A silicon carbide ceramic composite material and additive manufacturing method thereof

By using a 1.06μm wavelength ytterbium-doped fiber laser for selective laser printing of SiC ceramic composites, the problems of slow scanning speed and poor material performance of CO2 lasers are solved, and fast and accurate printing of high-content SiC ceramic composites and high-performance ceramics are achieved. Material manufacturing.

CN118561600BActive Publication Date: 2024-12-03SHANGHAI INST OF CERAMIC CHEM & TECH CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411046636.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-12-03
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The existing CO2 lasers are slow in SLS printing of SiC ceramic composite materials, and cannot achieve fast and accurate printing of high-content silicon carbide ceramic materials, and the material density and mechanical properties are poor.

Method used

Selected laser printing of SiC ceramic composite material was performed using a ytterbium-doped fiber laser with a wavelength of 1.06μm, combined with LSI technology to remove residual carbon, and densification was achieved by laser heating of SiC and binder.

Benefits of technology

It realizes rapid and accurate printing of higher content SiC ceramic composite materials, improves the density and mechanical properties of the material, and significantly improves manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118561600B_ABST
    Figure CN118561600B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of additive manufacturing technology, and specifically relates to a silicon carbide ceramic composite material and an additive manufacturing method thereof. The additive manufacturing method of the silicon carbide ceramic composite material comprises the following steps: (1) mixing SiC powder, a carbon source and a binder to obtain a composite powder; (2) using a fiber laser as a light source to perform selective laser printing on the obtained composite powder to obtain a silicon carbide blank; (3) performing a debonding treatment and a liquid phase reaction siliconization treatment on the silicon carbide blank to obtain the silicon carbide ceramic composite material. The additive manufacturing method of the present invention can achieve the printing of silicon carbide ceramic materials with a higher content, and the material has better density and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of additive manufacturing, and relates to a silicon carbide ceramic composite material and an additive manufacturing method thereof, and specifically to a preparation method of a SiC ceramic composite material that can be used for laser 3D printing (also known as selective laser sintering, SLS). Background Art

[0002] Additive manufacturing technology, also known as 3D printing technology, has developed significantly and rapidly in the past few decades and has received great attention. Its principle is based on the discrete stacking mechanism. The three-dimensional model is constructed and cut by computer CAD, and then the raw materials are deposited layer by layer under the control of the computer to construct the parts. Compared with traditional equal material manufacturing and subtractive manufacturing technology, additive manufacturing is not limited by molds or processing technology, solves the problem of difficult structural forming of complex-shaped products, reduces processing procedures, shortens processing cycles, and greatly saves processing costs. Moreover, the more complex the product structure, the more obvious the advantages of additive manufacturing. Therefore, it is widely used in the manufacture of polymers, metals and some ceramic components. In particular, for the manufacture of high-hardness and high-brittle materials such as SiC, additive manufacturing has incomparable advantages. Among them, laser 3D printing (also known as selective laser sintering, SLS) technology is one of the more mature technologies in additive manufacturing technology. Its working principle is: the raw material powder is spread on the powder bed by a roller or a scraper, and the powder is sintered by high-energy laser pulses to combine them together, and then the powder is spread and sintered, and so on until the part is completed. SLS molding is fast and simple, and can achieve rapid near-net-shape manufacturing of complex structural parts.

[0003] Laser technology has been widely used in modern manufacturing, medical treatment, communications and other fields, among which fiber lasers and CO 2 Lasers are two common types of lasers. Currently, the mainstream lasers for SLS printing are CO 2 Laser, CO 2 The light emission principle of laser is to use CO 2 The vibration of the molecules produces laser light, so CO 2 The laser has a relatively long working wavelength, generally 10.6 μm, which is more suitable for the processing of non-metallic materials. 2 Due to the limitation of laser device conditions, the laser scanning speed is often not high, which is not conducive to the rapid processing of SLS printing. 2 Lasers cannot print silicon carbide ceramic materials with higher content, and the density and mechanical properties of the materials are poor. Summary of the invention

[0004] In view of the above problems, the present invention provides an additive manufacturing method for silicon carbide ceramic composite materials, which preferably uses an ytterbium-doped fiber laser with a wavelength of 1.06 μm as a light source to perform selective laser printing of SiC ceramic composite materials, and uses the high scanning speed, high stability and small spot of the fiber laser to achieve fast and accurate printing of SiC ceramic composite materials with higher content. LSI technology is used to remove residual carbon, which reacts with molten Si to generate SiC to achieve densification.

[0005] In one aspect, the present invention provides a method for additive manufacturing of a silicon carbide ceramic composite material, comprising the following steps:

[0006] (1) SiC powder, a carbon source and a binder are mixed to obtain a composite powder; based on the total volume of the composite powder being 100 vol%, the volume of the SiC powder accounts for 55 to 75 vol%, the volume of the carbon source accounts for 5 to 25 vol%, and the volume of the binder accounts for 15 to 30 vol%;

[0007] (2) Using a fiber laser as a light source, the obtained composite powder is subjected to selective laser printing to obtain a silicon carbide blank; the parameters of the selective laser printing include: preheating the composite powder at 50-70° C. before printing; the laser wavelength is 0.8-1.5 μm, the spot size is 200-500 μm; the laser power is 60-150 W; the scanning speed is 15000-25000 mm / s; the layer thickness is 0.08-0.3 mm; and the scanning interval is 0.2-0.3 mm;

[0008] (3) The silicon carbide blank is subjected to a debonding treatment and a liquid phase reactive siliconizing treatment to obtain the silicon carbide ceramic composite material.

