A nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst and its preparation method and application
By co-doping nitrogen-fluorine-supported zinc-molybdenum diatomic oxygen reduction catalyst, the high cost and low activity of nitrogen-doped carbon-supported molybdenum single-atom catalysts are solved, and high Preparation of reactive oxygen reduction catalysts, suitable for fuel cells and zinc-air batteries.
Patent Information
- Application Number
- CN202411027436.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The existing nitrogen-doped carbon-supported molybdenum single-atom catalyst synthesis raw materials are expensive, and molybdenum atoms are prone to migration and agglomeration, resulting in low catalytic activity and hindering the actual output performance of fuel cells and zinc-air batteries.
The preparation method of nitrogen-fluorine-co-doped carbon-supported zinc-molybdenum diatom oxygen reduction catalyst is used to avoid molybdenum atoms by grinding and pyrolyzing the nitrogen-containing biomass with the fluorine source, combining the impregnation and secondary pyrolysis of the zinc and molybdenum sources. Migrate and optimize its activity, use cheap biomass as a precursor, introduce zinc atoms as a space separator and fluorine atoms to regulate the electronic structure of molybdenum.
It realizes a high-active catalyst with low cost and atomic dispersion, avoids molybdenum atom agglomeration, improves oxygen reduction reaction activity, is suitable for fuel cells and zinc-air battery cathodes, significantly improving the performance of the catalyst.
Smart Images

Figure CN118553937B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of oxygen reduction catalysts, and in particular to a nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst, and a preparation method and application thereof. Background Art
[0002] With the increasing depletion of fossil energy, new green energy conversion devices such as proton exchange membrane fuel cells (PEMFCs) and zinc-air batteries (ZABs) have attracted more and more attention from researchers. Fuel cells have many advantages such as high energy conversion efficiency, strong reliability, and no pollutant emissions, and are expected to provide stable energy for vehicles such as cars and ships; while zinc-air batteries have the characteristics of high theoretical energy density, low production cost, and simple structure, and also show broad development prospects. However, the slow oxygen reduction reaction (ORR) kinetics of the cathode seriously restricts the actual output performance of the above two batteries and leads to the current heavy dependence on platinum-based catalysts. The high price of platinum-based catalysts hinders the large-scale commercial application of fuel cells and zinc-air batteries. Therefore, it is urgent to develop an efficient non-precious metal oxygen reduction catalyst to replace platinum-based catalysts.
[0003] Among the numerous non-precious metal catalysts, nitrogen-doped carbon-supported molybdenum single-atom catalysts have attracted extensive attention from researchers. However, the current raw materials for the synthesis of nitrogen-doped carbon-supported molybdenum single-atom catalysts are expensive, which is not conducive to the large-scale commercial preparation of catalysts. On the other hand, during the high-temperature pyrolysis process to synthesize the catalyst, molybdenum atoms are prone to migration and agglomeration, thereby forming low-activity metal nanoparticles. In addition, as the active center of the catalyst, the molybdenum atom has a strong adsorption effect on the intermediates of the oxygen reduction reaction, which restricts the smooth progress of the subsequent elementary reactions, resulting in lower intrinsic catalytic activity.
[0004] In response to the above problems, it is urgently necessary to optimize from the perspectives of rationally selecting precursor materials, avoiding the migration and agglomeration of molybdenum atoms, and improving the intrinsic activity of molybdenum atoms, so as to prepare low-cost atomically dispersed oxygen reduction catalysts with good catalytic activity. Summary of the invention
[0005] The purpose of the present invention is to provide a nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst and a preparation method and application thereof in order to overcome the deficiencies of the prior art.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst, comprising the following steps:
[0008] 1) grinding nitrogen-containing biomass and a fluorine source, and pyrolyzing the obtained mixture under an argon atmosphere to obtain a nitrogen-fluorine co-doped carbon support;
[0009] 2) mixing the nitrogen-fluorine co-doped carbon support, the zinc source, the molybdenum source and the solvent, and then sequentially impregnating and vacuum drying to obtain a mixture powder;
[0010] 3) The mixture powder is pyrolyzed in an argon atmosphere to obtain a nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst.
