1 wt %, and most preferably 0.5 wt %.
[0044] In the present invention, the initiation method is preferably photoinitiation, thermal initiation or radiation initiation; the photoinitiator used in the photoinitiation is preferably one or more of α-ketoglutaric acid, hydroxycyclohexane phenone and 2-hydroxy-2-methyl-1-phenyl-1-propanone; the wavelength used in the photoinitiation is preferably ultraviolet light; the time of the photoinitiation is preferably 1~6h; the thermal initiator used in the thermal initiation is preferably one or more of azobisisobutylamidine hydrochloride, azobisisobutylimidazoline hydrochloride and ammonium persulfate; the temperature of the thermal initiation is preferably 40~60℃; the time is preferably 4~8h; the radiation source of the radiation initiation is selected from 60Co, γ rays, ions or neutrons or microwaves.
[0045] In the present invention, the freezing temperature is preferably -40 to 0°C, more preferably -30 to -10°C, and most preferably -25 to -15°C; the freezing time is preferably 12 to 72 hours, more preferably 20 to 60 hours, and most preferably 30 to 50 hours. In the present invention, the freezing can significantly enhance the strong hydrogen bonding interactions between the carboxyl groups of polyacrylic acid and the hydroxyl groups of polyvinyl alcohol, between the carboxyl groups and the carboxyl groups, and between the hydroxyl groups.
[0046] In the present invention, the ablation temperature is preferably 10-80°C, more preferably 20-70°C, and most preferably 20-60°C; the ablation time is preferably 1-12h, more preferably 3-10h, and most preferably 4-6h. In the present invention, the effect of ablation is that freeze-thaw cycle treatment can enhance hydrogen bond interactions, and low-temperature ablation can ensure that newly formed hydrogen bonds are not destroyed.
[0047] In the present invention, the number of cycles is preferably 1 to 9 times, more preferably 2 to 7 times, and most preferably 3 to 5 times.
[0048] After the acidic hydrogel precursor is obtained, the present invention applies pressure while salting out the acidic hydrogel precursor in a salting-out agent to obtain the hydrogel.
[0049] In the present invention, the salting-out agent is preferably a saturated salting-out agent solution at 20-60 ° C; the salt in the saturated salting-out agent solution includes one or more of sodium sulfate, magnesium sulfate, ammonium sulfate, sodium chloride, lithium chloride, calcium chloride, sodium phosphate, ammonium nitrate and lithium nitrate. When the salt is two or more of the above-mentioned specific selections, the present invention does not have any special restrictions on the ratio of the above-mentioned specific substances, and can be mixed in any ratio. In the present invention, the preparation of the saturated salting-out agent solution is preferably to mix salt and water to obtain a saturated salting-out agent solution. The present invention does not have any special restrictions on the mixing process, and the process well known to those skilled in the art is used to ensure that the salt is completely dissolved in water.
[0050] In the present invention, the salting-out time is preferably 0 min to 6 h, more preferably 0.5 to 4 h, and most preferably 1 to 3 h.
[0051] In the present invention, the pressure is preferably applied by covering the plate; the application is preferably applied by applying 10 1 ~10 3 Pa's pressure.
[0052] In the present invention, the water content of the hydrogel is preferably 1% to 50%, more preferably 10% to 40%, and most preferably 20% to 30%.
[0053] The present invention also provides a hydrogel prepared by the preparation method described in the above technical solution.
[0054] In the present invention, the mechanical properties of the hydrogel are adjustable, the tensile fracture stress of the hydrogel is adjustable in the range of 82-15000 kPa, the tensile modulus is adjustable in the range of 85-2500 kPa, and the dissipated energy is adjustable in the range of 0.9-54 MJ / m 3 .
[0055] The present invention also provides the application of the hydrogel described in the above technical solution in the field of transparent protective materials. In the present invention, the field of transparent protective materials is preferably bulletproof glass, anti-theft glass, special protective glass, interlayer of tempered glass, composite layer of film and substrate, bulletproof clothing, sports wrist guards or knee pads, national defense and military industry, civil commercial field or public protection field; the national defense and military industry preferably includes aviation, aerospace, navigation, ships or military high-performance bulletproof equipment; the civil commercial field preferably includes building materials, automobiles, trains or high-speed rail fields; the public protection field preferably includes escort bulletproof vehicles, military and police explosion-proof, shields, bulletproof vests, bombproof, bulletproof head covers or protective tools.
