A method for preparing nano polyphenylene sulfide fiber

Through the blend granulation and melt spinning technology of thermodynamic incompatible alkali-soluble polyester and polyphenylene sulfide, the difficulty in preparing nano-grade fibers and pollution problems in the existing technology is solved, and stable and efficient nano-polyphenylene sulfide is achieved. Ether fiber preparation, suitable for a variety of application fields.

CN118547397BActive Publication Date: 2024-11-22DONGHUA UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410995580.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-22
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

It is difficult to effectively prepare nano-grade polyphenylene sulfide fibers in the prior art, and traditional methods require organic solvents to cause contamination, and the fiber diameter distribution is uneven and is not suitable for large-scale production.

Method used

Thermodynamically incompatible alkali-soluble polyester and polyphenylene sulfide are used to mix and granulate, and the alkali-soluble polyester is removed by melt spinning and dissolving it in alkali solution to prepare nano-grade polyphenylene sulfide fibers, using low temperature co-collect Mix granulation and adjust the mass fraction of polyphenylene sulfide to control the fiber diameter distribution.

Benefits of technology

It has achieved stable, efficient and environmentally friendly nanopolyphenylene sulfide fiber preparation, with controllable fiber diameter and narrow diameter distribution, and is suitable for battery separators, electrolytic water separators, air purification filter materials and composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118547397B_ABST
    Figure CN118547397B_ABST
Patent Text Reader

Abstract

The present invention relates to a preparation method of nano polyphenylene sulfide fiber, comprising uniformly mixing alkali-soluble polyester and polyphenylene sulfide, blending and granulating to obtain a blended masterbatch; wherein the average particle size of the alkali-soluble polyester is 1-5 mm; the average particle size of the polyphenylene sulfide is 50-1000 μm; the blending and granulating temperature is 245-275° C.; then the blended masterbatch and the alkali-soluble polyester are uniformly mixed, melt-spinned, drawn and heat-set, and the alkali-soluble polyester is dissolved and removed to obtain the nano polyphenylene sulfide fiber. The present invention adopts a low-temperature blending and granulating method, while ensuring that the polyphenylene sulfide is uniformly dispersed in the alkali-soluble polyester, the degradation of the alkali-soluble polyester is minimized. The nano polyphenylene sulfide fiber obtained based on this preparation method has the characteristics of controllable fiber diameter, narrow fiber diameter distribution, and easy dispersion, which provides a practical technical route for the large-scale preparation of nano polyphenylene sulfide fibers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of nanofibers, and in particular relates to a method for preparing nano polyphenylene sulfide fibers. Background Art

[0002] Polyphenylene sulfide fiber is a high-performance fiber with excellent high temperature resistance and chemical corrosion resistance. Its glass transition temperature is 85°C and its melting point is 285°C. The long-term use temperature of polyphenylene sulfide fiber can reach above 200°C, and the limiting oxygen index is 36, which has good flame retardancy. It can be used in special harsh environments such as high temperature and strong corrosion. Nano polyphenylene sulfide fiber refers to polyphenylene sulfide fiber with a fiber diameter of less than 1μm. Compared with traditional micron-level ultrafine polyphenylene sulfide fibers, nano polyphenylene sulfide fibers have a higher specific surface area and have very broad application prospects in many fields such as energy and environment.

[0003] The melt blending phase separation method is a method for preparing nanofibers with scalable prospects. That is, two polymers with different viscosities are blended and spun in a certain proportion. The polymer with high viscosity and small proportion will spontaneously form "islands" due to poor fluidity, and the polymer with low viscosity and large proportion will spontaneously form a "sea" due to good fluidity. The final nanofibers are obtained by dissolving and removing the "sea" component. This method is also called the indefinite island sea method. Compared with the traditional fixed island sea method, the fiber diameter obtained is smaller, but the diameter distribution is often larger. Finding two blended polymers with suitable spinning temperature and viscosity difference is the key to realizing this technology, especially for polyphenylene sulfide that requires high-temperature processing.

[0004] The invention patent of China Patent Publication No. CN103409847A discloses "a method for preparing polyphenylene sulfide ultrafine fiber" and the invention patent of China Patent Publication No. CN103774277A discloses "a method for preparing polyphenylene sulfide ultrafine fiber and its preparation method". The two methods respectively select polyamide and polyolefin and polyphenylene sulfide for blending and spinning to prepare polyphenylene sulfide ultrafine fiber. Both methods require organic solvent for fiber opening treatment, which will cause great pollution, and the fiber diameter distribution is wide, the fiber diameter is uncontrollable, and the conditions for large-scale production of nano polyphenylene sulfide fiber are not met.

