A polypropylene pearlescent film and its preparation method and application in facial mask base material

By introducing modified xanthan gum copolymer into the polypropylene pearlescent film, the problems of poor electrostatic performance and low natural degradation rate of the polypropylene pearlescent film in facial mask substrates are solved, achieving efficient static electricity management and improved biodegradability. .

CN118560135BActive Publication Date: 2024-10-15烟台富利新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411062332.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-15
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

When the existing polypropylene pearlescent film is used in facial mask substrates, it has poor electrostatic adsorption and repulsion properties, and its natural degradation rate is low.

Method used

By introducing modified xanthan gum copolymer into the polypropylene pearlescent film and preparing it by graft copolymerization of xanthan gum, methyl methacrylate and methacryloyloxyethyltrimethylammonium chloride, the antistatic properties and Natural degradation rate. The modified xanthan gum copolymer is graft-copolymerized with deionized water, methyl methacrylate and methacryloyloxyethyltrimethylammonium chloride solution in a reaction bottle under nitrogen protection to form a copolymer with compatibilization and resistance properties. Materials with electrostatic properties are added to the outer layer, middle layer and inner surface layer of the polypropylene pearlescent film.

Benefits of technology

It significantly improves the antistatic performance and natural degradation rate of polypropylene pearlescent film, avoids unstable performance due to compatibility issues, and achieves excellent electrostatic performance and biodegradability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention discloses a polypropylene pearlescent film and a preparation method thereof and an application thereof in a facial mask base material, belonging to the technical field of polypropylene pearlescent film. The high-density polypropylene pearlescent film comprises an outer layer, an intermediate layer and an inner layer, wherein the outer layer comprises: polypropylene, polypropylene carbonate, xanthan gum, titanium dioxide, organic pearlescent masterbatch, calcium carbonate and an antioxidant; the intermediate layer comprises: polypropylene, titanium dioxide, organic pearlescent masterbatch and a modified xanthan gum copolymer; the inner layer comprises: polypropylene, titanium dioxide and a modified xanthan gum copolymer. The modified xanthan gum copolymer is prepared by graft copolymerization of xanthan gum with methyl methacrylate and methacryloyloxyethyl trimethylammonium chloride. The polypropylene pearlescent film prepared by the present application has an excellent natural degradation rate, and its antistatic layer has excellent antistatic properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polypropylene pearlescent films, and in particular to a polypropylene pearlescent film and a preparation method thereof and application thereof in a facial mask base material. Background Art

[0002] Polypropylene pearlescent film has the advantages of low specific gravity, high strength, good weather resistance, good tear resistance, soft texture, excellent printing performance and durability. Polypropylene pearlescent film has been widely used in printing, packaging, cosmetics and other aspects because it has the characteristics of both plastic and paper. With the increase in the application scenarios of polypropylene pearlescent film, more requirements are put forward for polypropylene pearlescent film. For example, when polypropylene pearlescent film is used in facial mask base materials, one side of the pearlescent film is required to have a certain electrostatic adsorption performance, and the other side has the performance of repelling static electricity, so as to avoid adhesion between different combinations. Generally, the side with electrostatic adsorption performance is treated with corona, and the side that needs electrostatic repulsion is added with antistatic agent. However, in many cases, the antistatic effect of adding antistatic agent is not good due to the amount of addition; at the same time, many existing polypropylene pearlescent films cannot be naturally degraded or the natural degradation rate is relatively low.

[0003] The Chinese invention patent application with publication number CN112721370A discloses a BOPP pearlescent film and its preparation method and application. Although the antistatic surface of the polypropylene pearlescent film disclosed in the patent application has a good antistatic effect, its natural degradation rate is relatively low. Summary of the invention

[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a polypropylene pearlescent film and a preparation method thereof and application in a facial mask base material.

[0005] To achieve the above object, the present invention is implemented through the following technical solutions:

[0006] A polypropylene pearlescent film comprises an outer layer, an intermediate layer and an inner layer, wherein the outer layer comprises the following raw materials in parts by weight: polypropylene: 15-20 parts, polypropylene carbonate: 20-30 parts, xanthan gum: 20-30 parts, titanium dioxide: 1-2 parts, organic pearlescent masterbatch: 8-15 parts, calcium carbonate: 1-2 parts, antioxidant: 1-2 parts;

[0007] The intermediate layer comprises the following raw materials in parts by weight: polypropylene: 20-25 parts, titanium dioxide: 1-2 parts, organic pearlescent masterbatch: 5-10 parts, modified xanthan gum copolymer: 50-60 parts;

[0008] The inner surface layer comprises the following raw materials in parts by weight: polypropylene: 15-20 parts, titanium dioxide: 1-2 parts, modified xanthan gum copolymer: 35-40 parts;

[0009] The modified xanthan gum copolymer is prepared by graft copolymerization of xanthan gum, methyl methacrylate and methacryloyloxyethyl trimethyl ammonium chloride.