[0011] Preferably, in step 1), the nitrogen-containing biomass comprises one or more of glycine, glucosamine, hypoxanthine, chitin, D-arginine, thymine, D-aspartic acid, taurine and polymerized protein; and the fluorine source comprises one or more of 1-fluoropyridine tetrafluoroborate, N-fluoropyridine trifluoromethanesulfonate, ammonium fluoride, levofloxacin and 5-fluorocytosine.
[0012] Preferably, in step 1), the mass ratio of the nitrogen-containing biomass to the fluorine source is 1:1-20, and the grinding time is 10-15 min.
[0013] Preferably, the pyrolysis temperature in step 1) is 800-1000°C, the pyrolysis time is 0.5-3.5h, and the heating rate to the pyrolysis temperature is 3-10°C / min.
[0014] Preferably, in step 2), the zinc source comprises one or more of zinc dimethacrylate, zinc nitrate hexahydrate, zinc chloride, zinc monoethyl fumarate and zinc acetate; the molybdenum source comprises one or more of ammonium molybdate tetrahydrate, molybdenum acetylacetonate, sodium molybdate dihydrate and ammonium octamolybdate; and the solvent comprises one or more of methanol, ethanol, ether, ethylene glycol, water and N,N-dimethylformamide.
[0015] Preferably, in step 2), the molar ratio of the molybdenum source to the zinc source is 1:1-5, and the mass molar ratio of the nitrogen-fluorine co-doped carbon support to the molybdenum source is 1-2 g: 0.002-0.004 mol.
[0016] Preferably, in step 2), stirring is performed during the impregnation process at a speed of 60-700 r / min for 6-12 h; the vacuum drying time is 6-8 h, and the vacuum drying temperature is 50-80°C.
[0017] Preferably, in step 3), the pyrolysis temperature is 750-950°C, the pyrolysis time is 0.5-2h, and the heating rate to the pyrolysis temperature is 3-10°C / min.
[0018] The present invention also provides a nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst prepared by the preparation method.
[0019] The present invention also provides the use of the nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst in a battery cathode, and the battery is a proton exchange membrane fuel cell or a zinc-air battery.
[0020] The beneficial effects of the present invention include:
[0021] 1) The present invention uses biomass as a nitrogen-containing precursor for synthesizing the catalyst. Biomass raw materials are abundant in reserves and low in price, which is conducive to the commercial preparation of the catalyst.
[0022] 2) The present invention prepares a nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst through fluorination treatment, bimetallic source impregnation and secondary pyrolysis treatment. The preparation method does not require complicated acid washing and etching treatment, is easy to operate, and is conducive to the large-scale preparation of the catalyst.
[0023] 3) The present invention introduces a zinc source as a spatial isolation agent, and uses zinc atoms to isolate each molybdenum atom in space, thereby effectively avoiding the migration and agglomeration of molybdenum atoms during the pyrolysis process. In addition, most of the zinc atoms evaporate during the pyrolysis process, and only a small part of the zinc atoms are doped in the carbon carrier, thereby avoiding the formation of zinc-molybdenum alloy particles.
[0024] 4) The present invention introduces fluorine atom doping to adjust the d-band center electronic structure of molybdenum atoms, thereby optimizing the Mo-N x The charge distribution near the active site reduces the adsorption of molybdenum atoms on oxygen reduction reaction intermediates, promotes the smooth progress of subsequent elementary reactions, and ultimately effectively improves the intrinsic oxygen reduction activity of the catalyst.
