A method for preparing a surface hardened layer of zirconium and zirconium alloy

By forming an oxygenated layer and a tetrahedral amorphous carbon coating on the surface of zirconium and zirconium alloy materials, the problem of insufficient hardness and wear resistance of zirconium alloy materials is solved, higher surface hardness and corrosion resistance are achieved, and extended extended service life.

CN118547243BActive Publication Date: 2024-10-11XIAN PUMP & VALVE GENERAL FACTORY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411008396.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-11
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

Zirconium and zirconium alloy materials have low surface hardness and poor wear resistance, which results in the hardened layer not being dense enough in strong corrosion and heavy load environments, making it difficult to achieve stable applications.

Method used

ZrO2 powder is used to cover, heat and oxygenate to form an oxygenation layer, followed by diffusion of oxygen elements, and magnetron sputtering of a tetrahedral amorphous carbon coating. The temperature and holding time are adjusted to remove material stress and form a thicker hardened layer.

Benefits of technology

It significantly improves the surface hardness and corrosion resistance of zirconium and zirconium alloy materials, extends the service life under extreme working conditions, improves the bonding effect of each layer of materials and reduces the friction coefficient.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118547243B_ABST
    Figure CN118547243B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of metal plating, and relates to a method for preparing a surface hardened layer of zirconium and zirconium alloys. The present invention provides a method for preparing a surface hardened layer of zirconium and zirconium alloys, which first heats and oxygenates, then diffuses the oxygen element, and finally magnetron sputters a tetrahedral amorphous carbon coating to obtain a composite hardened layer on the surface of zirconium and zirconium alloys. The preparation method provided by the present invention enables the plated oxygen-permeated layer and the tetrahedral amorphous carbon layer to have good bonding with the zirconium and zirconium alloy substrate, so that each level of film layer has a higher surface hardness and good corrosion resistance. In harsh working conditions, the product will not fail due to problems with a single hardened layer, and has extremely strong stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal plating and relates to a method for preparing a surface hardening layer of zirconium and zirconium alloy. Background Art

[0002] Zirconium and zirconium alloys have moderate density, are resistant to most inorganic acids, organic acids, strong alkalis and molten salts, have excellent corrosion resistance, and have good comprehensive mechanical properties. They are widely used in the chemical industry. However, due to the low hardness, poor wear resistance and easy bite of zirconium materials, the surface of the zirconium ball valve ball often wears, affecting its functional use. Therefore, improving the surface hardness of zirconium or zirconium alloy materials and enhancing their wear resistance are of great significance to extending their service life and stable operation.

[0003] At present, the surface hardening of zirconium or zirconium alloy materials mainly adopts a single treatment method, such as heating oxidation, thermal spraying or surface sputtering coating. Heating oxidation or thermal spraying is a common method for surface hardening of zirconium or zirconium alloy materials. However, for strong corrosive environments, it is difficult for the sprayed layer to achieve the same corrosion resistance as the parent material; for heavy loads and strong particle wear environments, the hardened layer produced by existing oxygen permeation is not dense enough, and the thin hardened layer thickness cannot achieve stable application. Tetrahedral amorphous carbon (TAC) coating is a hydrogen-free DLC (diamond-like carbon) coating. Its film layer can reach more than 85% (diamond) SP3 bond content, with extremely high hardness, extremely low friction coefficient, high elastic modulus, wide light transmittance range, good chemical inertness and other advantages. Its physical and chemical properties are similar to those of diamond. Tetrahedral amorphous carbon coating is mainly used for the performance of automotive engine parts, and has the characteristics of high melting point, high oxidation resistance and good chemical corrosion resistance. However, the thickness of tetrahedral amorphous carbon coating is small, and it will cause the coating to crack when it exceeds a certain thickness. Summary of the invention

[0004] The object of the present invention is to solve at least one of the above-mentioned technical problems. By using it, a thicker hardened layer can be prepared on the surface of zirconium and zirconium alloys in a simple and low-cost manner. To this end, the present invention provides a method for preparing a hardened layer on the surface of zirconium and zirconium alloys to solve this need in the art.

[0005] The present invention provides a method for preparing a surface hardened layer of zirconium and zirconium alloy, which comprises:

[0006] A substrate, wherein the substrate is zirconium or a zirconium alloy;

[0007] The substrate is covered with ZrO2 powder, heated and oxygenated, oxygen element is diffused to form an oxygenated layer, and finally a tetrahedral amorphous carbon coating is magnetron sputtered;

[0008] The temperature of the heating oxygenation is 600-800°C, and the oxygenation time is 3-5h;

[0009] The temperature of oxygen diffusion is 400-550°C, and the insulation time is 10-24h;

[0010] The coating temperature of the magnetron sputtering is 80-200°C.

