A dual-functional oxygen catalyst cobalt iron / carbon composite nanomaterial and preparation method thereof

Through the MOF pyrolysis-replacement-alloying method of cobalt iron/carbon composite nanomaterials, high-content CoFe alloy nanosheets are prepared, which solves the problems of high catalyst cost and low reaction rate in the existing technology, and achieves efficient oxidation. Catalysis of reduction reactions, suitable for reversible fuel cells.

CN118553936BActive Publication Date: 2024-10-11YANGZHOU HYDROGEN ENERGY R&D MOTOR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411019549.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-11
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

Existing reversible fuel cells lack bifunctional oxygen electrocatalysts that can simultaneously accelerate the rates of oxidation-reduction reaction (ORR) and oxygen evolution reaction (OER). Moreover, traditional catalysts have high costs and limited resources, making it difficult to use them commercially on a large scale.

Method used

Cobalt-iron/carbon composite nanomaterials are used as bifunctional oxygen catalysts and are prepared through MOF pyrolysis-replacement-alloying methods to form high-content CoFe alloy nanosheets to improve catalytic activity and stability.

Benefits of technology

It significantly reduces the catalyst preparation cost and improves the utilization rate and electrochemical performance of the catalyst. It is suitable as an oxygen electrocatalyst for reversible fuel cells and improves the reaction rate and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118553936B_ABST
    Figure CN118553936B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a cobalt-iron-carbon composite nanomaterial that can be used as an OER / ORR bifunctional catalyst, wherein the composite nanomaterial comprises CoFe alloy nanoparticles and a carbon nanosheet carrier. The CoFe alloy nanoparticles have the characteristics of small particle size and uniform dispersion. The composite material of the present invention exhibits excellent bifunctional oxygen electrode catalytic activity, and has a significant cost advantage compared with traditional commercial precious metal catalysts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of reversible fuel cells, and in particular to a dual-functional oxygen catalyst cobalt iron / carbon composite nanomaterial and a preparation method thereof. Background Art

[0002] With the continuous development of human society, the demand for energy is getting higher and higher, and the environmental pollution problems are becoming more and more severe. The development of green new energy technology has become an inevitable choice for achieving sustainable development. Reversible fuel cells are a new type of battery technology based on reversible redox reactions, which can convert chemical energy into electrical energy or electrical energy into chemical energy. Unlike traditional fuel cells, reversible fuel cells can perform both fuel cell reactions (corresponding to the oxygen electrode side for oxygen reduction reaction: ORR) and water electrolysis reactions (corresponding to the oxygen electrode side for oxygen evolution reaction: OER), thereby realizing applications in both energy storage and energy conversion. Among them, the catalyst is a key part of the reversible fuel cell, which can speed up the reaction rate and improve the energy conversion efficiency. However, reversible fuel cells still face serious problems in their applications. The main reason is the lack of a bifunctional oxygen electrocatalyst that can simultaneously accelerate the reaction rates of OER and ORR and operate efficiently and stably for a long time.

[0003] Generally speaking, due to the high irreversibility of the oxygen electrode reaction, it is difficult for a single catalyst to efficiently catalyze both ORR and OER reactions at the same time. The catalyst commonly used on the oxygen electrode side of reversible fuel cells is a physical mixture of two commercial catalysts, Pt / C and RuO2. On the one hand, Pt and Ru have problems such as high unit price, limited resources, and easy poisoning, which are not conducive to large-scale commercial use from a cost perspective. On the other hand, simply physically mixing the two monofunctional catalysts increases the amount of catalyst used, which is not conducive to the full utilization of active sites and the improvement of performance. Therefore, the development of low-cost, high-performance bifunctional oxygen catalysts is of great significance to promoting the development of reversible fuel cell technology. Summary of the invention

[0004] The catalyst commonly used on the oxygen electrode side of reversible fuel cells is a physical mixture of two commercial catalysts, Pt / C and RuO2. On the one hand, Pt and Ru have problems such as high unit price, limited resources, and easy poisoning, which are not conducive to large-scale commercial use from a cost perspective. On the other hand, the simple physical mixing of two monofunctional catalysts increases the amount of catalyst used, which is not conducive to the full utilization of active sites and the improvement of performance. Therefore, the development of low-cost, high-performance bifunctional oxygen catalysts is of great significance to promote the development of reversible fuel cell technology.