[0025] 5) The biomass-derived nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst prepared by the present invention has atomically dispersed high active sites, exhibits good oxygen reduction activity, and can be used as a catalyst in the cathode of zinc-air batteries or proton exchange membrane fuel cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a photo of the biomass-derived nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst of Example 1;
[0027] Figure 2 This is a transmission electron micrograph of the biomass-derived nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst of Example 1;
[0028] Figure 3 is an X-ray diffraction (XRD) spectrum of the biomass-derived nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst of Example 1;
[0029] Figure 4 The linear voltammetric scanning curves of the nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst of Example 1 and the nitrogen-doped carbon-supported molybdenum single-atom oxygen reduction catalyst of Comparative Example 1 in KOH solution. DETAILED DESCRIPTION
[0030] The present invention provides a method for preparing a nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst, comprising the following steps:
[0031] 1) grinding nitrogen-containing biomass and a fluorine source, and pyrolyzing the obtained mixture under an argon atmosphere to obtain a nitrogen-fluorine co-doped carbon support;
[0032] 2) mixing the nitrogen-fluorine co-doped carbon support, the zinc source, the molybdenum source and the solvent, and then sequentially impregnating and vacuum drying to obtain a mixture powder;
[0033] 3) The mixture powder is pyrolyzed in an argon atmosphere to obtain a nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst.
[0034] In the present invention, the nitrogen-containing biomass in step 1) preferably comprises one or more of glycine, glucosamine, hypoxanthine, chitin, D-arginine, thymine, D-aspartic acid, taurine and polymerized protein; the fluorine source preferably comprises one or more of 1-fluoropyridine tetrafluoroborate, N-fluoropyridine trifluoromethanesulfonate, ammonium fluoride, levofloxacin and 5-fluorocytosine.
[0035] In the present invention, in step 1), the mass ratio of the nitrogen-containing biomass to the fluorine source is preferably 1:1-20, more preferably 1:3-15, and more preferably 1:5-10; the grinding time is preferably 10-15 min, more preferably 11-14 min, and more preferably 12-13 min.
[0036] In the present invention, the pyrolysis temperature in step 1) is preferably 800-1000°C, more preferably 850-950°C, and more preferably 900°C; the pyrolysis time is preferably 0.5-3.5h, more preferably 1-3h, and more preferably 2h; the heating rate to the pyrolysis temperature is preferably 3-10°C / min, more preferably 5-8°C / min, and more preferably 6-7°C / min.
[0037] In the present invention, the zinc source in step 2) preferably comprises one or more of zinc dimethacrylate, zinc nitrate hexahydrate, zinc chloride, zinc monoethyl fumarate and zinc acetate; the molybdenum source preferably comprises one or more of ammonium molybdate tetrahydrate, molybdenum acetylacetonate, sodium molybdate dihydrate and ammonium octamolybdate; and the solvent preferably comprises one or more of methanol, ethanol, ether, ethylene glycol, water and N,N-dimethylformamide.
[0038] In the present invention, the molar ratio of the molybdenum source and the zinc source in step 2) is preferably 1:1-5, more preferably 1:2-4, and more preferably 1:3; the mass molar ratio of the nitrogen-fluorine co-doped carbon support and the molybdenum source is preferably 1-2 g: 0.002-0.004 mol, more preferably 1.2-1.8 g: 0.0025-0.0035 mol, and more preferably 1.5-1.6 g: 0.003 mol.
[0039] In the present invention, the mass volume ratio of the nitrogen-fluorine co-doped carbon support and the solvent is preferably 1-2 g:30-50 mL, more preferably 1.2-1.8 g:35-45 mL, and more preferably 1.5-1.6 g:40 mL.
[0040] In the present invention, stirring is preferably performed during the impregnation process in step 2), and the stirring speed is preferably 60-700 r / min, more preferably 80-500 r / min, more preferably 100-300 r / min, and the stirring time is preferably 6-12 h, more preferably 8-10 h, more preferably 9 h; the vacuum drying time is preferably 6-8 h, more preferably 6.5-7.5 h, more preferably 7 h; the vacuum drying temperature is preferably 50-80 ° C, more preferably 60-70 ° C, more preferably 65 ° C.
[0041] In the present invention, the pyrolysis temperature in step 3) is preferably 750-950°C, more preferably 800-900°C, the pyrolysis time is preferably 0.5-2h, more preferably 1-1.5h, and the heating rate to the pyrolysis temperature is preferably 3-10°C / min, more preferably 5-8°C / min, and more preferably 6-7°C / min.