[0005] The invention patent with Chinese patent publication number CN113151930A discloses "island-type polyphenylene sulfide ultrafine fibers and preparation methods thereof". This method adopts a method of directly mixing and spinning alkali-soluble polyester particles and polyphenylene sulfide particles blended with different viscosities to prepare ultrafine polyphenylene sulfide fibers. The average diameter of the prepared fibers cannot reach the nanometer level, and the fiber diameter distribution is wide, and it does not have the ability to stably produce a large amount of nano polyphenylene sulfide fibers. Summary of the invention

[0006] In view of the defects of the prior art, the technical problem to be solved by the present invention is to provide a method for preparing nano-polyphenylene sulfide fibers, and in particular to a stable, efficient and environmentally friendly method for preparing nano-polyphenylene sulfide fibers.

[0007] The present invention provides a method for preparing nano polyphenylene sulfide fiber, comprising:

[0008] S1: mixing thermodynamically incompatible alkali-soluble polyester and polyphenylene sulfide, blending and granulating to obtain a blended masterbatch of alkali-soluble polyester and polyphenylene sulfide; the average particle size of the alkali-soluble polyester in step S1 is 1-5 mm; the average particle size of the polyphenylene sulfide is 50-1000 μm; the blending and granulating temperature is 245-275° C.;

[0009] S2: mixing the blended masterbatch and the alkali-soluble polyester, performing melt spinning, drawing and heat setting, and obtaining alkali-soluble polyester and polyphenylene sulfide blended fibers;

[0010] S3: Soaking the blended fibers in an alkaline solution to dissolve and remove the alkali-soluble polyester to obtain nano-polyphenylene sulfide fibers.

[0011] The mixing in steps S1 and S2 is performed by placing the mixture in a high-speed mixer and mixing it uniformly.

[0012] Preferably, the alkali-soluble polyester in steps S1 and S2 is dried alkali-soluble polyester; wherein the drying temperature is 80-160°C, and the time is 12-20 hours; wherein the drying method is blast drying; the polyphenylene sulfide in step S1 is dried polyphenylene sulfide; wherein the drying temperature is 80-170°C, and the time is 10-24 hours; wherein the drying method is vacuum drying.

[0013] More preferably, the drying temperature of the alkali-soluble polyester particles in steps S1 and S2 is 80-140° C., and the drying time is 12-16 hours. The drying temperature of the polyphenylene sulfide powder in step S1 is 120-160° C., and the drying time is 12-16 hours.

[0014] Preferably, in step S1, the average particle size of the alkali-soluble polyester is 1-3 mm; the average particle size of the polyphenylene sulfide is 50-600 μm.

[0015] In the step S1, the alkali-soluble polyester is alkali-soluble polyester particles; and the polyphenylene sulfide is polyphenylene sulfide powder.

[0016] Preferably, the mass percentage of polyphenylene sulfide in the blended masterbatch in step S1 is 30-80wt%.

[0017] Further preferably, the mass percentage of polyphenylene sulfide in the blended masterbatch in step S1 is 40-60wt%.

[0018] Preferably, a twin-screw extruder is used for the blending and granulation in step S1.

[0019] More preferably, the temperature of the blending and granulation in step S1 is 250-270°C.

[0020] Preferably, the blended masterbatch in step S2 is a dried blended masterbatch; wherein the drying temperature is 80-160° C., and the time is 14-24 hours; wherein the drying method is air drying followed by vacuum drying.

[0021] Further preferably, the drying temperature of the blended masterbatch in step S2 is 100-140° C., and the drying time is 14-18 hours.

[0022] Preferably, in the step S2, the melt spinning temperature is 295-330°C, and the winding speed is 100-1000m / s; the melt spinning adopts a single-screw melt spinning machine; the stretching and heat setting process parameters are: the stretching temperature is 60-100°C, the heat setting temperature is 100-160°C, and the stretching multiple is 2-5 times.

[0023] Further preferably, in step S2, the melt spinning temperature is 295-315°C; the melt spinning winding speed is 100-500m / s; the drawing temperature of the blended fiber is 70-90°C, the heat setting temperature is 120-140°C, and the drawing multiple is 3-4 times.

[0024] Preferably, the alkali-soluble polyester in step S2 is alkali-soluble polyester particles; the average particle size of the alkali-soluble polyester is 1-5 mm.