[0009] In the method for additive manufacturing of silicon carbide ceramic composite materials provided by the present invention, a fiber laser is selected to perform selective laser printing of SiC ceramic composite materials, and its operating wavelength is between 0.8 and 1.5 μm (preferably 1.0 to 1.2 μm), and the spot size is 200 to 500 μm. 2 The laser (520 μm) is smaller, the laser power is usually higher, and the scanning speed is faster, which is more conducive to the fast and precise processing of SLS printing.

[0010] Preferably, in step (1), based on the total volume of the composite powder being 100 vol%, the volume of the SiC powder accounts for 65-75 vol%, the volume of the carbon source accounts for 5-15 vol%, and the volume of the binder accounts for 15-30 vol%.

[0011] Preferably, in step (1), the particle size of the SiC powder is 5 to 80 μm; the density of the SiC powder is 3.0 to 3.3 g / cm 3 .

[0012] Preferably, in step (1), the carbon source is carbon fiber and / or graphite; the length of the carbon fiber is 30 to 200 μm; the diameter of the carbon fiber is 6 to 12 μm; the density of the carbon fiber is 1.50 to 2.50 g / cm 3 ; The particle size of the graphite is 20 to 50 μm; The density of the graphite is 1.5 to 2.5 g / cm 3 .

[0013] Preferably, in step (1), the binder is at least one of phenolic resin, epoxy resin, polyamide, urea-formaldehyde resin, asphalt resin and polyvinyl alcohol; the density of the binder is 0.8-1.5 g / cm 3 .

[0014] Preferably, in step (1), the mixing method is ball milling; the parameters of the ball milling mixing include: ball milling speed of 60 to 600 r / min, ball milling time of 2 to 12 h, and ball-to-material ratio of (2 to 5): 1;

[0015] After ball milling and mixing, the mixture is sieved; the mesh number of the sieve is 50 to 300 meshes.

[0016] Preferably, in step (2), the fiber laser is an ytterbium-doped fiber laser with a laser wavelength of 1.06 μm and a spot size of 200 μm.

[0017] Preferably, the parameters of the debonding treatment include: in a vacuum atmosphere, an inert atmosphere (such as an argon atmosphere) or a nitrogen atmosphere, first heating to 200 ° C at a heating rate of 1 to 3 ° C / min, then continuing to heat to 200 to 600 ° C at a heating rate of 0.25 to 2 ° C / min, and finally heating to 600 to 1200 ° C at a heating rate of 1 to 2 ° C / min and keeping warm for 30 to 120 minutes, and then filling with an inert atmosphere (such as an argon atmosphere) and cooling to room temperature.

[0018] Preferably, the parameters of the liquid phase reactive siliconization include: in an inert atmosphere (for example, an argon atmosphere) or a nitrogen atmosphere, first heating to 1200°C at a heating rate of 5 to 10°C / min, then continuing to heat to 1200 to 1400°C at a heating rate of 3 to 5°C / min, and finally heating to 1450 to 1700°C at a heating rate of 1 to 3°C / min and keeping warm for 30 to 60 min, then cooling to 1000 to 1300°C at a cooling rate of 1 to 5°C / min, and finally filling with an inert atmosphere (for example, an argon atmosphere) and cooling to room temperature.

[0019] In another aspect, the present invention provides a silicon carbide ceramic composite material prepared according to the above method, wherein the main components of the silicon carbide ceramic composite material include SiC, residual carbon and free silicon.

[0020] Preferably, the open porosity of the silicon carbide ceramic composite material is 0.67-2.15%; the density of the silicon carbide ceramic composite material is 97.85-99.33%; the bulk density of the silicon carbide ceramic composite material is 2.715-2.769 g / cm 3 ; The flexural strength of the silicon carbide ceramic composite material is 193.087 to 291.127 MPa; the elastic modulus of the silicon carbide ceramic composite material is 228.2339 to 300.7185 GPa; the fracture toughness of the silicon carbide ceramic composite material is 2.547 to 3.958 MPa·m 1 / 2 .

[0021] The additive manufacturing method adopted in the present invention can realize rapid laser 3D printing of silicon carbide ceramic composite materials, providing a basis for improving the printing speed and printing accuracy of 3D printed SiC ceramics.

[0022] Since fiber laser and CO 2 Different laser light emission principles lead to different wavelengths of light. Different materials have different absorption rates for different wavelengths of light during SLS printing. For example, SiC absorbs 1.06 μm light more strongly than 10.6 μm light, while organic adhesives absorb 10.6 μm light more strongly than 1.06 μm light. Therefore, for SLS printing of SiC ceramics, different lasers have different printing principles. 2 Laser printing mainly heats the adhesive directly when the laser scans, and the adhesive absorbs the 10.6 μm wavelength to soften it, while fiber laser printing heats the SiC particles to increase their temperature and transfer heat to the adhesive to soften it. The two soften the adhesive in different ways, so the connection effect and connection state during printing will be different, and the final performance of the silicon carbide ceramic composite material will also be different.