[0042] The present invention also provides a nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst prepared by the preparation method.
[0043] The present invention also provides the use of the nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst in a battery cathode, and the battery is a proton exchange membrane fuel cell or a zinc-air battery.
[0044] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0045] Example 1
[0046] 4 g of hypoxanthine and 5 g of ammonium fluoride were manually ground with a pestle in an agate mortar for 12 min to obtain a uniform mixture. The mixture was then placed in a tubular furnace filled with argon and heated to 900 °C at a heating rate of 5 °C / min. Pyrolysis was continued at 900 °C for 2 h. After the pyrolysis was completed, it was cooled to room temperature to obtain a nitrogen-fluorine co-doped carbon support.
[0047] 1.5 g of nitrogen-fluorine co-doped carbon support, 0.006 mol of zinc chloride and 0.003 mol of sodium molybdate dihydrate were added to 40 mL of water, and magnetically stirred at a speed of 80 r / min for 8 h to ensure full impregnation, followed by vacuum drying at 60 ° C (vacuum degree of 130 Pa) for 7 h to obtain a mixture powder.
[0048] The mixed powder was placed in a tubular furnace filled with argon, heated to 900°C at a heating rate of 5°C / min, and pyrolyzed at 900°C for 1.5 hours. After the pyrolysis was completed, it was cooled to room temperature to obtain a biomass-derived nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst.
[0049] Example 2
[0050] 4 g of glycine and 20 g of 1-fluoropyridine tetrafluoroborate were ground in an agate mortar for 15 min to obtain a uniform mixture. The mixture was then placed in a tubular furnace filled with argon and heated to 950 °C at a heating rate of 8 °C / min. Pyrolysis was continued at 950 °C for 1 h. After the pyrolysis was completed, it was cooled to room temperature to obtain a nitrogen-fluorine co-doped carbon support.
[0051] 1.2 g of nitrogen-fluorine co-doped carbon support, 0.01 mol of zinc nitrate hexahydrate and 0.0025 mol of ammonium octamolybdate were added to 35 mL of ethylene glycol, and magnetically stirred at a speed of 300 r / min for 6 h to ensure full impregnation, followed by vacuum drying at 50°C (vacuum degree of 130 Pa) for 8 h to obtain a mixture powder.
[0052] The mixed powder was placed in a tubular furnace filled with argon, heated to 900°C at a heating rate of 8°C / min, and pyrolyzed at 900°C for 1 hour. After the pyrolysis was completed, it was cooled to room temperature to obtain a biomass-derived nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst.
[0053] Example 3
[0054] 4 g of D-aspartic acid and 12 g of levofloxacin were ground in an agate mortar for 10 min to obtain a uniform mixture. The mixture was then placed in a tubular furnace filled with argon and heated to 850 °C at a heating rate of 3 °C / min. Pyrolysis was continued at 850 °C for 3 h. After the pyrolysis was completed, it was cooled to room temperature to obtain a nitrogen-fluorine co-doped carbon support.
[0055] 1.6 g of nitrogen-fluorine co-doped carbon support, 0.01 mol of zinc acetate and 0.0035 mol of ammonium molybdate tetrahydrate were added to 45 mL of methanol, and magnetically stirred at a speed of 100 r / min for 10 h to ensure full impregnation, and then vacuum dried at 70°C (vacuum degree of 130 Pa) for 6 h to obtain a mixture powder.
[0056] The mixed powder was placed in a tubular furnace filled with argon, heated to 800°C at a heating rate of 3°C / min, and pyrolyzed at 800°C for 2 hours. After the pyrolysis was completed, it was cooled to room temperature to obtain a biomass-derived nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst.
[0057] Example 4
[0058] 4 g of glucosamine and 40 g of 5-fluorocytosine were ground in an agate mortar for 12 min to obtain a uniform mixture. The mixture was then placed in a tubular furnace filled with argon and heated to 900 °C at a heating rate of 6 °C / min. Pyrolysis was continued at 900 °C for 2 h. After the pyrolysis was completed, it was cooled to room temperature to obtain a nitrogen-fluorine co-doped carbon support.
