A titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material and a preparation method thereof
By using components such as zirconium oxide, tabular corundum and nano-alumina, a stable refractory material is formed, which solves the problem of insufficient anti-penetration and anti-erosion properties of traditional aluminum-zirconium refractory materials at high temperatures, achieving higher fire-resistant performance and service life.
Patent Information
- Application Number
- CN202411036261.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-31
AI Technical Summary
Traditional aluminum-zirconium refractory materials have problems with insufficient anti-penetration and anti-erosion properties at high temperatures. Especially during the metal smelting process, they are easily penetrated and corroded by liquid or vapor electrolytes, resulting in structural damage to the material.
Using zirconia and plate-like corundum as the main raw materials, titanium oxide and samarium oxide are added to form aluminum titanate, which is combined with nano-alumina to form a micropore structure, stabilize the crystal form of zirconia, and improve the anti-penetration and anti-erosion properties of the material.
Significantly improves the anti-penetration and anti-erosion properties of refractory materials, extends their service life, and enhances the thermal shock stability and mechanical properties of the material.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of refractory materials, and in particular relates to a titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material and a preparation method thereof. Background Art
[0002] Traditional refractory materials are made of natural ores (such as refractory clay, silica, dolomite, etc.). With the advancement of technology, more and more industrial and synthetic raw materials are used in the manufacture of refractory materials. Therefore, there are many types of refractory materials on the market, such as silicon oxide, aluminum silicate, dolomite, spinel, carbonaceous, zirconium-containing and special refractory materials. In recent years, zirconium-containing refractory materials have developed into a very important special refractory material.
[0003] Aluminum-zirconium refractory materials are widely used in the preparation of functional refractory devices for continuous casting, such as metal smelting furnaces. During the melting process of the smelting furnace, the molten pool needs to frequently receive new materials, and the solution temperature fluctuates greatly. The upper solution of the molten pool is an acidic high-silicon solution, and the lower part is an iron-rich residue, which also contains a large amount of calcium oxide, magnesium oxide, potassium oxide, sodium oxide, etc., that is, alkaline components. Therefore, the lining material of the pool wall is required to have both excellent acid corrosion resistance and excellent alkali corrosion resistance. The Chinese patent application document with the publication number CN107311624A discloses an anti-erosion gunning material, wherein clay, glass fiber and quartz are mixed and sieved to obtain a mixed powder, acrylic acid is then mixed with sodium hydroxide solution and stirred with the mixed powder and sodium dodecylbenzene sulfonate to obtain an emulsified mixed solution, and the emulsified mixed solution is reacted with Tween-80, ammonium persulfate and the like to obtain a binder, and graphite, alumina and rice husk are crushed and sieved and then calcined to obtain a calcined product, which is ball-milled and sieved with zirconium boride and aluminum magnesium spinel and then fully stirred with magnesia, high-alumina bauxite, binder and the like to obtain an anti-erosion gunning material. The gunning material obtained by this method has good high temperature strength, good volume stability and excellent erosion resistance when used, and is an ideal material for hot repair of refractory components, but it does not have the performance of being resistant to both acid erosion and alkali erosion.
[0004] In addition, during the metal smelting process, the traditional aluminum electrolytic cell refractory materials will be penetrated and eroded by the liquid or vapor electrolyte in the cell at high temperature, resulting in the destruction of the refractory structure. How to improve the anti-permeability performance of refractory materials is also a technical problem that restricts the development of refractory materials. The Chinese patent application document with publication number CN107352978A discloses a high-strength anti-seepage brick and its preparation process, the formula of which includes special high-alumina bauxite clinker with a particle diameter of 3mm≤d<5mm, special high-alumina bauxite clinker with a particle diameter of 1mm≤d<3mm, fused magnesia with a particle diameter of 1mm≤d<3mm, fused magnesia with a particle diameter of 0.1mm≤d<1mm, zirconium concentrate powder with a particle diameter of 0.1mm≤d<1mm containing zirconium greater than or equal to 65%, chromium concentrate, composite clay with a ratio of Guangxi clay: Suzhou kaolin of 1:1, fused magnesia aluminum spinel powder, fused magnesia powder, and andalusite micropowder. After the components are mixed and formed into green bricks, they are sent to the drying room for drying until the residual moisture of the green bricks is ≤1%; they are fired in a high-temperature tunnel kiln, using natural gas as fuel, and the temperature is controlled at 1500-1600°C; this makes the high-strength anti-seepage bricks have good thermal shock stability, strong anti-seepage and anti-corrosion capabilities, and long service life. Summary of the invention
[0005] In order to solve the technical problems of poor anti-permeability and poor anti-erosion performance existing in the related art, the purpose of the present invention is to provide a titanium-doped anti-permeability and anti-corrosion aluminum-zirconium refractory material and a preparation method thereof.