[0023] For the printing of high-content silicon carbide ceramic composites, the path scanned by the laser is mainly SiC. 2 When printing with a laser, the absorption of light at 10.6 μm is less, and the bonding state of the organic adhesive becomes worse. However, when printing with a fiber laser, the laser heats the SiC to soften the adhesive, and the heat is more uniform, resulting in a better bonding state. 2 Compared with lasers, fiber lasers have a deeper laser penetration depth, which is more conducive to transferring laser heat to the bottom, resulting in better printing effects. However, too low laser scanning power will cause the powder to be irradiated for a long time, and the viscosity of the powder will decrease after softening, resulting in poor bonding effect; too fast scanning speed cannot fully soften the organic adhesive to achieve bonding. Therefore, specific printing parameters are required to prevent the organic adhesive from being directly heated and carbonized by the high-power fiber laser, thereby achieving the printing of high-content silicon carbide ceramic composites.

[0024] Beneficial effects of the present invention:

[0025] Compared with the prior art, the present invention mainly has the following technical advantages:

[0026] (1) The laser produced by the fiber laser used in the present invention is more 2 Lasers have better beam quality: smaller focused spot, higher work efficiency, and are suitable for processing fine structures;

[0027] (2) The laser scanning speed (25000mm / s) generated by the fiber laser used in the present invention is much higher than that of CO 2 Laser (7620mm / s), wide scanning distance (0.18mm (CO 2 )→0.3mm (optical fiber) can shorten the scanning path, thus significantly improving manufacturing efficiency;

[0028] (3) The stability and photothermal conversion efficiency of the fiber laser used in this invention are much higher than those of CO 2 Laser. This method can be used for SLS rapid prototyping of metals, polymers and ceramics;

[0029] (4) The fiber laser used in the present invention can achieve the printing of silicon carbide ceramic materials with higher content, and the density and mechanical properties of the materials are better. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a SEM image of the silicon carbide ceramic composite material prepared in Example 8;

[0031] Figure 2The SEM images of the silicon carbide ceramic composite materials prepared in each embodiment and comparative example, wherein (a)-(j) are respectively embodiments 1-7, comparative example 7, comparative example 8, and comparative example 1;

[0032] Figure 3 are printed photos, wherein (k) is comparative example 2, and (l) is comparative example 3;

[0033] Figure 4 Thermogravimetric analysis of phenolic resin (PR). DETAILED DESCRIPTION

[0034] To further explain the content, characteristics and practical effects of the present invention, the present invention is described in detail below in conjunction with the embodiments. It should be pointed out that the modification method of the design of the present invention is not limited to these specific embodiments. Without departing from the spirit and connotation of the design of the present invention, the equivalent replacement and modification made by those skilled in the art on the basis of reading the content of the present invention are also within the scope of the present invention. In the absence of special instructions, each percentage refers to the volume percentage.

[0035] In the present invention, fiber laser is used to print silicon carbide ceramic composite materials. Fiber laser is more stable in use, light-to-heat conversion efficiency, cost and maintenance than CO 2 Lasers have great advantages and are more conducive to the application of fiber lasers in the rapid and precise selective laser printing and manufacturing of SiC ceramic composite materials. The SiC ceramic composite material prepared by the additive manufacturing method of the present invention has good density and mechanical properties, thereby expanding the use of fiber lasers in 3D printing SiC components.

[0036] The method of the present invention can realize rapid laser 3D printing of high-content silicon carbide ceramic composite materials, providing a basis for improving the printing speed and printing accuracy of 3D printed SiC ceramics. The following is an exemplary description of the additive manufacturing method of the silicon carbide ceramic composite material provided by the present invention.

[0037] Preparation of composite powder for laser 3D printing. SiC powder, carbon source and binder are ball-milled and sieved to obtain composite powder for laser 3D printing. Wherein, based on the total volume of the composite powder for laser 3D printing as 100 vol%, the volume proportion of SiC powder is 55-75 vol% (for example, 55 vol%, 60 vol%, 65 vol%, 70 vol%, 75 vol%, etc.), the volume proportion of carbon source is 5-25 vol% (for example, 5 vol%, 10 vol%, 15 vol%, 20, 25 vol%, etc.), and the volume proportion of binder is 15-30 vol% (for example, 15 vol%, 20 vol%, 25 vol%, 30 vol%, etc.). If the carbon source content is too high, the volume expansion of the silicon-carbon reaction during reaction sintering blocks the pores, so that the carbon inside the sample cannot fully react, forming a raw material, resulting in a decrease in the mechanical properties of the final ceramic sample.

[0038] In an optional embodiment, the particle size of the SiC powder may be 5 to 80 μm. The density of the SiC powder may be 3.0 to 3.3 g / cm 3 For example, the density is 3.20 g / cm 3 of SiC powder.