[0059] 1.5 g of nitrogen-fluorine co-doped carbon support, 0.009 mol of zinc dimethacrylate and 0.003 mol of molybdenum acetylacetonate were added to 45 mL of ether, and magnetically stirred at a speed of 100 r / min for 9 h to ensure full impregnation, followed by vacuum drying at 70 ° C (vacuum degree of 130 Pa) for 7 h to obtain a mixture powder.
[0060] The mixed powder was placed in a tubular furnace filled with argon, heated to 900°C at a heating rate of 6°C / min, and pyrolyzed at 900°C for 2 hours. After the pyrolysis was completed, it was cooled to room temperature to obtain a biomass-derived nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst.
[0061] Comparative Example 1
[0062] 1.314 g of 2-methylimidazole was dissolved in 80 mL of methanol to obtain solution A; 1.19 g of zinc nitrate hexahydrate and 0.16 g of molybdenum acetylacetonate were dissolved in 40 mL of methanol to obtain solution B; solution A and solution B were mixed and continuously magnetically stirred at 25° C. for 24 h to obtain a suspension.
[0063] The suspension was centrifugally washed with methanol (centrifugal speed of 5000r / min) three times, and then vacuum dried at 60°C for 10h to obtain ZnMo-ZIF precursor powder; the ZnMo-ZIF precursor powder was placed in a tubular furnace, heated to 900°C at a heating rate of 5°C / min under an argon atmosphere, and continuously pyrolyzed at 900°C for 2h to obtain a ZIF-derived nitrogen-doped carbon-supported molybdenum single-atom oxygen reduction catalyst.
[0064] A photo of the biomass-derived nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst prepared in Example 1 is shown in FIG. Figure 1 As shown. Figure 1 It can be seen that the yield of the biomass-derived nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst prepared in Example 1 reached 1.3568 g, reaching the gram-level preparation level.
[0065] The transmission electron microscopy image of the biomass-derived nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst prepared in Example 1 is as follows: Figure 2 The X-ray diffraction (XRD) spectrum of the biomass-derived nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst prepared in Example 1 is shown in Figure 3 As shown. Figure 2 , 3 It can be seen that no obvious metal nanoparticles were observed in the biomass-derived nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst of Example 1, and no characteristic peaks corresponding to molybdenum-based nanoparticles were observed. Only the characteristic peak corresponding to graphite carbon existed near 25°, indicating that the molybdenum atoms did not migrate and agglomerate during the pyrolysis process, and therefore no molybdenum-based nanoparticles were formed.
[0066] The biomass-derived nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst prepared in Example 1 and the ZIF-8-derived nitrogen-doped carbon-supported molybdenum single-atom oxygen reduction catalyst prepared in Comparative Example 1 were subjected to linear voltammetric scanning tests in an oxygen-saturated KOH aqueous solution (the concentration of KOH was 0.1 mol / L) using a PINE rotating disk electrode and a Shanghai Chenhua CHI-760E electrochemical workstation. The scanning rate was 10 mV / s, the scanning range was 0.2~1.2V (RHE), and the disk speed was 1600 rpm. The linear voltammetric scanning curves of the nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst in Example 1 and the nitrogen-doped carbon-supported molybdenum single-atom oxygen reduction catalyst in Comparative Example 1 in KOH solution are as shown in FIG. Figure 4 As shown. Figure 4 It can be seen that the half-wave potential and limiting diffusion current density of the biomass-derived nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst of Example 1 are significantly higher than those of Comparative Example 1, indicating that the introduction of zinc atoms and the doping of fluorine atoms effectively improve the oxygen reduction activity of the catalyst.