[0006] In order to achieve the above object, the technical solution of the present invention is as follows:
[0007] A titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material comprises the following components and their weight proportions: 20-30 parts of zirconium oxide, 30-50 parts of plate-shaped corundum, 5-10 parts of additives, and 3-8 parts of binders; the additives are composed of titanium oxide and samarium oxide in a mass ratio of 14-17:3-6.
[0008] In the present invention, zirconium oxide and plate-shaped corundum are used as the main raw materials to prepare the refractory material. The crystal structure of alumina is dense, so it is not easily affected by oxidation and corrosion. At high temperatures, alumina ceramics have high thermal stability and thermal shock strength and can withstand the erosion of high-temperature gas flow. Monoclinic zirconium oxide undergoes a phase change at 1000°C-1200°C and transforms into tetragonal zirconium oxide, resulting in volume shrinkage. After the temperature is reduced, the tetragonal zirconium oxide will transform back to monoclinic zirconium oxide, resulting in volume expansion and the generation of microcracks, which has the effect of microcrack toughening on the refractory material and improves the thermal shock resistance of the material, but the material's anti-permeability and anti-erosion properties will deteriorate. When the temperature exceeds 2370℃, the tetragonal zirconium oxide will transform into the cubic zirconium oxide. The cubic zirconium oxide will not change the lattice due to the decrease of temperature, but the sintering temperature of the refractory material during the preparation process cannot reach 2370℃. Therefore, the present invention stabilizes or partially stabilizes the crystal form of zirconium oxide in the tetragonal phase by adding additives, so that it does not undergo drastic volume changes, reduces the generation of microcracks inside the refractory material, and thus improves the anti-permeability and anti-erosion properties. Titanium oxide and aluminum oxide can form aluminum titanate during the sintering process, which has a low thermal expansion coefficient and good thermal shock stability, but aluminum titanate will decompose at 1200℃, and aluminum titanate crystals are prone to form microcracks inside the material when cooling, affecting the mechanical strength of the material; the inventor has found through research that samarium oxide can play a pinning role inside the crystal, which can greatly reduce the microcracks that appear when the aluminum titanate crystal is cooled, and improve the volume density of the refractory material, thereby improving the anti-permeability and anti-erosion properties. In addition, the addition of samarium oxide can form a solid solution with zirconium oxide at high temperature, avoiding the generation of microcracks caused by the crystal transformation of zirconium oxide.
[0009] Furthermore, the particle size of the additive in the titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material is 150-200nm.
[0010] Furthermore, the binder in the titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material is one of ammonium phosphate, aluminum dihydrogen phosphate, and sodium tripolyphosphate.
[0011] Furthermore, the titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material includes the following components and their weight proportions: 27 parts of zirconium oxide, 43 parts of plate-shaped corundum, 8 parts of additives, and 6 parts of binders; the additives are composed of titanium oxide and samarium oxide in a mass ratio of 16:5.
[0012] Furthermore, the titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material also includes a composite refractory coating component, which includes the following components and their weight proportions: 20-30 parts of nano-alumina, 5-10 parts of sodium dodecylbenzene sulfonate, 3-6 parts of sodium silicate, and 40-50 parts of water.
[0013] In the present invention, nano-alumina is used to form an alumina nano-precursor on the surface of the titanium-doped corrosion-resistant aluminum-zirconium refractory material through a vacuum impregnation method, and a microporous structure is formed on the surface of the refractory material, making it difficult for the corrosive medium to penetrate through the pores of the refractory material, thereby effectively blocking the entry of the corrosive medium; in addition, the nano-alumina forms a nano-coating on the surface of the titanium-doped corrosion-resistant aluminum-zirconium refractory material to prevent the corrosive medium from wetting the refractory material, effectively reducing the penetration of the corrosive medium into the refractory material, thereby improving the permeability resistance and corrosion resistance of the refractory material.