[0010] The modified xanthan gum copolymer is prepared by the following method:

[0011] Under nitrogen protection, add deionized water and xanthan gum to the reaction bottle, stir and mix, and heat to 40-50°C; slowly add methyl methacrylate ethanol solution, methacryloyloxyethyl trimethyl ammonium chloride solution, and ammonium persulfate solution to the reaction bottle at the same time, dropwise for 0.5-1h, and graft copolymerize for 1-2h to obtain a modified xanthan gum copolymer. The reaction route is as follows:

[0012]

[0013] Among them, XG stands for xanthan gum.

[0014] The mass ratio of the xanthan gum, the ethanol solution of methyl methacrylate, the methacryloyloxyethyl trimethyl ammonium chloride solution and the ammonium persulfate solution is 30:(8-10):(3-5):(0.5-1).

[0015] The concentration of the ammonium persulfate solution is 0.05-0.1 mol / L.

[0016] The concentration of the methyl methacrylate ethanol solution is 25-30 wt %.

[0017] The methacryloyloxyethyltrimethylammonium chloride solution is a 70-80wt% aqueous solution.

[0018] The antioxidant is one of 2,6-di-tert-butyl-p-cresol and 2,6-di(octadecyl)-4-methylphenol.

[0019] A method for preparing a polypropylene pearlescent film comprises the following steps:

[0020] S1: Extruding the outer layer raw material, the middle layer raw material and the inner layer raw material through an extruder respectively;

[0021] S2: extruding each layer of raw materials extruded by the extruder through a T-type die, and then longitudinally stretching and transversely stretching, followed by cooling, corona treatment of the outer layer, and trimming;

[0022] Among them, the extrusion temperature of the outer layer raw material and the inner layer raw material is 230°C, and the extrusion temperature of the middle layer raw material is 250°C; the preheating section temperature of longitudinal stretching is 130°C, the stretching section temperature is 142°C, the shaping section temperature is 145°C, the longitudinal stretching ratio is 4.9, the preheating section temperature of transverse stretching is 167°C, the stretching section temperature is 155°C, the shaping section temperature is 171°C, the transverse stretching ratio is 9 times, and the corona is 34.

[0023] Furthermore, the polypropylene pearlescent film is used in facial mask base materials.

[0024] Due to the adoption of the above technical solution, the beneficial effects of the present invention include:

[0025] (1) The present invention prepares a modified xanthan gum copolymer with antistatic and compatibilizing properties by graft copolymerization of xanthan gum with methyl methacrylate and methacryloyloxyethyl trimethyl ammonium chloride. The prepared modified xanthan gum copolymer is added to a polypropylene pearlescent film to improve the antistatic properties of the antistatic layer of the pearlescent film and the natural degradation rate of the polypropylene pearlescent film.

[0026] (2) Xanthan gum itself is an anionic polymer with a certain antistatic effect, but its antistatic performance is relatively weak. By grafting methacryloyloxyethyl trimethylammonium chloride onto xanthan gum, an amphoteric modified xanthan gum is prepared, which improves the antistatic performance of xanthan gum; by grafting methyl methacrylate onto xanthan gum, the compatibility of xanthan gum and polypropylene is improved. The reason is that the polypropylene of the present application is a random copolymer of polypropylene grafted with methyl methacrylate, and the two contain the same functional groups, thereby improving the compatibility of the two and avoiding the instability of the performance of the polypropylene pearlescent film due to compatibility problems; xanthan gum belongs to the carbohydrate polysaccharide class and is easily biodegraded naturally. Therefore, the polypropylene pearlescent film prepared in the present application has excellent natural degradation performance. DETAILED DESCRIPTION

[0027] The invention will be further described below in conjunction with the embodiments, but the invention is not limited to these embodiments.