[0005] The present application provides a method for preparing a bifunctional oxygen catalyst cobalt iron / carbon composite nanomaterial, using the following technical solution:

[0006] A method for preparing a bifunctional oxygen catalyst cobalt iron / carbon composite nanomaterial comprises the following steps:

[0007] S1. dissolving sodium dodecyl sulfate and a cobalt precursor in deionized water to obtain solution 1; dispersing dimethylimidazole in deionized water to obtain solution 2; then, rapidly injecting solution 2 into solution 1, stirring to completely disperse it, heating the obtained suspension, and then centrifuging to collect the product, and washing it with deionized water and ethanol for multiple times, respectively, to obtain sheet-like ZIF-67;

[0008] S2. The obtained flaky ZIF-67 is preheated and then heated to 800-900°C to obtain Co / C. The whole process is carried out in a N2 atmosphere.

[0009] S3. The Co / C prepared in step S2 is added to the water containing the iron precursor, stirred, the suspension is collected by centrifugation, washed several times with methanol, and then dried at room temperature to obtain a Pre-CoFe precursor;

[0010] S4. The powder obtained in step S3 is heated to 600-800 ℃ to obtain CoFe / C, and the whole process is carried out in a N2 atmosphere;

[0011] S5. The powder obtained in step S4 is heated to 200° C. to obtain CoFe / CO. The whole process is carried out in an O2 atmosphere.

[0012] By adopting the above technical scheme, solution two is injected into solution one at a high speed, stirred to make it completely dispersed, the obtained suspension is heated, and then the product is collected by centrifugation. Because sodium dodecyl sulfate is easily soluble in deionized water, deionized water is used to wash away the sodium dodecyl sulfate in the sample, and the flaky ZIF-67 is easily hydrolyzed. After the deionized water washing is completed, it is immediately washed with ethanol, which can protect the morphology of ZIF-67 and facilitate subsequent drying; the dried ZIF-67 powder is pre-calcined at a low temperature, which can effectively maintain the morphology of ultra-thin nanosheets, and the size of Co particles will not be agglomerated too large. Therefore, we choose to keep it at 300 degrees for two hours, which has a certain effect on the maintenance of the morphology of ultra-thin nanosheets, and then calcine it at a high temperature of 800-900℃ to obtain Co / C powder with the morphology of ultra-thin nanosheets. The whole process is carried out in a N2 atmosphere to prevent the Co particles from being oxidized; the Co / C powder is then added to an aqueous solution containing an iron precursor to carry out a replacement reaction of Fe ions, washed with methanol several times, and then dried at room temperature to obtain a core-shell structure Pre -CoFe precursor; then heated to 600-800℃ to form a homogeneous alloy material CoFe / C (in the morphology of square nanosheets). Since the alloy particles are composed of two or more metals, the multi-component structure of the alloy particles can provide better mechanical properties at the microscale, so its strength can be higher than that of single-component core-shell particles. The chemical properties of the alloy particles can be adjusted by selecting different components, thereby increasing its stability under different environmental conditions. In contrast, single-component core-shell particles may be prone to chemical reactions or oxidation under certain conditions. The multi-component structure of the alloy particles can improve their electrochemical properties. For example, alloy particles can provide better conductivity and electrocatalytic activity, which is very important for applications such as electronic devices and catalysts. Alloy particles usually have a higher melting point and better thermal stability, which is very useful for materials used under high temperature conditions because they can maintain their structure and properties, while core-shell particles may melt or deform at high temperatures; then low-temperature oxidation is used to form partial oxides on their surface, which is conducive to the OER reaction.