[0056] The preparation method of the transparent antifreeze hydrogel with adjustable mechanical properties provided by the present invention is described in detail below in conjunction with the examples, but they should not be construed as limiting the scope of protection of the present invention.
[0057] Example 1
[0058] Under 95°C water bath conditions, 1g of polyvinyl alcohol (PVA) powder (PVA-224, degree of polymerization of 2400, molecular weight of 200,000) was dissolved in 70mL of deionized water, and then 29g of acrylic acid monomer (AA) was added, and sulfuric acid solution (mass concentration of 95%) was added dropwise to make the hydrogen ion concentration reach 1mol / L, and then 0.135g of α-ketoglutaric acid was added and dissolved evenly at room temperature of 37°C. The prepared solution was poured into a glass mold, and after vacuum defoaming at room temperature, it was placed under an ultraviolet lamp (wavelength of 365nm) for 6h, and then placed in a -20°C environment for freezing for 30h, and then ablated at 25°C for 5h. The above freezing and ablation process was repeated 3 times to obtain an acidic hydrogel precursor;
[0059] The acidic hydrogel precursor was placed in a 100 mL volumetric flask, and 100 g of sodium nitrate was dissolved in deionized water at 25° C. to obtain a saturated sodium nitrate solution;
[0060] The acidic hydrogel precursor is placed in the saturated sodium nitrate solution, the pressure applied to the hydrogel precursor material per unit area is 50 Pa, and it is immersed at 60° C. for 4 hours to obtain a hydrogel (denoted as PVA / PAA-NaNO3H2SO4hydrogel).
[0061] Example 2
[0062] Under 95°C water bath conditions, 15g of polyvinyl alcohol (PVA) powder (PVA-235, degree of polymerization of 3500, molecular weight of 300,000) was dissolved in 70mL of deionized water, and then 5g of acrylic acid monomer (AA) was added, and hydrochloric acid solution (mass concentration of 37%) was added dropwise to make the hydrogen ion concentration reach 1mol / L, and then 0.135g of alkyl iodonium salt was added and dissolved evenly at room temperature of 37°C. The prepared solution was poured into a glass mold, and after standing at room temperature for 12h to completely defoam, it was placed under an ultraviolet lamp (wavelength of 365nm) for 6h, and then frozen at -20°C for 30h, and then ablated at 25°C for 5h. The above freezing and ablation process was repeated 3 times to obtain an acidic hydrogel precursor;
[0063] The acidic hydrogel precursor was placed in a 100 mL volumetric flask, and 56 g of sodium chloride was dissolved in deionized water at 25° C. to obtain a saturated sodium chloride solution;
[0064] The acidic hydrogel precursor is placed in the saturated sodium chloride solution, the pressure applied to the hydrogel precursor material per unit area is 500Pa, and it is immersed at 25°C for 2 hours to obtain a hydrogel. (Recorded as PVA / PAA-NaCl HClhydrogel)
[0065] Example 3
[0066] Under 95°C water bath conditions, 1g of polyvinyl alcohol (PVA) powder (PVA-224, degree of polymerization of 2400, molecular weight of 200,000) was dissolved in 70mL of deionized water, and then 29g of acrylic acid monomer (AA) was added. After sulfuric acid solution was added dropwise to make the hydrogen ion concentration reach 1mol / L, 0.135g of α-ketoglutaric acid was added and dissolved evenly at room temperature of 37°C. The prepared solution was poured into a glass mold, and after vacuum defoaming at room temperature, it was placed under an ultraviolet lamp (wavelength of 365nm) for 6h, and then frozen at -20°C for 30h, and then ablated at 25°C for 5h. The above freezing and ablation process was repeated 3 times to obtain an acidic hydrogel precursor.
[0067] The acidic hydrogel precursor was placed in a 100 mL volumetric flask, and 550 g of lithium chloride was dissolved in deionized water at 25° C. to obtain a saturated lithium chloride solution;
[0068] The acidic hydrogel precursor is placed in the saturated lithium chloride solution, a pressure of 50 Pa is applied to the hydrogel precursor material per unit area, and the solution is immersed at 60° C. for 4 hours to obtain a hydrogel (denoted as PVA / PAA-LiCl H2SO4 hydrogel).