[0028] Example 1 Preparation of modified xanthan gum copolymer:

[0029] Under nitrogen protection, 900 g of deionized water and 300 g of xanthan gum were added to the reaction bottle, stirred and mixed, and the temperature was raised to 40°C; 80 g of ethanol solution of methyl methacrylate (30 wt%), 30 g of methacryloyloxyethyltrimethylammonium chloride solution (80 wt%), and 5 g of ammonium persulfate solution (0.1 mol / L) were slowly added to the reaction bottle at the same time, and the addition was continued for 0.5 h. The graft copolymerization reaction was carried out for 1 h. The mixture was cooled to room temperature, 500 g of acetone was added, stirred and precipitated, and filtered to obtain a modified xanthan gum copolymer.

[0030] Example 2 Preparation of modified xanthan gum copolymer:

[0031] Under nitrogen protection, 900 g of deionized water and 300 g of xanthan gum were added to the reaction bottle, stirred and mixed, and the temperature was raised to 45°C; 90 g of ethanol solution of methyl methacrylate (28 wt%), 40 g of methacryloyloxyethyltrimethylammonium chloride solution (75 wt%), and 8 g of ammonium persulfate solution (0.08 mol / L) were slowly added to the reaction bottle at the same time, and the addition was continued for 1 hour. The graft copolymerization reaction was carried out for 1.5 hours, and the mixture was cooled to room temperature. 500 g of acetone was added, stirred and precipitated, and filtered to obtain a modified xanthan gum copolymer.

[0032] Example 3 Preparation of modified xanthan gum copolymer:

[0033] Under nitrogen protection, 900 g of deionized water and 300 g of xanthan gum were added to the reaction bottle, stirred to dissolve and mix, and the temperature was raised to 50°C; 100 g of ethanol solution of methyl methacrylate (25 wt%), 50 g of methacryloyloxyethyltrimethylammonium chloride solution (70 wt%), and 10 g of ammonium persulfate solution (0.05 mol / L) were slowly added to the reaction bottle at the same time, and the addition was continued for 1 hour. The graft copolymerization reaction was carried out for 2 hours, and the mixture was cooled to room temperature. 500 g of acetone was added, stirred, precipitated, and filtered to obtain a modified xanthan gum copolymer.

[0034] Example 4

[0035] A polypropylene pearlescent film, with a thickness of 0.20 mm, an outer layer and an inner layer having a thickness of 0.06 mm, and an intermediate layer having a thickness of 0.08 mm; the outer layer is composed of raw materials of: polypropylene: 150 g, polypropylene carbonate: 200 g, xanthan gum: 200 g, titanium dioxide: 10 g, organic pearlescent masterbatch: 80 g, calcium carbonate: 10 g, and antioxidant (2,6-di-tert-butyl-p-cresol): 10 g;

[0036] The raw material composition of the middle layer is: polypropylene: 200g, titanium dioxide: 10g, organic pearlescent masterbatch: 50g, modified xanthan gum copolymer (prepared in Example 1): 500g;

[0037] The raw material composition of the inner surface layer is: polypropylene: 150g, titanium dioxide: 10g, modified xanthan gum copolymer (prepared in Example 1): 350g.

[0038] Example 5

[0039] A polypropylene pearlescent film, with a thickness of 0.20 mm, an outer layer and an inner layer having a thickness of 0.06 mm, and an intermediate layer having a thickness of 0.08 mm; the outer layer has a raw material composition of: polypropylene: 180 g, polypropylene carbonate: 250 g, xanthan gum: 250 g, titanium dioxide: 15 g, organic pearlescent masterbatch: 100 g, calcium carbonate: 15 g, and an antioxidant (2,6-di(octadecyl)-4-methylphenol): 15 g;

[0040] The raw material composition of the middle layer is: polypropylene: 225g, titanium dioxide: 15g, organic pearlescent masterbatch: 80g, modified xanthan gum copolymer (prepared in Example 2): 550g;

[0041] The raw material composition of the inner surface layer is: polypropylene: 180g, titanium dioxide: 15g, modified xanthan gum copolymer (prepared in Example 2): 380g.

[0042] Example 6

[0043] A polypropylene pearlescent film, with a thickness of 0.20 mm, an outer layer and an inner layer having a thickness of 0.06 mm, and an intermediate layer having a thickness of 0.08 mm; the outer layer is composed of raw materials of: polypropylene: 200 g, polypropylene carbonate: 300 g, xanthan gum: 300 g, titanium dioxide: 20 g, organic pearlescent masterbatch: 150 g, calcium carbonate: 20 g, and antioxidant (2,6-di-tert-butyl-p-cresol): 20 g;

[0044] The raw material composition of the middle layer is: polypropylene: 250g, titanium dioxide: 20g, organic pearlescent masterbatch: 100g, modified xanthan gum copolymer (prepared in Example 3): 600g;

[0045] The raw material composition of the inner surface layer is: polypropylene: 200g, titanium dioxide: 20g, modified xanthan gum copolymer (prepared in Example 3): 400g.