[0039] In an optional embodiment, the carbon source may be carbon fiber or graphite; the length of the carbon fiber may be 30 to 200 μm. The diameter of the carbon fiber may be 6 to 12 μm. The density of the carbon fiber may be 1.50 to 2.50 g / cm 3 For example, the density is 1.76 g / cm 3 The particle size of the graphite may be 20 to 50 μm. The density of the graphite may be 1.5 to 2.5 g / cm 3 For example, the density is 2.0 g / cm 3 of graphite.

[0040] In an optional embodiment, the binder is at least one of phenolic resin, epoxy resin, and polyamide; the density of the binder is 0.8 to 1.5 g / cm 3 For example, the density is 1.10 g / cm 3 Adhesive.

[0041] In an optional embodiment, the main component of the composite powder for laser 3D printing is 55-75 vol% of the particle size of 5-80 μm and the density of 3.20 g / cm 3 SiC powder, 5-25 vol%, length 30-200 μm, diameter 6-12 μm, density 1.76 g / cm 3Carbon fiber or particle size 20 ~ 50 μm, density 2.0 g / cm 3 Graphite, and 15-30 vol% with a density of 1.10 g / cm 3 Adhesive.

[0042] In an optional embodiment, the parameters of the ball milling include: the ball milling speed may be 60-600 r / min, the ball milling time may be 2-12 h, and the ball milling material ratio may be (2-5): 1. The mesh size of the sieving may be 50-300 meshes.

[0043] Preparation of silicon carbide blanks. Using fiber laser as light source, the composite powder is printed into silicon carbide blanks by laser 3D printing method.

[0044] In an optional embodiment, the laser wavelength of the fiber laser is 1.06 μm, and the spot size is 200 to 500 μm.

[0045] In an optional embodiment, the parameters of the laser 3D printing method include: preheating the composite powder at 50-70°C before printing; laser power of 60-150W; scanning speed of 15000-25000 mm / s; layer thickness of 0.08-0.3mm (for example, 0.08mm, 0.1mm, 0.15mm, 0.2mm, 0.25mm, 0.3mm, etc.); scanning spacing of 0.2-0.3 mm (for example, 0.2mm, 0.25mm, 0.3mm). For example, the laser power is 60 W, the scanning speed is 20000 mm / s, the layer thickness is 0.1 mm, and the scanning spacing is 0.3 mm. If the preheating temperature is low, the "fluidity" of the phenolic resin cannot be improved; if the preheating temperature is too high, the physical properties of the binder will change, and even have a certain viscosity, which is not conducive to the compact stacking and high-density blank molding. If the laser power is too high, the organic adhesive will absorb too much heat and directly lose the bonding effect or even carbonize. If the scanning speed is too low, it will cause a high printing point temperature to form a high temperature gradient and cause the printed part to warp and deform.

[0046] Debonding treatment. The obtained silicon carbide blank is subjected to debonding treatment to obtain the silicon carbide ceramic composite material. The parameters of the debonding treatment include: vacuum atmosphere, inert atmosphere (such as argon atmosphere) or nitrogen atmosphere; the temperature of the debonding treatment is 600 to 1200 °C; and the time of the debonding treatment is 400 to 800 min.

[0047] In an optional embodiment, the parameters of the debonding treatment include: first, the heating rate at 0 (or room temperature) to 200 ° C is 1 to 3 ° C / min; the heating rate at 200 to 600 ° C is 1 ° C / min; the heating rate at more than 600 ° C is 1 to 2 ° C / min, and after keeping at the highest temperature for 30 minutes, argon or nitrogen is filled to cool to room temperature. As an example, the silicon carbide blank is debonded for 657 minutes under vacuum and 900 ° C. The debonding system is 0 (or room temperature) to 200 ° C: heating rate 3 ° C / min; 200 to 600 ° C: heating rate 1 ° C / min; 600 to 900 ° C: heating rate 2 ° C / min, keep at 900 ° C for 30 minutes; fill with argon and cool to room temperature.

[0048] Liquid phase reactive siliconizing treatment. The debonded silicon carbide blank is subjected to liquid phase reactive siliconizing treatment to obtain the silicon carbide ceramic composite material. In the liquid phase siliconizing reaction, the reaction between silicon and carbon (Si+C=SiC) is a chemical reaction of volume expansion, which is generally accompanied by a volume expansion of 50% or even greater. Therefore, if the carbon content is too high, on the one hand, the volume expansion of the silicon-carbon reaction will block the pores so that the carbon inside the sample cannot fully react, forming a raw material, resulting in a decrease in the mechanical properties of the final ceramic sample; on the other hand, the sample will deform and crack due to excessive expansion. The parameters of the liquid phase reactive siliconizing treatment include: the atmosphere is an inert atmosphere (for example, an argon atmosphere) or a nitrogen atmosphere; the temperature of the liquid phase reactive siliconizing is 1450 to 1700 °C; the time of the liquid phase reactive siliconizing is 200 to 400 min.