[0013] Preferably, in step S1, the cobalt precursor is at least one of cobalt nitrate, cobalt chloride and cobalt sulfate.

[0014] By adopting the above technical solution, the composition of the cobalt precursor is optimized, which is conducive to the formation of flaky ZIF-67.

[0015] Preferably, in step S3, the iron precursor is at least one of ferrous chloride, ferric chloride, ferrous sulfate, and ferric nitrate; and the mass ratio of the Co / C powdered solid to the iron precursor is (1 to 4):1.

[0016] By adopting the above technical solution, the composition of the iron precursor and the amount of the iron precursor are optimized, which is conducive to the formation of the Pre-CoFe precursor.

[0017] Preferably, in step S3, the stirring temperature is 60 to 100°C, and the stirring time is 8 to 16 h.

[0018] By adopting the above technical solution, the reaction temperature and reaction time of the Fe ion replacement reaction are optimized, and the Co / C powdered solid and the iron precursor fully react to form the Pre-CoFe precursor.

[0019] The composite material prepared by the preparation method is CoFe alloy nanoparticles loaded on a carrier, the content of CoFe alloy nanoparticles in the composite material is 50 to 60 wt%; the carrier is a carbon carrier, the morphology of the carrier is a nanosheet structure, and the diameter of the carrier is 1-1.5 μm; the surface of the CoFe alloy nanoparticles will be oxidized at low temperature to form an oxide layer.

[0020] By adopting the above technical solution, CoFe / C with the morphology of square nanosheets is obtained. The ultra-thin nanosheets have a high specific surface area, which means that the material per unit mass has more surface available for electrochemical reactions, which provides more reaction interfaces for electrochemical reactions, thereby increasing the reaction rate and efficiency; in addition, due to the special structure and smaller size of the nanosheets, ions and electrons can be transmitted faster between the surfaces of the nanosheets. This rapid transmission helps to improve the kinetic response of the electrochemical reaction and reduce the resistance of the electrode, thereby improving the electrochemical performance.

[0021] Slight oxidation of metal particles will form an oxide layer on the surface of the particles. This oxide layer can change the structure and electronic state of the metal surface, thereby providing more active sites and increasing the chance of catalytic reaction. The oxide layer can also help organize oxygen adsorption and charge transfer on the metal surface, promoting the OER reaction. The formation of the oxide layer will cause the electronic structure of the metal particles to be adjusted. This adjustment may modify the energy band structure of the metal surface, giving it better electron transfer performance and improving the conductivity of the OER reaction. The oxide layer can introduce new active sites and increase the reaction activity of the metal surface. These active sites can provide more reaction intermediate adsorption sites or participate in the reaction, thereby increasing the rate of the OER reaction.

[0022] The beneficial effects of the present invention are as follows: the present invention aims to provide a method for preparing a cobalt-iron / carbon composite nanocatalyst for a reversible fuel cell, which is based on MOF pyrolysis-replacement-alloying. Compared with the traditional method for preparing a catalyst, the steps are simple, and the obtained catalyst is a nanosheet-loaded CoFe alloy composite material with a high metal loading (up to 55wt%), uniform nanoparticle size, uniform distribution, high catalytic activity of OER / ORR, and greatly reduces the preparation cost of the catalyst compared to the traditional Pt / C-RuO2 catalyst, improves the utilization rate of the catalyst, and is suitable for use as an oxygen electrocatalyst for a reversible fuel cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the X-ray diffraction pattern of the CoFe / CO catalyst obtained in Example 1.

[0024] Figure 2 This is a transmission electron microscopy image of the CoFe / CO catalyst obtained in Example 1.

[0025] Figure 3 This is a transmission electron microscopy image of the CoFe / CO catalyst prepared in Comparative Example 1.