[0014] Furthermore, the particle size of the nano-alumina is 200-300nm.
[0015] The present invention also provides a method for preparing the titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material, comprising the following steps:
[0016] S1: Grinding and sieving zirconium oxide and plate-like corundum to obtain zirconium oxide powder and plate-like corundum powder respectively;
[0017] S2: mixing the zirconium oxide powder and the plate-like corundum powder obtained in step S1 uniformly, grinding them together, adding additives, spraying an aqueous solution of a binder after mixing them uniformly, grinding them together, and obtaining an embryo mud material;
[0018] S3: pressing the embryo mud obtained in step S2 into a shape to obtain a rough brick, drying, heating, sintering, and cooling to obtain a refractory brick;
[0019] S4: uniformly mix the components in the composite refractory coating, add the refractory bricks obtained in step S3, evacuate the mixture, heat up for reaction, take out the refractory bricks after cooling, heat up, sinter, and cool to obtain a titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material.
[0020] Furthermore, the screening in step S1 of the method for preparing the titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material is through a 200-mesh sieve.
[0021] Furthermore, the mass percentage of the aqueous solution of the binder in step S2 of the method for preparing the titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material is 23-27%.
[0022] Furthermore, in step S3 of the preparation method of titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material, the drying temperature is 80-90°C, the heating rate is 20-30°C / h, the sintering temperature is 1700-1850°C, the sintering time is 24-28h, and the cooling rate is 40-60°C / h.
[0023] Furthermore, in the preparation method of titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material, the temperature of the heating reaction in step S4 is 120-130°C, and the reaction time is 2-3h; the heating rate is 40-50°C / h, the sintering temperature is 1000-1300°C, the sintering time is 1-1.5h, and the cooling rate is 30-40°C / h.
[0024] Compared with the prior art, the titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material and the preparation method thereof provided by the present invention have the following technical advantages:
[0025] (1) In the present invention, zirconium oxide and plate-shaped corundum are used as the main raw materials to prepare the refractory material. The crystal structure of alumina is dense and not easily affected by oxidation and corrosion. At high temperatures, alumina ceramics have high thermal stability and thermal shock strength and can withstand the erosion of high-temperature gas flow;
[0026] (2) In the present invention, by adding additives, the crystal form of zirconium oxide is stabilized or partially stabilized in the tetragonal phase, so that it does not undergo drastic volume changes, reducing the generation of microcracks inside the refractory material, thereby improving the anti-penetration and anti-erosion properties.
[0027] (3) In the present invention, nano-alumina is used to form an alumina nano-precursor on the surface of the titanium-doped corrosion-resistant aluminum zirconium refractory material through a vacuum impregnation method, and a nano-coating with a microporous structure is formed on the surface of the refractory material, making it difficult for the corrosive medium to wet and penetrate through the pores of the refractory material, thereby improving the permeability resistance and corrosion resistance of the refractory material. DETAILED DESCRIPTION
[0028] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments. Those skilled in the art can make various modifications based on the basic idea of the present invention, but as long as they do not deviate from the basic idea of the present invention, they are all within the scope of the present invention.
[0029] Example 1
[0030] A titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material comprises the following components and their weight proportions: 20 parts of zirconium oxide, 50 parts of plate-shaped corundum, 5 parts of an additive with a particle size of 150 nm, and 3 parts of sodium tripolyphosphate; 20 parts of nano-alumina with a particle size of 200 nm, 5 parts of sodium dodecylbenzene sulfonate, 3 parts of sodium silicate, and 50 parts of water; the additive is composed of titanium oxide and samarium oxide in a mass ratio of 14:3.