[0049] In an optional embodiment, the parameters of the liquid phase reaction siliconization treatment include: a heating rate of 5 to 10 °C / min at 0 (or room temperature) to 1200 °C; a heating rate of 3 to 5 °C / min at 1200 to 1400 °C; heating to the maximum temperature at a heating rate of 1 to 3 °C / min, keeping at the maximum temperature for 30 to 60 min, cooling to 1200 °C, and a cooling rate of 1 to 5 °C / min; finally, filling with argon or nitrogen and cooling to room temperature. As an example, the laser 3D printed porous SiC blank after debonding is siliconized for 290 min at 1550 °C in vacuum. The siliconizing system is 0 (or room temperature) ~ 1200 ℃: heating rate 10 ℃ / min; 1200 ~ 1550 ℃: heating rate 2 ~ 5 ℃ / min; keeping at 1600 ℃ for 30 ~ 180 min; 1600 ~ 1200 ℃: cooling rate 5 ℃ / min; filling with argon gas and cooling to room temperature.

[0050] In the present invention, the density of the silicon carbide ceramic composite material obtained by testing the Archimedes drainage method is 97.0-99.9%; the bulk density is 2.5-2.8 g / cm 3The flexural strength of the obtained silicon carbide ceramic composite material was tested by a three-point bending test (Instron-1195, Instron, USA) and was 172-300 MPa, and the elastic modulus was 200-320 GPa. The fracture toughness of the obtained silicon carbide ceramic composite material was tested by a three-point bending test (Instron-1195, Instron, USA) and was 2.5-4 MPa·m 1 / 2 .

[0051] The following examples are further cited to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are only an example within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description of this article, and are not limited to the specific values ​​​​exemplified below. If there is no special explanation in the following examples and comparative examples, the fiber laser used is an ytterbium-doped fiber laser with a laser wavelength of 1.06μm. The CO used 2 The laser wavelength of the laser is 10.6 μm.

[0052] Example 1 (65 vol% SiC-5 vol% C f -30vol%PR, fiber laser printing power 60W)

[0053] (1) 65 vol% SiC, 5 vol% C f The powder with 30 vol% PR was ball-milled at a speed of 60 r / min, a ball-to-material ratio of 3:1, and a ball-milling time of 2 h. After ball-milling, SiC composite powder for laser 3D printing was obtained by sieving through a 200 μm sieve.

[0054] (2) The obtained composite powder for laser 3D printing is subjected to selective laser printing to obtain a laser 3D printed SiC blank; wherein the selective laser printing parameters include: preheating the composite powder at 60°C before printing; the laser wavelength is 1.06 μm, the spot size is 500 μm, the fiber laser printing power is 60 W, the scanning speed is 20000 mm / s, the layer thickness is 0.1 mm, and the scanning interval is 0.3 mm;

[0055] (3) Debonding the obtained laser 3D printed SiC blank under vacuum and 900°C to obtain a debonded laser 3D printed SiC blank. The debonding system is as follows: room temperature to 200°C: heating rate 3°C / min; 200 to 600°C: heating rate 1°C / min; 600 to 900°C: heating rate 2°C / min, keeping at 900°C for 30 min; filling with argon gas and cooling to room temperature;

[0056] (4) The debonded laser 3D printed SiC blank was siliconized at 1600 °C under vacuum conditions to obtain a fiber laser printed silicon carbide ceramic composite material. The siliconization process was as follows: room temperature to 1200 °C: heating rate 10 °C / min; 1200 to 1400 °C: heating rate 3 °C / min, 1400 to 1600 °C: heating rate 3 °C / min, keeping at 1600 °C for 60 min; 1600 to 1200 °C: cooling rate 5 °C / min; and cooling to room temperature by filling with argon gas.

[0057] The density of the silicon carbide ceramic composite material prepared in this embodiment 1 is 98.29%, and the bulk density is 2.743 g / cm 3 , flexural strength is 285.198MPa, elastic modulus is 291.6101GPa, fracture toughness is 3.587MPa·m 1 / 2 .

[0058] Example 2

[0059] The preparation method of Example 2 is basically the same as that of Example 1, with the only difference being: the ball-to-material ratio is 4:1, the ball milling time is 1 hour, and the fiber laser printing power is 70W.

[0060] The silicon carbide ceramic composite material prepared in Example 2 has a density of 98.48% and a bulk density of 2.751 g / cm 3 , flexural strength is 269MPa, elastic modulus is 281GPa, fracture toughness is 3.78MPa·m 1 / 2 .

[0061] Example 3

[0062] The preparation method of Example 3 is basically the same as that of Example 1, with the only difference being: the ball-to-material ratio is 2:1, the ball milling time is 4 hours, and the fiber laser printing power is 80W.

[0063] The silicon carbide ceramic composite material prepared in Example 3 has a density of 99.33% and a bulk density of 2.751 g / cm 3 , flexural strength is 253MPa, elastic modulus is 274GPa, fracture toughness is 3.53MPa·m 1 / 2 .

[0064] Example 4

[0065] The preparation method of Example 4 is basically the same as that of Example 1, with the only difference being: the ball-to-material ratio is 5:1, the ball milling time is 1 h, and the fiber laser printing power is 90 W.