[0026] Figure 4 This is the thermogravimetric analysis diagram of the CoFe / CO catalyst obtained in Example 1 under O2 atmosphere.

[0027] Figure 5 The OER linear scanning curves of CoFe / CO obtained in Example 1 and CoFe / C obtained in Comparative Example 2 are shown.

[0028] Figure 6 The OER linear scan curves of CoFe / CO were prepared for Example 1 and Comparative Examples 3 to 4.

[0029] Figure 7 The ORR linear scan curves of CoFe / CO were prepared for Example 1 and Comparative Examples 3 to 4.

[0030] Figure 8 The OER linear scan curves of CoFe / CO were prepared for Examples 1 to 3.

[0031] Fig. 9 The ORR linear scan curves of CoFe / CO were prepared for Examples 1 to 3. DETAILED DESCRIPTION

[0032] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0033] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0034] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments. Example

[0035] The following description is given by taking Example 1 as an example. Example 1

[0036] (1) 1.6 g sodium dodecyl sulfate and 1.415 g cobalt precursor were dissolved in 120 mL deionized water to obtain solution 1, and then 3.195 g dimethylimidazole was dispersed in 20 mL deionized water to obtain solution 2; then solution 2 was quickly injected into solution 1 and stirred for 10 minutes to make it completely dispersed. The obtained suspension was heated at 80°C for 12 h, the product was collected by centrifugation, and washed with deionized water and ethanol three times respectively to obtain flaky ZIF-67.

[0037] (2) The obtained ZIF-67 flakes were heated to 300°C and maintained for 2 h, and then heated to 900°C and maintained for 2 h to obtain Co / C. The whole process was carried out in a N2 atmosphere with a heating rate of 2°C min -1 .

[0038] (3) Add 10 mg of the prepared Co / C into 10 mL of water containing 90 μmol of iron precursor, stir at 80 °C for 24 h, collect the suspension by centrifugation, wash it several times with methanol, and dry it at room temperature to obtain the Pre-CoFe precursor.

[0039] (4) The powder obtained in the previous step was heated to 600°C and maintained for 2 h to obtain CoFe / C. The whole process was carried out in a N2 atmosphere with a heating rate of 2°C min -1 .

[0040] (5) Heat the powder obtained in the previous step to 200℃ and keep it for 2 h to obtain CoFe / CO. The whole process is carried out in an O2 atmosphere. The heating rate is 2℃·min -1 .

[0041] As shown in Table 1, Examples 2 to 3 are different from Example 1 in that the mass ratio (M1:M2) of the Co / C powdered solid to the iron precursor is different.

[0042] Table 1 shows the mass ratio of Co / C powder solid to iron precursor

[0043] Example Example 1 Example 2 Example 3 M1:M2 1:1 2:1 4:1

[0044] Comparative Example 1

[0045] (1) 1.6 g sodium dodecyl sulfate and 1.415 g cobalt precursor were dissolved in 120 mL deionized water to obtain solution 1, and then 3.195 g dimethylimidazole was dispersed in 20 mL deionized water to obtain solution 2; then solution 2 was quickly injected into solution 1 and stirred for 10 minutes to make it completely dispersed. The obtained suspension was heated at 80°C for 12 h, the product was collected by centrifugation, and washed with deionized water and ethanol three times respectively to obtain flaky ZIF-67.

[0046] (2) The obtained ZIF-67 flakes were heated to 900℃ and maintained for 2 h to obtain Co / C. The whole process was carried out in a N2 atmosphere with a heating rate of 2℃·min -1 .

[0047] (3) Add 10 mg of the prepared Co / C into 10 mL of water containing 90 μmol of iron precursor, stir at 80 °C for 24 h, collect the suspension by centrifugation, wash it several times with methanol, and dry it at room temperature to obtain the Pre-CoFe precursor.