[0025] Preferably, in step S2, the mass fraction of polyphenylene sulfide in the blended fibers is 10-40wt%.

[0026] Further preferably, in step S2, the mass fraction of polyphenylene sulfide in the blended fibers is 10-30wt%.

[0027] Preferably, the alkali in the alkali solution in step S3 is at least one of NaOH and KOH; the concentration of the alkali solution is 4-10wt%; and the bath-solid ratio (mass ratio) of the alkali solution to the blended fiber is 100-30:1.

[0028] Further preferably, the concentration of the alkali solution in step S3 is 6-8wt%; and the bath-solid ratio (mass ratio) of the alkali solution to the blended fiber is 100-50:1.

[0029] Preferably, in step S3, the blended fibers are immersed in an alkaline solution at a dissolving temperature of 60-100° C. and a dissolving time of 0.5-2 h.

[0030] More preferably, in step S3, the dissolution temperature is 80-100° C. and the dissolution time is 0.5-1 h.

[0031] The invention provides a nano polyphenylene sulfide fiber prepared by the method. The average diameter of the nano polyphenylene sulfide fiber is 200-800nm, the diameter distribution of the nano polyphenylene sulfide fiber is narrow, and the standard deviation is less than 150nm.

[0032] The invention provides an application of the nano polyphenylene sulfide fiber in the fields of battery diaphragms, water electrolysis diaphragms, air purification filter materials and composite materials.

[0033] The preparation method of the nano polyphenylene sulfide fiber of the present invention comprises the processes of blending alkali-soluble polyester and polyphenylene sulfide into granules, spinning, drawing, winding, fiber opening, etc. The present invention adopts a low-temperature blending and granulation method to minimize the degradation of the alkali-soluble polyester while ensuring that the polyphenylene sulfide is uniformly dispersed in the alkali-soluble polyester. The nano polyphenylene sulfide fiber obtained by the preparation method has the characteristics of controllable fiber diameter, narrow fiber diameter distribution, and easy dispersion, and provides a practical technical route for the large-scale preparation of nano polyphenylene sulfide fibers.

[0034] Beneficial Effects

[0035] The present invention provides a method for preparing a nano polyphenylene sulfide fiber, wherein alkali-soluble polyester particles and polyphenylene sulfide powder with a smaller particle size are blended to prepare a master batch at a temperature below the melting point of polyphenylene sulfide, and then the blended master batch is mixed with the alkali-soluble polyester particles and melt-spinned. The method adopts the polyphenylene sulfide powder with a smaller particle size for blending and granulation, which significantly improves the dispersion size and uniformity of the polyphenylene sulfide melt in the alkali-soluble polyester melt during the melt spinning process, so that the obtained nano polyphenylene sulfide fiber has a small diameter and a narrow distribution. This blending and granulation method below the melting point of polyphenylene sulfide can greatly reduce the degradation problem of alkali-soluble polyester at high temperature to ensure the smooth progress of subsequent spinning. In addition, the diameter of the nano fiber can be easily regulated by regulating the mass fraction of polyphenylene sulfide in the blended fiber. The alkali-soluble polyester can be dissolved in alkali solution, avoiding the use of organic solvents, which provides conditions for the large-scale green preparation of nano polyphenylene sulfide fibers.

[0036] The preparation method of the invention is suitable for preparing nano polyphenylene sulfide fibers, and the prepared nano polyphenylene sulfide fibers are suitable for preparing battery diaphragms, water electrolysis diaphragms, air purification filter materials, composite materials and many other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a scanning electron microscope image of the nano polyphenylene sulfide fiber prepared in Example 1 of the present invention;

[0038] Figure 2This is a scanning electron microscope image of the nano polyphenylene sulfide fiber prepared in Example 2 of the present invention;

[0039] Figure 3 This is a scanning electron microscope image of the nano-polyphenylene sulfide fiber prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0040] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0041] Example 1

[0042] S1: Weigh 50 parts of alkali-soluble polyester particles with an average particle size of 2 mm and dry them at 80°C for 14 hours by air blast drying, and weigh 50 parts of polyphenylene sulfide powder with an average particle size of 300 μm and dry them at 120°C for 12 hours by vacuum drying. The two materials are mixed evenly by a high-speed mixer and then transferred to a twin-screw extruder for granulation. After granulation by a twin-screw extruder at 250°C, the alkali-soluble polyester and polyphenylene sulfide blended masterbatch is obtained.