[0046] Comparative Example 1

[0047] The polypropylene pearlescent film in this comparative example is substantially the same as that in Example 5, except that the modified xanthan gum copolymer in the middle layer and the inner surface layer is replaced by an equal weight of unmodified xanthan gum.

[0048] Comparative Example 2

[0049] The polypropylene pearlescent film in this comparative example is basically the same as that in Example 5, except that the modified xanthan gum copolymer in the middle layer is replaced by 475 g of xanthan gum, 38 g of methyl methacrylate, and 38 g of methacryloyloxyethyltrimethylammonium chloride; and the modified xanthan gum copolymer in the inner surface layer is replaced by 328 g of xanthan gum, 27 g of methyl methacrylate, and 27 g of methacryloyloxyethyltrimethylammonium chloride.

[0050] Comparative Example 3

[0051] The polypropylene pearlescent film in this comparative example is substantially the same as that in Example 5, except that the modified xanthan gum copolymer in the middle layer and the inner surface layer is replaced by an equal weight of modified lignin, and the modified lignin is prepared by the following method:

[0052] Under nitrogen protection, 900 g of deionized water and 300 g of syringyl lignin were added to the reaction bottle, stirred to dissolve and mix, and the temperature was raised to 45 ° C; 90 g of methyl methacrylate ethanol solution (28 wt%), 40 g of methacryloyloxyethyl trimethyl ammonium chloride solution (75 wt%), and 8 g of ammonium persulfate solution (0.08 mol / L) were slowly added to the reaction bottle at the same time, and the addition was continued for 1 hour. The graft copolymerization reaction was carried out for 1.5 hours, and the mixture was cooled to room temperature. 500 g of acetone was added, stirred and precipitated, and filtered to obtain a modified lignin copolymer.

[0053] Comparative Example 4

[0054] The polypropylene pearlescent film in this comparative example is basically the same as that in Example 5, except that the modified xanthan gum copolymer in the middle layer and the inner surface layer is replaced with an equal weight of unmodified xanthan gum, and 38 g and 27 g of AS11N type antistatic agent are added to the middle layer and the inner surface layer, respectively.

[0055] Comparative Example 5

[0056] The polypropylene pearlescent film is prepared by the method in Example 2 of the Chinese invention patent application with publication number CN112721370A.

[0057] The titanium dioxide used in the examples and comparative examples of the present application is DuPont R-706, the calcium carbonate is KJ-106, and the weight average molecular weight of polypropylene carbonate is 1.3×10 5 The pearlescent masterbatch was ZG905, the polypropylene was a random copolymer of polypropylene grafted with methyl methacrylate (TPC COSMOPLENE, brand FL7540L), and the xanthan gum was purchased from Shandong Fufeng Fermentation Co., Ltd.

[0058] The polypropylene pearlescent films of Examples 4-6 and Comparative Examples 1-4 of the present application were prepared by the following process:

[0059] S1: Extruding the outer layer raw material, the middle layer raw material and the inner layer raw material through an extruder respectively;

[0060] S2: extruding each layer of raw materials extruded by the extruder through a T-type die, and then longitudinally stretching and transversely stretching, followed by cooling, corona treatment of the outer layer, and trimming;

[0061] Among them, the extrusion temperature of the outer layer raw material and the inner layer raw material is 230°C, and the extrusion temperature of the middle layer raw material is 250°C; the preheating section temperature of longitudinal stretching is 130°C, the stretching section temperature is 142°C, the shaping section temperature is 145°C, the longitudinal stretching ratio is 4.9, the preheating section temperature of transverse stretching is 167°C, the stretching section temperature is 155°C, the shaping section temperature is 171°C, the transverse stretching ratio is 9 times, and the corona is 34.

[0062] The polypropylene pearlescent films prepared in Examples 4-6 and Comparative Examples 1-5 were subjected to antistatic tests and degradation rate tests for the antistatic layer (inner surface layer). The antistatic test was performed according to GB / T 1410-2006 "Test Method for Volume Resistivity and Surface Resistivity of Solid Insulating Materials", and the degradation rate was tested for 120 days according to the method of ASTM D5511-2018 standard. The test results are shown in Table 1.