[0048] (4) The powder obtained in the previous step was heated to 600°C and maintained for 2 h to obtain CoFe / C. The whole process was carried out in a N2 atmosphere with a heating rate of 2°C min -1 .

[0049] (5) Heat the powder obtained in the previous step to 200℃ and keep it for 2 h to obtain CoFe / CO. The whole process is carried out in an O2 atmosphere. The heating rate is 2℃·min -1 .

[0050] The difference between this comparative example and Example 1 is that in step (2), the obtained flaky ZIF-67 is directly heated to 900°C.

[0051] Comparative Example 2

[0052] (1) 1.6 g sodium dodecyl sulfate and 1.415 g cobalt precursor were dissolved in 120 mL deionized water to obtain solution 1, and then 3.195 g dimethylimidazole was dispersed in 20 mL deionized water to obtain solution 2; then solution 2 was quickly injected into solution 1 and stirred for 10 minutes to make it completely dispersed. The obtained suspension was heated at 80°C for 12 h, the product was collected by centrifugation, and washed with deionized water and ethanol three times respectively to obtain flaky ZIF-67.

[0053] (2) The obtained ZIF-67 flakes were heated to 300°C and maintained for 2 h, and then heated to 900°C and maintained for 2 h to obtain Co / C. The whole process was carried out in a N2 atmosphere with a heating rate of 2°C min -1 .

[0054] (3) Add 10 mg of the prepared Co / C into 10 mL of water containing 90 μmol of iron precursor, stir at 80 °C for 24 h, collect the suspension by centrifugation, wash it several times with methanol, and dry it at room temperature to obtain the Pre-CoFe precursor.

[0055] (4) The powder obtained in the previous step was heated to 600°C and maintained for 2 h to obtain CoFe / C. The whole process was carried out in a N2 atmosphere with a heating rate of 2°C min -1 .

[0056] The difference between this comparative example and Example 1 is that step 5 is omitted, and the prepared CoFe / C is not subjected to low-temperature oxidation calcination.

[0057] Comparative Example 3

[0058] The difference between this comparative example and Example 1 is that the powder obtained in step (5) is heated to 300°C.

[0059] Comparative Example 4

[0060] The difference between this comparative example and Example 1 is that the powder obtained in step (5) is heated to 400°C.

[0061] Combining Example 1 and Figure 1 It can be seen that by comparing the actually observed diffraction peaks with the known standard diffraction data (Co, Fe), by comparing the positions and relative intensities of the diffraction peaks, the diffraction peaks of the CoFe / CO catalyst are single-phase and no phase separation is found, indicating that the CoFe / C catalyst is a CoFe alloy catalyst.

[0062] Combined with Example 1, Comparative Example 1 and Figure 2 and 3 It can be seen that the composite catalyst material prepared without preheating treatment will have the following Figure 3 The agglomeration phenomenon shown in the figure shows that the CoFe / CO composite catalyst material prepared according to the above process flow has the morphology of square nanosheets, and the particles are evenly loaded on the carrier, the particle size distribution is uniform, and the ultra-thin nanosheets have a high specific surface area, which means that the material per unit mass has more surface available for electrochemical reactions, which provides more reaction interfaces for electrochemical reactions, thereby increasing the reaction rate and efficiency; in addition, due to the special structure and small size of the nanosheets, ions and electrons can be transmitted faster between the nanosheet surfaces, and this rapid transmission helps to improve the kinetic response of the electrochemical reaction and reduce the resistance of the electrode. Therefore, the material exhibits excellent electrocatalytic performance.

[0063] Combining Example 1 and Figure 4 It can be seen that the obtained catalyst is a nanosheet-loaded CoFe alloy composite material with a metal loading of up to 59.94 wt%, which provides more reaction intermediate adsorption sites or participates in the reaction, thereby increasing the rate of the OER reaction.