[0043] S2: Weigh 10 parts of blended masterbatch and dry them at 120℃ for 15h, first by air drying and then by vacuum drying. Weigh 30 parts of alkali-soluble polyester particles with an average particle size of 2mm and dry them at 120℃ for 12h. Mix the two materials thoroughly and transfer them into a single-screw spinning machine for spinning. The spinning temperature is 310℃ and the winding speed is 500m / s. The fiber is stretched at 80℃ and heat-set at 120℃ to obtain alkali-soluble polyester and polyphenylene sulfide blended fiber with a stretching multiple of 4 times.

[0044] S3: Soak the blended fiber in 8wt% sodium hydroxide solution to dissolve the alkali-soluble polyester, the dissolution temperature is 100℃, and the time is 1h. The sodium hydroxide solution and the blended fiber bath solid ratio is 50:1. After dissolving and removing the alkali-soluble polyester, nano polyphenylene sulfide fiber is finally obtained. The fiber diameter distribution is 200-400nm, and the average diameter is 300nm.

[0045] Example 2

[0046] The preparation method of this embodiment is the same as that of embodiment 1, except that 10 parts of the blended masterbatch and 25 parts of the alkali-soluble polyester particles are weighed for melt spinning. The prepared nano polyphenylene sulfide fiber has a diameter distribution of 400-600 nm and an average diameter of 500 nm.

[0047] Example 3

[0048] The preparation method of this embodiment is the same as that of embodiment 1, except that 10 parts of the blended masterbatch and 20 parts of the alkali-soluble polyester particles are weighed for melt spinning. The prepared nano polyphenylene sulfide fiber has a diameter distribution of 600-800 nm and an average diameter of 700 nm.

[0049] Example 4

[0050] The preparation method of this embodiment is the same as that of embodiment 1, except that the winding speed during the spinning process is 300 m / s. The diameter distribution of the prepared nano polyphenylene sulfide fibers is 400-700 nm, and the average diameter is 550 nm.

[0051] Example 5

[0052] The preparation method of this embodiment is the same as that of embodiment 1, except that the winding speed during the spinning process is 100 m / s. The prepared nano polyphenylene sulfide fiber has a diameter distribution of 500-800 nm and an average diameter of 650 nm.

[0053] Example 6

[0054] The preparation method of this embodiment is the same as that of Embodiment 1, except that the average particle size of the polyphenylene sulfide powder used in the twin-screw extruder for blending and granulation is 100 μm, and the diameter distribution of the nano-polyphenylene sulfide fibers finally prepared is 150-250 nm, with an average diameter of 200 nm.

[0055] Example 7

[0056] The preparation method of this embodiment is the same as that of Embodiment 1, except that the average particle size of the polyphenylene sulfide powder used in the twin-screw extruder for blending and granulation is 500 μm, and the diameter distribution of the nano-polyphenylene sulfide fibers finally prepared is 250-550 nm, and the average diameter is 400 nm.

[0057] Example 8

[0058] The preparation method of this embodiment is the same as that of embodiment 1, except that the drafting ratio of the alkali-soluble polyester and polyphenylene sulfide blended fiber is 3.5 times, and the diameter distribution of the finally prepared nano polyphenylene sulfide fiber is 300-500nm, and the average diameter is 400nm.

[0059] Example 9

[0060] The preparation method of this embodiment is the same as that of embodiment 1, except that the drafting ratio of the alkali-soluble polyester and polyphenylene sulfide blended fiber is 3 times, and the diameter distribution of the finally prepared nano polyphenylene sulfide fiber is 400-600nm, and the average diameter is 500nm.

[0061] Comparative Example 1

[0062] The twin-screw extruder blending and granulation method in this comparative example is the same as that in Example 1, except that the granulation temperature is 285° C., and the floating fibers are serious during the spinning process, and the blended fibers cannot be prepared. Therefore, the nano-polyphenylene sulfide fibers cannot be successfully prepared in the end.

[0063] Comparative Example 2

[0064] The twin-screw extruder co-blending granulation method in this comparative example is the same as that in Example 1, except that the granulation temperature is 240° C. During the granulation process, the twin-screw extruder alarm shows that the pressure is too high, and the co-blending granulation cannot be carried out smoothly.

[0065] Comparative Example 3

[0066] The twin-screw extruder blending and granulation method in this comparative example is the same as that in Example 1, except that the polyphenylene sulfide used in the twin-screw extruder granulation is particles with an average particle size of 2 mm. During the granulation process, the twin-screw extruder alarm shows that the pressure is too high, and the blending and granulation cannot be carried out smoothly.