[0063] Table 1 Test results of antistatic and degradation rate of polypropylene pearlescent films prepared in Examples 4-6 and Comparative Examples 1-5

[0064]

[0065] It can be seen from the data of Examples 4, 5 and 6 in Table 1 that the surface resistance of the antistatic layer of the polypropylene pearlescent film prepared in this application is less than 3.9×10 8 Ω, the degradation rate is higher than 60%, with excellent antistatic properties and natural degradation properties.

[0066] Comparative Examples 1, 2, 3, and 4 are comparative examples of replacing modified xanthan gum with unmodified xanthan gum, unmodified xanthan gum with a mixture of methyl methacrylate and methacryloyloxyethyl trimethyl ammonium chloride, modified lignin, unmodified xanthan gum, and AS11N antistatic agent. It can be seen from the data in Table 1 that the surface resistance of the antistatic layer is greater than 7.6×10 8 Ω, the degradation rate is comparable to that of Examples 4-6.

[0067] Comparative Example 5 is a polypropylene pearlescent film prepared by the method of Example 2 of Chinese invention patent application with publication number CN112721370A, and its degradation rate is only 32.7%.

[0068] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. However, any equivalent changes, modifications and evolutions made by ordinary technicians in the field without departing from the scope of the technical solution of the present invention by using the technical content disclosed above are all equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.

Claims

1. A polypropylene pearlescent film, consisting of an outer layer, an intermediate layer and an inner layer, It is characterized in that The outer layer is composed of the following raw materials in parts by weight: polypropylene: 15-20 parts, polypropylene carbonate: 20-30 parts, xanthan gum: 20-30 parts, titanium dioxide: 1-2 parts, organic pearlescent masterbatch: 8-15 parts, calcium carbonate: 1-2 parts, antioxidant: 1-2 parts; The middle layer is composed of the following raw materials in parts by weight: polypropylene: 20-25 parts, titanium dioxide: 1-2 parts, organic pearlescent masterbatch: 5-10 parts, modified xanthan gum copolymer: 50-60 parts; The inner surface layer is composed of the following raw materials in parts by weight: polypropylene: 15-20 parts, titanium dioxide: 1-2 parts, modified xanthan gum copolymer: 35-40 parts; The modified xanthan gum copolymer is prepared by graft copolymerization of xanthan gum with methyl methacrylate and methacryloyloxyethyl trimethylammonium chloride; The modified xanthan gum copolymer is prepared by the following method: Under nitrogen protection, deionized water and xanthan gum were added to the reaction bottle, stirred and mixed, and the temperature was raised to 40-50° C.; methyl methacrylate ethanol solution, methacryloyloxyethyl trimethyl ammonium chloride solution, and ammonium persulfate solution were slowly added to the reaction bottle at the same time, and the addition was carried out for 0.5-1 h, and the graft copolymerization reaction was carried out for 1-2 h to obtain a modified xanthan gum copolymer; The mass ratio of the xanthan gum, methyl methacrylate ethanol solution, methacryloyloxyethyl trimethyl ammonium chloride solution, and ammonium persulfate solution is 30:(8-10):(3-5):(0.5-1); The concentration of the ammonium persulfate solution is 0.05-0.1 mol / L; The concentration of the methyl methacrylate ethanol solution is 25-30wt%; The methacryloyloxyethyl trimethyl ammonium chloride solution is a 70-80wt% aqueous solution; The polypropylene is a random copolymer of polypropylene grafted with methyl methacrylate.

2. A polypropylene pearlescent film according to claim 1, It is characterized in that The antioxidant is one of 2,6-di-tert-butyl-p-cresol and 2,6-di(octadecyl)-4-methylphenol.

3. A method for preparing the polypropylene pearlescent film according to any one of claims 1 to 2, It is characterized in that The following steps are involved: S1: Extruding the outer layer raw material, the middle layer raw material and the inner layer raw material through an extruder respectively; S2: extruding each layer of raw materials extruded by the extruder through a T-type die, and then longitudinally stretching and transversely stretching, followed by cooling, corona treatment of the outer layer, and trimming; Among them, the extrusion temperature of the outer layer raw material and the inner layer raw material is 230°C, and the extrusion temperature of the middle layer raw material is 250°C; the preheating section temperature of longitudinal stretching is 130°C, the stretching section temperature is 142°C, the shaping section temperature is 145°C, the longitudinal stretching ratio is 4.9, the preheating section temperature of transverse stretching is 167°C, the stretching section temperature is 155°C, the shaping section temperature is 171°C, the transverse stretching ratio is 9 times, and the corona is 34.

4. Application of the polypropylene pearlescent film according to any one of claims 1 to 2 in a facial mask base material.