[0066] The silicon carbide ceramic composite material prepared in Example 4 has a density of 99.00% and a bulk density of 2.759 g / cm 3 , flexural strength is 255MPa, elastic modulus is 291GPa, fracture toughness is 3.65MPa·m 1 / 2 .

[0067] Example 5

[0068] The preparation method of Example 5 is basically the same as that of Example 1, with the only difference being that the powder composition used is 60 vol% SiC-20 vol% graphite C-20 vol% PR, and the fiber laser printing power is 100 W.

[0069] The silicon carbide ceramic composite material prepared in Example 5 has a density of 97.94% and a bulk density of 2.754 g / cm 3 , flexural strength is 271MPa, elastic modulus is 297GPa, fracture toughness is 3.75MPa·m 1 / 2 .

[0070] Example 6

[0071] The preparation methods of Example 6 are basically the same as those of Example 5, with the only difference being that the ball-to-material ratio is 4:1 and the fiber laser printing power is 110W.

[0072] The silicon carbide ceramic composite material prepared in Example 6 has a density of 97.97% and a bulk density of 2.715 g / cm 3 , flexural strength is 255MPa, elastic modulus is 282GPa, fracture toughness is 3.47MPa·m 1 / 2 .

[0073] Example 7

[0074] The preparation method of this embodiment 7 is basically the same as that of embodiment 5, with the only difference being: the ball-to-material ratio is 2:1, the ball milling time is 4 hours, and the fiber laser printing power is 120W.

[0075] The silicon carbide ceramic composite material prepared in Example 7 has a density of 98.03% and a bulk density of 2.736 g / cm 3 , flexural strength is 283MPa, elastic modulus is 300GPa, fracture toughness is 3.83MPa·m 1 / 2 .

[0076] Example 8

[0077] The preparation method of Example 8 is basically the same as that of Example 1, except that the powder composition used is 65 vol% SiC-15 vol% C f -20vol%PR, fiber laser printing power 130W.

[0078] The silicon carbide ceramic composite material prepared in Example 8 has a density of 97.85% and a bulk density of 2.769 g / cm 3 , flexural strength is 291MPa, elastic modulus is 310GPa, fracture toughness is 3.95MPa·m 1 / 2 .

[0079] Example 9

[0080] The preparation method of this embodiment 9 is basically the same as that of embodiment 8, with the only difference being: the ball-to-material ratio is 4:1; and the fiber laser printing power is 140W.

[0081] The silicon carbide ceramic composite material prepared in Example 9 has a density of 98.01% and a bulk density of 2.730 g / cm 3 , flexural strength is 277MPa, elastic modulus is 293GPa, fracture toughness is 3.84MPa·m 1 / 2 .

[0082] Example 10

[0083] The preparation method of this Example 10 is basically the same as that of Example 8, with the only differences being: a ball-to-material ratio of 2:1; a ball milling time of 4 hours, and a fiber laser printing power of 150W.

[0084] The silicon carbide ceramic composite material obtained in Example 10 has a density of 98.29% and a bulk density of 2.746 g / cm 3 , flexural strength is 253MPa, elastic modulus is 286GPa, fracture toughness is 3.85MPa·m 1 / 2 .

[0085] Embodiment 11

[0086] The preparation method of this Example 11 is basically the same as that of Example 8, with the only difference being that the powder composition used is 70 vol% SiC-10 vol% Cf-20 vol% PR.

[0087] Example 12

[0088] The preparation method of this embodiment 12 is basically the same as that of embodiment 8, with the only difference being: the scanning speed is 15000 mm / s.

[0089] Example 13

[0090] The preparation method of this embodiment 13 is basically the same as that of embodiment 8, with the only difference being: the scanning speed is 25000 mm / s.

[0091] Embodiment 14

[0092] The preparation method of Example 14 is basically the same as that of Example 8, except that the composition of the composite powder is 60 vol% SiC-20 vol% C f -20vol%PR.

[0093] Embodiment 15

[0094] The preparation method of Example 15 is basically the same as that of Example 8, except that: 55 vol% SiC-25 vol% C f -20vol%PR.

[0095] Example 16

[0096] The preparation method of Example 16 is basically the same as that of Example 8, except that: 75 vol% SiC-5 vol% C f -20vol%PR.

[0097] Embodiment 17

[0098] The preparation method of Example 17 is basically the same as that of Example 8, except that the powder composition used is 70 vol% SiC-15 vol% C f -15vol%PR.

[0099] Embodiment 18

[0100] The preparation method of Example 18 is basically the same as that of Example 8, except that the powder composition used is 55 vol% SiC-15 vol% C f -30vol%PR.

[0101] Embodiment 19

[0102] The preparation method of this Example 19 is basically the same as that of Example 8, with the only difference being that the composite powder is preheated at 50° C. before printing.

[0103] Embodiment 20

[0104] The preparation method of Example 20 is basically the same as that of Example 8, with the only difference being that the composite powder is preheated at 70° C. before printing.

[0105] Embodiment 21

[0106] The preparation method of this Example 21 is basically the same as that of Example 8, with the only difference being that the layer thickness is 0.08 mm.

[0107] Embodiment 22

[0108] The preparation method of this Example 22 is basically the same as that of Example 8, with the only difference being that the layer thickness is 0.3 mm.