[0067] Comparative Example 4

[0068] This comparative example is the same as the twin-screw extruder blending and granulation method in Example 1, except that only polyphenylene sulfide powder with an average particle size of 300 μm is used for granulation during the twin-screw blending and granulation, and no alkali-soluble polyester particles are added. After granulation, 5 parts of polyphenylene sulfide particles obtained by granulation by a twin-screw extruder are weighed and 35 parts of alkali-soluble polyester particles with an average particle size of 2 mm are dried and mixed, and then melt-spun directly. The final polyphenylene sulfide fiber has a diameter distribution of 0.5-2 μm and an average diameter of 1.4 μm. The average fiber diameter cannot completely reach the nanometer level, and the fiber diameter distribution is wide.

Claims

1. A method for preparing nano polyphenylene sulfide fiber, comprising: S1: Evenly mix the alkali-soluble polyester and polyphenylene sulfide, blend and granulate to obtain a blended masterbatch of the alkali-soluble polyester and polyphenylene sulfide; wherein the average particle size of the alkali-soluble polyester is 1-5 mm; the average particle size of the polyphenylene sulfide is 50-1000 μm; the blending and granulation temperature is 245-275° C.; wherein the mass percentage of polyphenylene sulfide in the blended masterbatch is 30-80wt%; S2: mixing the blended masterbatch and the alkali-soluble polyester, performing melt spinning, drawing and heat setting, and obtaining a blended fiber of the alkali-soluble polyester and polyphenylene sulfide; the mass fraction of the polyphenylene sulfide in the blended fiber is 10-40wt%; and the drawing ratio is 2-5 times; S3: Soaking the blended fibers in an alkaline solution to dissolve and remove the alkali-soluble polyester, thereby obtaining nano-polyphenylene sulfide fibers.

2. The method for preparing nano polyphenylene sulfide fiber according to claim 1, characterized in that: The alkali-soluble polyester in steps S1 and S2 is dried alkali-soluble polyester; wherein the drying temperature is 80-160°C, and the time is 12-20 hours; wherein the drying method is blast drying; the polyphenylene sulfide in step S1 is dried polyphenylene sulfide; wherein the drying temperature is 80-170°C, and the time is 10-24 hours; wherein the drying method is vacuum drying.

3. The method for preparing nano polyphenylene sulfide fiber according to claim 1, characterized in that: In the step S1, the average particle size of the alkali-soluble polyester is 1-3 mm; the average particle size of the polyphenylene sulfide is 50-600 μm; the alkali-soluble polyester is alkali-soluble polyester particles; and the polyphenylene sulfide is polyphenylene sulfide powder.

4. The method for preparing nano polyphenylene sulfide fiber according to claim 1, characterized in that: In the step S1, a twin-screw extruder is used for blending and granulation.

5. The method for preparing nano polyphenylene sulfide fiber according to claim 1, characterized in that: The blended masterbatch in step S2 is a dried blended masterbatch; wherein the drying temperature is 80-160° C., and the time is 14-24 hours; wherein the drying method is first air drying and then vacuum drying; The alkali-soluble polyester in step S2 is alkali-soluble polyester particles; the average particle size of the alkali-soluble polyester is 1-5 mm.

6. The method for preparing nano polyphenylene sulfide fiber according to claim 1, characterized in that: In the step S2, the melt spinning temperature is 295-330° C., and the winding speed is 100-1000 m / s; the melt spinning adopts a single screw melt spinning machine; The stretching and heat setting process parameters are as follows: the stretching temperature is 60-100°C, and the heat setting temperature is 100-160°C.

7. The method for preparing nano polyphenylene sulfide fiber according to claim 1, characterized in that: The alkali in the alkali solution in step S3 is at least one of NaOH and KOH; the concentration of the alkali solution is 4-10wt%; and the bath-solid ratio of the alkali solution to the blended fiber is 100-30:

1.

8. The method for preparing nano polyphenylene sulfide fiber according to claim 1, characterized in that: In step S3, the blended fibers are immersed in an alkaline solution at a dissolving temperature of 60-100° C. for a dissolving time of 0.5-2 h.

9. A nano polyphenylene sulfide fiber prepared by the method of claim 1, characterized in that: The average diameter of the nano polyphenylene sulfide fiber is 200-800nm.

10. Use of the nano polyphenylene sulfide fiber according to claim 9 in the fields of battery diaphragms, water electrolysis diaphragms, air purification filter materials, and composite materials.