[0011] Furthermore, in the method for preparing the surface hardened layer of zirconium and zirconium alloy provided by the present invention, the purity of the ZrO2 powder is not less than 99.5wt%, and the powder particle size is 100 mesh.

[0012] Furthermore, in the method for preparing the surface hardened layer of zirconium and zirconium alloy provided by the present invention, the diffusion of oxygen element is carried out under vacuum conditions.

[0013] Furthermore, in the method for preparing the surface hardened layer of zirconium and zirconium alloy provided by the present invention, before the magnetron sputtering, the oxygen-permeated layer and deformation generated by heating oxygenation are removed. In the method for preparing the surface hardened layer of zirconium and zirconium alloy provided by the present invention, the thickness of the oxygen-permeated layer on the surface is 30-60 μm.

[0014] Furthermore, in the method for preparing the surface hardened layer of zirconium and zirconium alloy provided by the present invention, the magnetron sputtering comprises: evacuating to a vacuum degree of less than 3×10 -4 Pa, and then an inert gas with a gas flow rate of 1000~3000sccm was introduced, and a tetrahedral amorphous carbon coating was magnetron sputtered using a graphite C target.

[0015] Furthermore, in the method for preparing the surface hardened layer of zirconium and zirconium alloy provided by the present invention, the inert gas is Ar gas;

[0016] The purity of the graphite C target is not less than 99.999wt%.

[0017] On the other hand, the present invention relates to a zirconium and zirconium alloy material containing a surface hardened layer, wherein the zirconium and zirconium alloy material is prepared by the preparation method.

[0018] Furthermore, in the zirconium and zirconium alloy materials containing a surface hardened layer provided by the present invention, the zirconium and zirconium alloy materials are spheres with a roundness of less than 0.02 mm.

[0019] Furthermore, in the zirconium and zirconium alloy materials containing a surface hardening layer provided by the present invention, the thickness of the oxygen permeation layer is 0.15-0.25 mm, and the thickness of the tetrahedral amorphous carbon coating is 2-6 μm.

[0020] Furthermore, in the zirconium and zirconium alloy material containing a surface hardened layer provided by the present invention, the hardness of the oxygen-permeated layer is not less than 900 HV0.1 The hardness of the tetrahedral amorphous carbon coating is not less than 2500 HV 0.1 ; In the zirconium and zirconium alloy materials, the hardness of the substrate, the oxygen-permeated layer, and the tetrahedral amorphous carbon coating increases in sequence.

[0021] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects or advantages:

[0022] The purpose of the present invention is to prepare a hardened layer on the surface of zirconium and zirconium alloy materials, improve the surface hardness, corrosion resistance and product service life under extreme working conditions. To this end, the present invention first prepares an oxygen-permeated layer on the surface of zirconium and zirconium alloy materials, and then prepares a tetrahedral amorphous carbon coating to achieve a hardened layer with a relatively large thickness plated on the surface of zirconium and zirconium alloy materials. The present invention further adjusts the reaction temperature or insulation temperature of heated oxygen permeation, oxygen element diffusion and magnetron sputtering. By adjusting the reaction temperature, the material stress is fully removed to avoid deformation of the substrate, and it has the effects of improving the bonding effect of each layer of material, reducing the friction coefficient, and improving the surface hardness. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 This is a photo of oxygen permeation layer thickness detection.

[0025] Figure 2 This is a photo of PVD coating layer thickness detection. DETAILED DESCRIPTION

[0026] The technical scheme of the present invention is described below in conjunction with the examples, but the present invention is not limited to the following examples. The experimental methods and detection methods described in each example are conventional methods unless otherwise specified; the reagents and materials are commercially available unless otherwise specified. The "%" indicates mass percentage unless otherwise specified.

[0027] Example 1

[0028] This embodiment takes a DN25 R60702 industrial pure zirconium ball valve ball as an example, and forms a hardened layer on its surface.

[0029] Step 1: Prepare the DN25 R60702 industrial pure zirconium ball valve ball by machining. The outer diameter of the ball is 0.2 mm larger than the final size. Then, the ball is ultrasonically cleaned with acetone and blown dry.

[0030] Step 2: Place the sphere in ZrO2 powder and cover it completely; the ZrO2 powder has a purity of 99.5% and a powder size of 100 mesh. Place it in an ordinary resistance furnace for heating and oxygenation. The heating and oxygenation temperature is 600°C and the oxygenation time is 3 hours.