[0069] Figure 2is the transmittance of the hydrogel in the visible light range at room temperature and after being refrigerated at -20°C for 30 hours, Figure 2 It can be seen that the gel has good antifreeze properties, maintaining a transmittance of more than 90% in the visible light wavelength range at room temperature and low temperature. This is due to the presence of high concentrations of salt ions, which prevents the water in the gel from crystallizing due to temperature drops.
[0070] Comparative Example 1
[0071] Referring to Example 1, except that no sulfuric acid solution was added, a hydrogel (denoted as PVA / PAA-LiCl hydrogel) was obtained.
[0072] Figure 1 The stress-strain curves of the hydrogels described in Example 3 and Comparative Example 1 (where Ⅰ is PVA / PAA-LiCl hydrogel, and Ⅱ is PVA / PAA-LiCl- 1 mol / L H2SO4 hydrogel rapidly prepared in this patent) are shown in FIG. Figure 1 It can be seen that the mechanical properties of the hydrogel described in Example 3 are more excellent, especially the elastic modulus is increased from 1 MPa to 3 MPa.
[0073] Comparative Example 2
[0074] Referring to Example 2, the difference is that no hydrochloric acid solution is added to obtain a hydrogel (denoted as PVA / PAA HClhydrogel);
[0075] Figure 3 The stress-strain curves of the PVA / PAA-NaCl HCl hydrogel prepared in Example 2 and the PVA / PAA HCl hydrogel prepared in Comparative Example 2 are shown in FIG. Figure 3 It can be seen that the mechanical properties of PVA / PAA-NaCl HCl hydroge are better than those of PVA / PAA HCl hydrogel, especially the fracture stress is increased from 1.8MPa to 7MPa.
[0076] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a hydrogel, characterized in that: The following steps are involved: After mixing the mixed solution of acrylic acid monomer and polyvinyl alcohol with the acid solution, adding an initiator for initiation, freezing and ablating are performed in sequence, and the freezing and ablating processes are repeated to obtain an acidic hydrogel precursor; salting out the acidic hydrogel precursor in a salting-out agent while applying pressure to obtain the hydrogel; The degree of polymerization of polyvinyl alcohol in the mixed solution of acrylic acid monomer and polyvinyl alcohol> 2000; The acid solution includes hydrochloric acid, nitric acid or sulfuric acid; The concentration of hydrogen ions in the mixed solution obtained after the mixing is 10 -7 ~2mol / L; The salting-out agent is a saturated salting-out agent solution at 20-60° C.; the salt in the saturated salting-out agent solution includes sodium nitrate or potassium chloride.
2. The preparation method according to claim 1, characterized in that The polyvinyl alcohol includes high-polymerization degree polyvinyl alcohol or ultra-high-polymerization degree polyvinyl alcohol; The number average molecular weight of the high polymerization degree polyvinyl alcohol is 170,000 to 220,000; The number average molecular weight of the ultra-high polymerization degree polyvinyl alcohol is 250,000 to 300,000; The alcoholysis degree of the polyvinyl alcohol is 87% to 89%.
3. The preparation method according to claim 1, characterized in that: The mass ratio of the acrylic acid monomer to the polyvinyl alcohol in the mixed solution of the acrylic acid monomer and the polyvinyl alcohol is 1:(1-100); The mass ratio of the total mass of the acrylic acid monomer and the polyvinyl alcohol in the mixed solution of the acrylic acid monomer and the polyvinyl alcohol to the solvent is 1:(1-9).
4. The preparation method according to claim 1, characterized in that: The initiator includes a photoinitiator, a thermal initiator or a radiation initiator.
5. The preparation method according to claim 1, characterized in that: The salting-out time is 0 min to 6 h.
6. The preparation method according to claim 1, characterized in that: The pressure is 10 1 ~10 3 Pa pressure; The water content of the hydrogel obtained after the pressure application is completed is 1% to 50%.
7. The hydrogel prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the hydrogel according to claim 7 in the field of transparent protective materials.
Citation Information
Patent Citations
Preparation method and application of high-strength oriented polyvinyl alcohol hydrogel