[0031] The preparation method of the titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material comprises the following steps:
[0032] S1: Grinding zirconium oxide and plate-like corundum respectively, and passing through a 200-mesh sieve to obtain zirconium oxide powder and plate-like corundum powder respectively;
[0033] S2: the zirconium oxide powder and the plate-like corundum powder obtained in step S1 are mixed evenly, mixed and ground, additives are added, and after mixing evenly, a 27% by mass binder aqueous solution is sprayed into the mixture, and mixed and ground to obtain an embryo mud material;
[0034] S3: pressing the embryo mud obtained in step S2 to obtain a rough brick, drying it at 90°C, heating it to 1700°C at a rate of 30°C / h, sintering it for 28h, cooling it, and controlling the cooling rate to 40°C / h to obtain a refractory brick;
[0035] S4: Evenly mix nano alumina, sodium dodecylbenzene sulfonate, sodium silicate and water, add the refractory bricks prepared in step S3, evacuate the mixture, heat to 120°C and react for 3 hours, take out the refractory bricks after cooling, heat to 1000°C at a rate of 50°C / h and sinter for 1.5 hours, cool, and control the cooling rate to 30°C / h to obtain titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material.
[0036] Example 2
[0037] A titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material comprises the following components and their weight proportions: 30 parts of zirconium oxide, 30 parts of plate-shaped corundum, 10 parts of an additive with a particle size of 200 nm, and 8 parts of ammonium phosphate; 30 parts of nano-alumina with a particle size of 300 nm, 10 parts of sodium dodecylbenzene sulfonate, 6 parts of sodium silicate, and 40 parts of water; the additive is composed of titanium oxide and samarium oxide in a mass ratio of 17:6.
[0038] The preparation method of the titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material comprises the following steps:
[0039] S1: Grinding zirconium oxide and plate-like corundum respectively, and passing through a 200-mesh sieve to obtain zirconium oxide powder and plate-like corundum powder respectively;
[0040] S2: the zirconium oxide powder and the plate-like corundum powder obtained in step S1 are mixed evenly, mixed and ground, additives are added, and after mixing evenly, a 23% by mass binder aqueous solution is sprayed into the mixture, and mixed and ground to obtain an embryo mud material;
[0041] S3: pressing the embryo mud obtained in step S2 to obtain a rough brick, drying it at 80°C, heating it to 1850°C at a rate of 20°C / h, sintering it for 24h, cooling it, and controlling the cooling rate to 60°C / h to obtain a refractory brick;
[0042] S4: Evenly mix nano alumina, sodium dodecylbenzene sulfonate, sodium silicate and water, add the refractory bricks prepared in step S3, evacuate the mixture, heat to 130°C and react for 2 hours, take out the refractory bricks after cooling, heat to 1300°C at a rate of 40°C / h and sinter for 1 hour, cool, and control the cooling rate to 40°C / h to obtain titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material.
[0043] Example 3
[0044] A titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material comprises the following components and their weight proportions: 27 parts of zirconium oxide, 43 parts of plate-shaped corundum, 8 parts of 185nm additives, 6 parts of aluminum dihydrogen phosphate; 27 parts of nano-alumina with a particle size of 255nm, 8 parts of sodium dodecylbenzene sulfonate, 5 parts of sodium silicate, and 47 parts of water; the additives are composed of titanium oxide and samarium oxide in a mass ratio of 16:5.
[0045] The preparation method of the titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material comprises the following steps:
[0046] S1: Grinding zirconium oxide and plate-like corundum respectively, and passing through a 200-mesh sieve to obtain zirconium oxide powder and plate-like corundum powder respectively;
[0047] S2: the zirconium oxide powder and the plate-like corundum powder obtained in step S1 are mixed evenly, mixed and ground, additives are added, and after mixing evenly, a 25% by mass binder aqueous solution is sprayed into the mixture, and mixed and ground to obtain an embryo mud material;
[0048] S3: pressing the embryo mud obtained in step S2 into a shape to obtain a rough brick, drying it at 88°C, heating it to 1800°C at a rate of 27°C / h, sintering it for 26h, cooling it, and controlling the cooling rate to 47°C / h to obtain a refractory brick;
[0049] S4: Evenly mix nano alumina, sodium dodecylbenzene sulfonate, sodium silicate and water, add the refractory bricks prepared in step S3, evacuate the mixture, heat to 126°C and react for 2.5h, take out the refractory bricks after cooling, heat to 1250°C at a rate of 45°C / h and sinter for 1.2h, cool, and control the cooling rate to 36°C / h to obtain titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material.
[0050] Comparative Example 1
[0051] The refractory material described in this comparative example is similar to that in Example 3. The difference between this comparative example and Example 3 is that the additive described in this comparative example is titanium oxide.