[0031] Step 3: Place the oxygen-infiltrated sphere in a vacuum resistance furnace for oxygen diffusion. The diffusion heating temperature is 400°C and the temperature is kept for 10 hours.

[0032] Step 4: Grind the sphere after oxygen diffusion to remove the loose oxygen-permeated layer and deformation on the surface and ensure the finished size of the sphere, with a roundness of less than 0.02 mm. Figure 1 This is a photo of oxygen permeation layer thickness detection.

[0033] Step 5: Use magnetron sputtering equipment to first evacuate to a vacuum degree of 2×10 -4 Pa, and then Ar gas is introduced with a gas flow rate of 1000sccm. A high-purity graphite C target is used with a purity of 99.999%. The coating temperature is 80℃. After the coating is completed, the furnace is cooled to below 100℃ and then taken out of the furnace and air-cooled to room temperature. The thickness of the obtained tetrahedral amorphous carbon coating is 2μm. Figure 2 This is a photo of PVD coating layer thickness detection.

[0034] Example 2

[0035] This embodiment takes a DN80 R60705 zirconium alloy ball valve ball as an example, and forms a hardened layer on its surface.

[0036] Step 1: Prepare the DN80 R60705 zirconium alloy ball valve ball by machining. The outer diameter of the ball is 0.5 mm larger than the final size. Then, the ball is ultrasonically cleaned with acetone and blown dry.

[0037] Step 2: Place the sphere in ZrO2 powder and cover it completely; the ZrO2 powder has a purity of 99.5% and a powder size of 100 mesh. Place it in an ordinary resistance furnace for heating and oxygenation. The heating and oxygenation temperature is 700°C and the oxygenation time is 4 hours.

[0038] Step 3: Place the oxygen-infiltrated sphere in a vacuum resistance furnace for oxygen diffusion. The diffusion heating temperature is 500°C and the temperature is kept for 18 hours.

[0039] Step 4: Grind the sphere after oxygen diffusion to remove the loose oxygen-permeated layer and deformation on the surface and ensure the finished size of the sphere, with a roundness of less than 0.02 mm.

[0040] Step 5: Use magnetron sputtering equipment to first evacuate to a vacuum degree of 1.5×10 -4Pa, and then Ar gas is introduced with a gas flow rate of 2000sccm. A high-purity graphite C target is used with a purity of 99.999%. The coating temperature is 140℃. After the coating is completed, the furnace is cooled to below 100℃ and then taken out of the furnace and air-cooled to room temperature. The thickness of the obtained tetrahedral amorphous carbon coating is 4μm.

[0041] Example 3

[0042] This embodiment takes a DN125 R60702 zirconium alloy ball valve ball as an example, and forms a hardened layer on its surface.

[0043] Step 1: Prepare the DN125 R60702 zirconium alloy ball valve ball by machining. The outer diameter of the ball is 0.8 mm larger than the final size. Then, the ball is ultrasonically cleaned with acetone and blown dry.

[0044] Step 2: Place the sphere in ZrO2 powder and cover it completely; the purity of ZrO2 powder is 99.8%, the powder size is 100 mesh, and it is placed in an ordinary resistance furnace for heating and oxygenation. The heating and oxygenation temperature is 800℃ and the oxygenation time is 5h.

[0045] Step 3: Place the oxygen-infiltrated sphere in a vacuum resistance furnace for oxygen diffusion at a diffusion heating temperature of 550°C for 24 hours.

[0046] Step 4: Grind the sphere after oxygen diffusion to remove the loose oxygen-permeated layer and deformation on the surface and ensure the finished size of the sphere, with a roundness of less than 0.02 mm.

[0047] Step 5: Use magnetron sputtering equipment to first evacuate to a vacuum degree of 1×10 -4 Pa, and then Ar gas is introduced with a gas flow rate of 3000sccm. A high-purity graphite C target is used with a purity of 99.999%. The coating temperature is 180℃. After the coating is completed, the furnace is cooled to below 100℃ and then taken out of the furnace and air-cooled to room temperature. The thickness of the obtained tetrahedral amorphous carbon coating is 6μm.

[0048] Comparative Example 1

[0049] This comparative example is the same as Example 1, except that the coating temperature during magnetron sputtering is room temperature.

[0050] Comparative Example 2

[0051] This comparative example is the same as Example 1, except that the oxygenation steps in Step 2 and Step 3 are replaced by those in Example 1 in CN104818449A.

[0052] Comparative Example 3

[0053] This comparative example is the same as Example 1, except that the oxygen permeation steps of step 2 and step 3 are not performed, and magnetron sputtering is directly performed.