[0109] Embodiment 23

[0110] The preparation method of this embodiment 23 is basically the same as that of embodiment 8, with the only difference being that the spot size is 200 μm.

[0111] Embodiment 24

[0112] The preparation method of this embodiment 24 is basically the same as that of embodiment 8, with the only difference being that the scanning interval is 0.2 mm.

[0113] Comparative Example 1

[0114] The preparation method of this comparative example 1 is basically the same as that of Example 8, except that: 2 The laser printing power is 45W, the scanning speed is 7620mm / s, the scanning spacing is 0.18mm, and the spot diameter is 520μm.

[0115] Comparative Example 2

[0116] The preparation method of this comparative example 2 is basically the same as that of example 8, except that: 2 The laser printing power is 130W, the scanning speed is 7620mm / s, the scanning spacing is 0.3mm, and the spot diameter is 520μm.

[0117] Comparative Example 3

[0118] The preparation methods of Comparative Example 3 and Example 8 are basically the same, except that the laser power is 180 W and the scanning speed is 500 mm / s.

[0119] Comparative Example 4

[0120] The preparation methods of Comparative Example 4 and Example 8 are basically the same, with the only difference being that the scanning speed is 7620 mm / s.

[0121] Comparative Example 5

[0122] The preparation methods of Comparative Example 5 and Example 8 are basically the same, with the only difference being that the scanning speed is 10000 mm / s.

[0123] Comparative Example 6

[0124] The preparation methods of Comparative Example 6 and Example 8 are basically the same, with the only difference being that the scanning speed is 30000 mm / s.

[0125] Comparative Example 7

[0126] The preparation method of this comparative example 7 is basically the same as that of Example 1, except that the powder composition used is 80 vol% SiC-20 vol% PR, and the fiber laser printing power is 130 W.

[0127] Comparative Example 8

[0128] The preparation method of Comparative Example 8 is basically the same as that of Example 9, except that the powder composition used is 50 vol% SiC-30 vol% C f -20vol%PR.

[0129] Table 1 is a comparison of printing parameters of each embodiment and comparative example:

[0130] .

[0131] It can be seen from Table 1 that the fiber printing laser power is much higher than that of CO 2 The printing efficiency of laser can be increased by 4 to 5 times.

[0132] Table 2 is a performance comparison of each embodiment and comparative example:

[0133] .

[0134] It can be seen from Table 2 that the effect of fiber printing in preparing SiC ceramic composites is not inferior to that of CO 2 Laser printing. Combining Comparative Example 4, Comparative Example 5, Example 12, Example 13, Example 8, and Comparative Example 6, it can be seen that as the scanning speed increases, the material properties first increase and then decrease. This is because too fast a scanning speed will not allow the organic adhesive to fully soften and achieve bonding. Referring to Comparative Example 3, if the scanning rate is too low, the temperature of the laser printing point is too high, and the organic adhesive is directly carbonized to make the printing ineffective. Referring to Comparative Examples 4-5, although the scanning rate is increased, the bending strength of the resulting material is low. Referring to Comparative Example 6, if the scanning rate is too high, the bending strength of the resulting material is low. Referring to Comparative Example 8, Example 15, Example 14, Example 8, Example 11, Example 16, and Comparative Example 7, it can be seen that as the SiC powder content increases, the material properties first increase and then decrease. This is because the carbon content in the sample will decrease as the SiC content increases. When the initial SiC content is low, the carbon content is high. After siliconization, the SiC content in the sample is too high, and the newly generated SiC is easy to block the siliconization channels, resulting in high residual carbon inclusions and performance degradation; as the SiC content increases, the carbon content in the sample decreases. After siliconization, the SiC content in the sample increases but not excessively, and the material properties increase; as the SiC content continues to increase, the carbon content in the sample is very small, and the newly generated SiC is less, and the material properties decrease. Referring to Comparative Example 4 and Comparative Example 2, at the same laser power and scanning speed, using CO 2Laser printing, due to the high laser power, caused the printing molten pool, printing failure, unable to prepare high content SiC ceramic composite materials (such as Figure 3 Referring to Comparative Example 3, the laser power of the fiber laser is too high and the scanning speed is too low, resulting in printing failure, and the preparation of high-content SiC ceramic composite materials cannot be achieved (e.g. Figure 3 in (l).

[0135] Figure 1 This is the SEM image of the silicon carbide ceramic composite material prepared in Example 8. Figure 2 (a)-(j) are SEM images of silicon carbide ceramic composite materials prepared in Examples 1-7, Comparative Example 7, Comparative Example 8, and Comparative Example 1. As can be seen from the figure, the SiC ceramic composite materials prepared by fiber laser printing have uniform microscopic components and no obvious defects.

[0136] Figure 4 This is the thermogravimetric analysis of phenolic resin (PR). As can be seen from the figure, the binder (phenolic resin (PR)) has begun to soften when the preheating temperature is 82°C, that is, it is no longer possible to print at a temperature above 82°C. This is because the physical properties of phenolic resin change at a temperature above 82°C, and even have a certain viscosity, which is not conducive to the compact stacking and high-density blank molding.