[0052] Comparative Example 2
[0053] The refractory material described in this comparative example is similar to that in Example 3. The difference between this comparative example and Example 3 is that an equal amount of yttrium oxide is used in this comparative example to replace the samarium oxide in the additive.
[0054] Comparative Example 3
[0055] The refractory material described in this comparative example is similar to that in Example 3. The difference between this comparative example and Example 3 is that the additive in this comparative example consists of titanium oxide and samarium oxide in a mass ratio of 5:16.
[0056] Comparative Example 4
[0057] The refractory material described in this comparative example is similar to that in Example 3. The difference between this comparative example and Example 3 is that in this comparative example, alumina with an equal particle size of 100 μm is used instead of nano alumina.
[0058] Comparative Example 5
[0059] The refractory material described in this comparative example is similar to that in Example 3. The difference between this comparative example and Example 3 is that in this comparative example, zirconium oxide with an equal particle size of 255 nm is used instead of nano alumina.
[0060] Test example
[0061] Test of anti-permeability and anti-erosion performance: The preparation method of refractory materials in Example 1-Example 3 and Comparative Example 1-Comparative Example 5 is as follows: In step S3, the embryo mud is pressed into a crucible shape, the outer size of the crucible is 10×10 cm, the diameter and depth of the crucible hole are 6 cm, and the other steps remain unchanged to obtain each group of test samples; the steel slag is ground into fine powder by a vibration mill, poured into the test sample after heat treatment, and tested at 1500°C in a buried carbon environment. The heating system is 20-200°C, 5°C / min; 200-1000°C, 10°C / min; 1000-1500°C, 5°C / min; 1500°C insulation for 3h. The weight of the test sample before the experiment is weighed m0, and after the experiment, it is cooled, the steel slag is poured out, and the weight of the test sample after the experiment is weighed m1, and the erosion rate of the test sample is calculated, and the erosion rate = (m0-m1) / m0×100%. The XRF analysis results of the steel slag are shown in Table 1. The test results are shown in Table 2.
[0062] Table 1 XRF composition analysis of steel slag
[0063]
[0064] Mechanical strength test: The maximum load that the refractory materials prepared in Examples 1 to 3 and Comparative Examples 1 to 3 can withstand was measured using a WE-300.600 hydraulic universal material testing machine, and the room temperature compressive strength was calculated. The test results are shown in Table 3.
[0065] Table 2 Test results of anti-penetration performance and anti-erosion performance
[0066]
[0067] It can be seen from Table 2 that the erosion rates of the test samples in Example 1 to Example 3 after the test are 4.53-5.44%, which indicates that the titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material provided by the present invention has good anti-penetration and anti-corrosion properties, among which the erosion rate of the test samples in Example 3 is the lowest, which is the best embodiment of the present invention.
[0068] Compared with Example 3, in Comparative Example 1, an equal amount of titanium oxide was used to replace samarium oxide, but the erosion rate increased, which shows that the addition of samarium oxide can effectively reduce the occurrence of microcracks in the test sample and improve the volume density of the material; in Comparative Example 2, an equal amount of yttrium oxide was used to replace the samarium oxide in the additive, but the erosion rate increased, which shows that not all rare metal oxides can play the role of samarium oxide; in Comparative Example 3, the mass ratio of titanium oxide and samarium oxide was changed, but the erosion rate increased, which shows that the components and amounts of the additives in the present invention have been optimized; in Comparative Example 4, micron-grade alumina was used to replace nano alumina, but the erosion rate increased significantly, which shows that the nano alumina in the present invention can form a microporous structure and a nano coating on the surface of the refractory material, effectively reduce the penetration of steel slag into the refractory material, thereby improving the permeability resistance and erosion resistance; in Comparative Example 5, nano zirconium oxide was used to replace nano alumina, but the erosion rate increased, which shows that not all nano oxides can play the technical effect of nano alumina.