[0054] Comparative Example 4

[0055] This comparative example is the same as Example 1, except that the heating temperature in step 3 is 650°C.

[0056] Test Case

[0057] This test example provides a performance test of zirconium and zirconium alloy materials containing a surface hardened layer produced by the above method.

[0058] Table 1: Basic performance parameters

[0059]

[0060] The zirconium and zirconium alloy materials with surface hardening layer prepared by the above method were subjected to corrosion resistance test, and the corrosion test was carried out for 100 hours in 1.8% dimethyl phosphine + 18% sodium chloride + 1.5% disodium hydrogen phosphate + distilled water medium at a temperature of 250°C and a pressure of 15MPa. After the corrosion test, the friction coefficient test was carried out. After the corrosion test, the sealing test was carried out after 3000 switches at room temperature and an air pressure of 0.6MPa. After disassembly, the surface of the sphere was observed for scratches. The test results are shown in Table 2.

[0061] Table 2: Test results

[0062]

[0063] As can be seen from Table 2, the present invention provides a method for preparing a surface hardened layer of zirconium and zirconium alloys. An oxygen permeation layer is first prepared on the surface of the zirconium and zirconium alloy material, and then a tetrahedral amorphous carbon coating is prepared to achieve a hardened layer with a relatively large thickness coated on the surface of the zirconium and zirconium alloy material. The hardened layer has an extremely low corrosion rate and friction coefficient, and as a valve body, it still has good sealing performance under extreme working conditions.

[0064] As described above, the basic principle, main features and advantages of the present invention are well described. The above embodiments and descriptions are only descriptions of the preferred implementation modes of the present invention, and the present invention is not limited by the above embodiments. Without departing from the spirit and scope of the present invention, various changes and improvements made by ordinary technicians in this field to the technical solution of the present invention should fall within the protection scope determined by the present invention.

Claims

1. A method for preparing a surface hardened layer of zirconium and zirconium alloys, characterized in that: include: A substrate, wherein the substrate is zirconium or a zirconium alloy; The substrate is covered with ZrO2 powder, heated and oxygenated, oxygen element is diffused to form an oxygenated layer, and finally a tetrahedral amorphous carbon coating is magnetron sputtered; The temperature of the heating oxygenation is 600-800°C, and the oxygenation time is 3-5h; The temperature of oxygen diffusion is 400-550°C, and the insulation time is 10-24h; The coating temperature of the magnetron sputtering is 80-200°C.

2. The method for preparing a surface hardened layer of zirconium and zirconium alloy according to claim 1, characterized in that: The purity of the ZrO2 powder is not less than 99.5wt%, and the powder particle size is 100 mesh.

3. The method for preparing a surface hardened layer of zirconium and zirconium alloy according to claim 1, characterized in that: The oxygen element diffusion is performed under vacuum conditions.

4. The method for preparing a surface hardened layer of zirconium and zirconium alloy according to claim 1, characterized in that: Before the magnetron sputtering, the loose oxygen-infiltrated layer and deformation amount on the surface generated by heating oxygen-infiltrated are removed.

5. The method for preparing a surface hardened layer of zirconium and zirconium alloy according to claim 1, characterized in that: The magnetron sputtering comprises: evacuating to a vacuum degree of less than 3×10 -4 Pa, and then an inert gas with a gas flow rate of 1000~3000sccm was introduced, and a tetrahedral amorphous carbon coating was magnetron sputtered using a graphite C target.

6. The method for preparing a surface hardened layer of zirconium and zirconium alloy according to claim 5, characterized in that: The inert gas is Ar gas; The purity of the graphite C target is not less than 99.999wt%.

7. A zirconium or zirconium alloy material containing a surface hardened layer, characterized in that: The zirconium and zirconium alloy materials are prepared by the preparation method described in any one of claims 1 to 6.

8. The zirconium and zirconium alloy material according to claim 7, characterized in that: The zirconium and zirconium alloy materials are spheres with a roundness less than 0.02 mm.

9. The zirconium and zirconium alloy material according to claim 7, characterized in that: The thickness of the oxygen permeation layer is 0.15-0.25 mm, and the thickness of the tetrahedral amorphous carbon coating is 2-6 μm.

10. The zirconium and zirconium alloy material according to claim 7, characterized in that: The hardness of the oxygen permeable layer is not less than 900HV 0.1 The hardness of the tetrahedral amorphous carbon coating is not less than 2500 HV 0.1 ; In the zirconium and zirconium alloy materials, the hardness of the substrate, the oxygen-permeated layer, and the tetrahedral amorphous carbon coating increases in sequence.