[0064] Combined with Example 1 and Comparative Example 2 and combined Figure 5 It can be seen that the slightly oxidized alloyed metal particles can improve the redox reaction (OER) activity. The main reasons are as follows:

[0065] Surface structure changes: Slight oxidation of metal particles will form an oxide layer on the surface of the particles. This oxide layer can change the structure and electronic state of the metal surface, thereby providing more active sites and increasing the chance of catalytic reaction. The oxide layer can also help organize oxygen adsorption and charge transfer on the metal surface, promoting the OER reaction;

[0066] Electronic regulation effect: The formation of the oxide layer will cause the electronic structure of the metal particles to be adjusted. This adjustment may modify the band structure of the metal surface, making it have better electron transport performance and improving the conductivity of the OER reaction;

[0067] Increased active sites: The oxide layer can introduce new active sites and increase the reactivity of the metal surface. These active sites can provide more adsorption sites for reaction intermediates or participate in the reaction, thereby increasing the rate of the OER reaction.

[0068] Combined with Example 1, Comparative Examples 3 and 4 and combined Figure 6 and 7 It can be seen that slightly oxidizing the alloyed metal particles can improve the OER activity, but further increasing the oxidation temperature (300℃ / 400℃) will not further improve the performance. Excessively high temperature may cause catalyst deactivation or structural instability.

[0069] Combined with Examples 1 to 3 and combined with Figure 8 and 9 It can be seen that by changing the metal components in the alloyed metal particles, the optimal ratio can be adjusted to further improve the OER performance and effectively regulate the type and number of surface active sites, electronic structure and crystal structure of the catalyst.

[0070] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a bifunctional oxygen catalyst cobalt iron / carbon composite nanomaterial, characterized in that: The steps include: S1. dissolving sodium dodecyl sulfate and a cobalt precursor in deionized water to obtain solution 1; dispersing dimethylimidazole in deionized water to obtain solution 2; then, rapidly injecting solution 2 into solution 1, stirring to completely disperse it, heating the obtained suspension, and then centrifuging to collect the product, and washing it with deionized water and ethanol for multiple times, respectively, to obtain sheet-like ZIF-67; S2. The obtained flaky ZIF-67 is preheated and then heated to 800-900°C to obtain Co / C. The whole process is carried out in a N2 atmosphere; wherein the preheating temperature is 300°C; S3. The Co / C prepared in step S2 is added to the aqueous solution containing the iron precursor, stirred, the suspension is collected by centrifugation, washed several times with methanol, and then dried at room temperature to obtain a Pre-CoFe precursor; S4. The powder obtained in step S3 is heated to 600-800 ℃ to obtain CoFe / C, and the whole process is carried out in a N2 atmosphere; S5. The powder obtained in step S4 is heated to 200° C. to obtain CoFe / CO. The whole process is carried out in an O2 atmosphere.

2. The preparation method according to claim 1, characterized in that: In step S1, the cobalt precursor is at least one of cobalt nitrate, cobalt chloride and cobalt sulfate.

3. The preparation method according to claim 1, characterized in that: In step S3, the iron precursor is at least one of ferrous chloride, ferric chloride, ferrous sulfate, and ferric nitrate; and the mass ratio of the Co / C powdered solid to the iron precursor is (1 to 4):

1.

4. The preparation method according to claim 1, characterized in that: In step S3, the stirring temperature is 60 to 100°C, and the stirring time is 8 to 24 h.

5. A composite nanomaterial prepared by the preparation method according to any one of claims 1 to 4, characterized in that: The composite nanomaterial is CoFe alloy nanoparticles loaded on a carrier, and the content of the CoFe alloy nanoparticles in the composite nanomaterial is 50 to 60 wt %.

6. The composite nanomaterial according to claim 5, characterized in that: The carrier is a carbon carrier, the morphology of the carrier is a nano-sheet structure, and the diameter of the carrier is 1-1.5 μm.

7. The composite nanomaterial according to claim 6, characterized in that: The surface of the CoFe alloy nanoparticles is oxidized at low temperature to form an oxide layer.