[0069] Table 3 Mechanical properties test results
[0070]
[0071] As shown in Table 3, the compressive strength of the refractory materials obtained in Examples 1 to 3 is 132-145MPa, and has good mechanical properties. Compared with Example 3, in Comparative Example 1, an equal amount of titanium oxide is used to replace samarium oxide, but the compressive strength of the refractory material obtained is greatly reduced, which shows that the addition of samarium oxide can greatly reduce the generation of microcracks inside the crystal and improve the mechanical properties of the refractory material; in Comparative Example 2, an equal amount of yttrium oxide is used to replace the samarium oxide in the additive, but the compressive strength is reduced, which shows that the effect of yttrium oxide is worse than that of samarium oxide, and not all rare metal oxides can achieve the technical effect of samarium oxide; in Comparative Example 3, the mass ratio of titanium oxide and samarium oxide is changed, but the compressive strength is reduced, which shows that the mass ratio of titanium oxide and samarium oxide in the present invention has been optimized.
[0072] The above embodiments are only preferred embodiments of the present invention, and are not intended to limit the present invention. Any person skilled in the art shall not modify the above embodiments without violating the spirit and scope of the present invention. Therefore, any modification, equivalent substitution and improvement made by those skilled in the art under the technical concept of the present invention shall still be covered by the claims of the present invention.
Claims
1. A titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material, characterized in that: The invention comprises the following components and their weight proportions: 20-30 parts of zirconium oxide, 30-50 parts of plate-shaped corundum, 5-10 parts of additives, and 3-8 parts of binders; the additives are composed of titanium oxide and samarium oxide in a mass ratio of 14-17:3-6; The titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material also includes a composite refractory coating component, which includes the following components and their weight proportions: 20-30 parts of nano-alumina, 5-10 parts of sodium dodecylbenzene sulfonate, 3-6 parts of sodium silicate, and 40-50 parts of water.
2. The titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material according to claim 1 is characterized in that: The particle size of the additive is 150-200 nm.
3. The titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material according to claim 1 is characterized in that: The binder is one of ammonium phosphate, aluminum dihydrogen phosphate and sodium tripolyphosphate.
4. The titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material according to claim 1, characterized in that: The invention comprises the following components and their weight proportions: 27 parts of zirconium oxide, 43 parts of plate-shaped corundum, 8 parts of additives and 6 parts of binders; the additives are composed of titanium oxide and samarium oxide in a mass ratio of 16:
5.
5. The titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material according to claim 1, characterized in that: The particle size of nano-alumina is 200-300nm.
6. The method for preparing the titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1: Grinding and sieving zirconium oxide and plate-like corundum to obtain zirconium oxide powder and plate-like corundum powder respectively; S2: mixing the zirconium oxide powder and the plate-like corundum powder obtained in step S1 uniformly, grinding them together, adding additives, spraying an aqueous solution of a binder after mixing them uniformly, grinding them together, and obtaining an embryo mud material; S3: pressing the embryo mud obtained in step S2 into a shape to obtain a rough brick, drying, heating, sintering, and cooling to obtain a refractory brick; S4: uniformly mix the components in the composite refractory coating, add the refractory bricks obtained in step S3, evacuate the mixture, heat up for reaction, take out the refractory bricks after cooling, heat up, sinter, and cool to obtain a titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material.
7. The method for preparing the titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material according to claim 6, characterized in that: The sieving in step S1 is through a 200-mesh sieve; the mass percentage of the aqueous solution of the binder in step S2 is 23-27%.
8. The method for preparing the titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material according to claim 6, characterized in that: In step S3, the drying temperature is 80-90°C, the heating rate is 20-30°C / h, the sintering temperature is 1700-1850°C, the sintering time is 24-28h, and the cooling rate is 40-60°C / h.
9. The method for preparing the titanium-doped anti-seepage and anti-corrosion aluminum-zirconium refractory material according to claim 6, characterized in that: The temperature of the temperature-raising reaction in step S4 is 120-130°C, and the reaction time is 2-3h; the heating rate is 40-50°C / h, the sintering temperature is 1000-1300°C, the sintering time is 1-1.5h, and the cooling rate is 30-40°C / h.
Citation Information
Patent Citations
Anti-erosion gunning mix
CN107311624A
High-strength seepage-proofing brick and preparation technology thereof
CN107352978A
Application of nanometer aluminum oxide-based composite ceramic coating
CN102443753A
Corrosion resistant ceramic paint and preparation method thereof
CN104403381A
Method for preparing anti-aging zirconia ceramic insert core
CN104944945A