Claims

1. An additive manufacturing method for silicon carbide ceramic composite materials, It is characterized in that It consists of the following steps: (1) SiC powder, a carbon source and a binder are mixed to obtain a composite powder; based on the total volume of the composite powder being 100 vol%, the volume of the SiC powder accounts for 55 to 75 vol%, the volume of the carbon source accounts for 5 to 25 vol%, and the volume of the binder accounts for 15 to 30 vol%; the carbon source is carbon fiber and / or graphite; and the binder is at least one of phenolic resin, epoxy resin, polyamide urea resin, asphalt resin and polyvinyl alcohol; (2) Using a fiber laser as a light source, the obtained composite powder is subjected to selective laser printing to obtain a silicon carbide blank; the parameters of the selective laser printing include: preheating the composite powder at 50-70° C. before printing; the fiber laser is an ytterbium-doped fiber laser, the laser wavelength is 0.8-1.5 μm, the spot size is 200-500 μm; the laser power is 60-150 W; the scanning speed is 15000-25000 mm / s; the layer thickness is 0.08-0.3 mm; and the scanning interval is 0.2-0.3 mm; (3) The silicon carbide blank is subjected to a debonding treatment and a liquid phase reactive siliconizing treatment to obtain the silicon carbide ceramic composite material.

2. The additive manufacturing method of the silicon carbide ceramic composite material according to claim 1, It is characterized in that In step (1), based on the total volume of the composite powder being 100 vol%, the volume of the SiC powder accounts for 65-75 vol%, the volume of the carbon source accounts for 5-15 vol%, and the volume of the binder accounts for 15-30 vol%.

3. The additive manufacturing method of the silicon carbide ceramic composite material according to claim 1, It is characterized in that In step (1), the particle size of the SiC powder is 5 to 80 μm; the density of the SiC powder is 3.0 to 3.3 g / cm 3 .

4. The additive manufacturing method of the silicon carbide ceramic composite material according to claim 1, It is characterized in that In step (1), the length of the carbon fiber is 30 to 200 μm; the diameter of the carbon fiber is 6 to 12 μm; the density of the carbon fiber is 1.50 to 2.50 g / cm 3 ; The particle size of the graphite is 20 to 50 μm; The density of the graphite is 1.5 to 2.5 g / cm 3 .

5. The additive manufacturing method of the silicon carbide ceramic composite material according to claim 1, It is characterized in that In step (1), the density of the binder is 0.8 to 1.5 g / cm 3 .

6. The additive manufacturing method of the silicon carbide ceramic composite material according to claim 1, It is characterized in that In step (1), the mixing method is ball milling; the parameters of the ball milling mixing include: a ball milling speed of 60 to 600 r / min, a ball milling time of 2 to 12 h, and a ball-to-material ratio of (2 to 5): 1; After ball milling and mixing, the mixture is sieved; the mesh number of the sieve is 50 to 300 meshes.

7. The additive manufacturing method of the silicon carbide ceramic composite material according to any one of claims 1 to 6, It is characterized in that In step (2), the laser wavelength is 1.06 μm.

8. The additive manufacturing method of the silicon carbide ceramic composite material according to any one of claims 1 to 6, It is characterized in that The parameters of the debonding treatment include: in a vacuum atmosphere, an inert atmosphere or a nitrogen atmosphere, first heating to 200°C at a heating rate of 1 to 3°C / min, then continuing to heat to 200 to 600°C at a heating rate of 0.25 to 2°C / min, and finally heating to 600 to 1200°C at a heating rate of 1 to 2°C / min and keeping the temperature for 30 to 120 min, and then filling with an inert atmosphere and cooling to room temperature.

9. The additive manufacturing method of the silicon carbide ceramic composite material according to any one of claims 1 to 6, It is characterized in that The parameters of the liquid phase reactive siliconization include: in an argon atmosphere or a nitrogen atmosphere, first heating to 1200°C at a heating rate of 5 to 10°C / min, then continuing to heat to 1200 to 1400°C at a heating rate of 3 to 5°C / min, finally heating to 1450 to 1700°C at a heating rate of 1 to 3°C / min and keeping warm for 30 to 60 min, then cooling to 1000 to 1300°C at a cooling rate of 1 to 5°C / min, and finally filling with an inert atmosphere and cooling to room temperature.

10. A silicon carbide ceramic composite material prepared by the additive manufacturing method according to claim 1, It is characterized in that The main components of the silicon carbide ceramic composite material include SiC, residual carbon and free silicon.

11. The silicon carbide ceramic composite material according to claim 10, It is characterized in that The open porosity of the silicon carbide ceramic composite material is 0.67 to 2.15%; The density of the silicon carbide ceramic composite material is 97.85-99.33%; The bulk density of the silicon carbide ceramic composite material is 2.715-2.769 g / cm 3 ; The flexural strength of the silicon carbide ceramic composite material is 193.087 to 291.127 MPa; The elastic modulus of the silicon carbide ceramic composite material is 228.2339 to 300.7185 GPa; The fracture toughness of the silicon carbide ceramic composite material is 2.547-3.958 MPa·m 1 / 2 .