[0067] In the nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst of the present invention, cheap and readily available biomass is used as a nitrogen-containing precursor, and the spatial isolation of zinc atoms effectively avoids the formation of low-activity molybdenum-based metal nanoparticles during pyrolysis; at the same time, fluorine atom doping can adjust the d-band electronic structure of molybdenum atoms and optimize the Mo-N xThe adsorption strength of the sites on oxygen reduction intermediates is improved, thereby improving the intrinsic catalytic activity. The nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic catalyst has atomic-level dispersed sites with high intrinsic activity and exhibits good oxygen reduction activity in proton exchange membrane fuel cells and zinc-air batteries; it solves the problems of high preparation cost, easy agglomeration of metal active centers, and limited intrinsic catalytic activity of the current nitrogen-doped carbon-supported molybdenum single-atom catalyst.
[0068] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst, characterized in that: The following steps are included: 1) grinding nitrogen-containing biomass and a fluorine source, and pyrolyzing the obtained mixture under an argon atmosphere to obtain a nitrogen-fluorine co-doped carbon support; 2) mixing the nitrogen-fluorine co-doped carbon support, the zinc source, the molybdenum source and the solvent, and then sequentially impregnating and vacuum drying to obtain a mixture powder; 3) pyrolyzing the mixture powder under an argon atmosphere to obtain a nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst; Step 1) the nitrogen-containing biomass comprises one or more of glycine, glucosamine, hypoxanthine, chitin, D-arginine, thymine, D-aspartic acid, taurine and polymerized protein; the fluorine source comprises one or more of 1-fluoropyridine tetrafluoroborate, N-fluoropyridine trifluoromethanesulfonate, ammonium fluoride, levofloxacin and 5-fluorocytosine; Step 1) The pyrolysis temperature is 800-1000°C, the pyrolysis time is 0.5-3.5h, and the heating rate to the pyrolysis temperature is 3-10°C / min; Step 3) The pyrolysis temperature is 750-950°C, the pyrolysis time is 0.5-2h, and the heating rate to the pyrolysis temperature is 3-10°C / min.
2. The method for preparing the nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst according to claim 1, characterized in that: Step 1) The mass ratio of the nitrogen-containing biomass to the fluorine source is 1:1-20, and the grinding time is 10-15 minutes.
3. The method for preparing the nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst according to claim 1 or 2, characterized in that: Step 2) the zinc source comprises one or more of zinc dimethacrylate, zinc nitrate hexahydrate, zinc chloride, zinc monoethyl fumarate and zinc acetate; the molybdenum source comprises one or more of ammonium molybdate tetrahydrate, molybdenum acetylacetonate, sodium molybdate dihydrate and ammonium octamolybdate; the solvent comprises one or more of methanol, ethanol, ether, ethylene glycol, water and N,N-dimethylformamide.
4. The method for preparing the nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst according to claim 3, characterized in that: Step 2) The molar ratio of the molybdenum source to the zinc source is 1:1-5, and the mass molar ratio of the nitrogen-fluorine co-doped carbon support to the molybdenum source is 1-2 g: 0.002-0.004 mol.
5. The method for preparing the nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst according to claim 4, characterized in that: Step 2) Stirring is performed during the impregnation process at a speed of 60-700 r / min for 6-12 h; the vacuum drying time is 6-8 h at a temperature of 50-80°C.
6. A nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst prepared by the method for preparing the nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst according to any one of claims 1 to 5.
7. Use of the nitrogen-fluorine co-doped carbon-supported zinc-molybdenum diatomic oxygen reduction catalyst in a battery cathode as claimed in claim 6, characterized in that: The battery is a proton exchange membrane fuel cell or a zinc-air battery.
Citation Information
Patent Citations
Fluorine and nitrogen co-doped three-dimensional graphene material and one-step carbonization preparation method thereof
CN109437165A
Carbon material with nitrogen, fluorine and transition metal co-doped graphene structure and one-step carbonization preparation method thereof
CN110148762A
ZIF-L derived multidimensional cross-linked structure Fe-N-C catalyst containing oxygen vacancies and Al-air battery
CN115440991A
Zinc-cobalt-nitrogen co-doped catalyst with hollow carbon shell structure as well as preparation method and application of zinc-cobalt-nitrogen co-doped catalyst
CN117899913A
Synergistic co-pyrolysis of biomass and methane for hydrocarbon fuels and chemicals production
US20180142159A1