Environmentally friendly and anti-oxidation wire and cable and processing technology

By using a combination of functionalized polyethylene and silicone rubber in wires and cables, combined with repair enhancers and modifiers, the problem of insufficient oxidation resistance and waterproofness of high-density polyethylene wires and cables is solved, and higher weather resistance is achieved. properties and mechanical properties.

CN118571546BActive Publication Date: 2024-10-11河北金桥线缆有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411065699.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-11
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

Existing high-density polyethylene wires and cables have poor oxidation resistance, poor environmental cracking resistance, and insufficient waterproof performance, making it difficult to meet environmental protection and high-performance requirements.

Method used

A combination of functionalized polyethylene and silicone rubber is used, and through the use of repair enhancers and modifiers, wires and cables with excellent corrosion resistance and UV resistance are formed, and their waterproofness and mechanical properties are improved.

Benefits of technology

Significantly improve the oxidation resistance, waterproofness and mechanical properties of wires and cables, enhance their weather resistance and waterproof performance, and meet the needs of environmental protection and high performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present application relates to the technical field of wire and cable manufacturing, and specifically discloses an environmentally friendly and antioxidant wire and cable and a processing technology, comprising the following steps: step S1, preparing a conductor; step S2, preparing an isolation layer; step S3, preparing an inner protective layer; step S4, preparing a wire and cable; a repair enhancer is added to the present application, the outer layer of the repair enhancer is a urea-formaldehyde resin structure in which urea and formaldehyde are chemically cross-linked and then modified by a water-resistant modifier, the inner core contains a functional monomer, the water-resistant modifier contains phenyl, pyridyl, pyrimidine, amide, amino and hydroxyl, and the functional monomer is prepared by chemically bonding 3,3'-dithiodipropionic acid and allyl glycidyl ether, and then chemically cross-linking with triethoxysilane; through the combined action of the above structures, the antioxidant, waterproof and mechanical properties of the wire and cable are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of wire and cable manufacturing, and more specifically, to an environmentally friendly and anti-oxidation wire and cable and a processing technology. Background Art

[0002] Wire and cable products are widely used in industries such as electricity, communications, and electrical equipment. The raw materials used for wire and cable special materials are mainly polyethylene and polyvinyl chloride, but polyvinyl chloride has poor stability to light and heat, and will produce a lot of smoke and chlorine when a fire occurs, which poses an environmental hazard. With the improvement of environmental awareness and the increasing demand for high-performance wires and cables, polyethylene has been more widely used in the processing and preparation of wires and cables.

[0003] In daily life, wires and cables generally use high-density polyethylene with good softness, ductility, electrical insulation and transparency as the inner sheath, but its oxidation resistance is poor, especially its environmental cracking resistance is not as good as low-density polyethylene, and it is easy to crack under the action of thermal oxidative aging. In the prior art, its oxidation resistance is often improved by adding antioxidants, but conventional antioxidants have a small molecular weight and cannot participate in cross-linking and curing reactions. They are easy to migrate and precipitate, resulting in poor oxidation resistance of wires and cables. In addition, the existing high-density polyethylene has poor waterproof performance and poor solvent resistance. Corrosive media such as water molecules can easily enter the interior of the high-density polyethylene material. Therefore, providing a processing technology for environmentally friendly and antioxidant wires and cables is a technical problem that needs to be solved at present. Summary of the invention

[0004] In order to solve the above problems, the present application provides an environmentally friendly and antioxidant wire and cable and a processing technology.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] An environmentally friendly and anti-oxidation wire and cable is provided with a conductor, an isolation layer, an inner sheath and a covering layer in sequence from the inside to the outside;

[0007] The processing technology of the environmentally friendly and anti-oxidation wire and cable comprises the following steps:

[0008] Step S1, preparing a conductor: selecting galvanized copper wires and tinned copper wires with diameters of 0.25-0.45 mm respectively, arranging the galvanized copper wires and the tinned copper wires at intervals, and twisting them tightly together to obtain a conductor;

[0009] Step S2, preparing an isolation layer: extruding cross-linked polyethylene to initially form a tube with a thickness of 3-5 mm matching the conductor, and further stretching it to tightly cover the conductor to form an isolation layer;

[0010] Step S3, preparing an inner protective layer: after wrapping the isolation layer with an alloy mesh material having a thickness of 1-1.5 mm, the functionalized polyethylene is directly extruded on the isolation layer wrapped with the alloy mesh material to form an inner protective layer with a compact structure;

[0011] Step S4, preparing wires and cables: finally, extruding the silicone rubber outside the inner protective layer to form a compact covering layer to obtain environmentally friendly and anti-oxidation wires and cables.

[0012] Preferably, in step S3, the functionalized polyethylene is prepared by uniformly blending, by weight, 100-120 parts of high-density polyethylene, 22-28 parts of maleic anhydride grafted polyethylene, 14-30 parts of aluminum hydroxide, 26-32 parts of a repair enhancer, 3-5 parts of a carbon black masterbatch, 2-4 parts of a processing aid and 2-3 parts of a fluoroalkyl polyether modified polysiloxane, and then extruding and molding through a twin-screw extruder.

[0013] Preferably, the extrusion process of the twin-screw extruder is: zone 1 170-180°C, zone 2 180-185°C, zone 3 185-190°C, zone 4 190-195°C, zone 5 195-200°C, die head temperature 200°C; screw speed 200rpm.

[0014] Preferably, the alloy mesh material is a silicon-germanium alloy mesh.

[0015] Preferably, the processing aid is one of calcium stearate, zinc stearate and barium stearate.

[0016] Preferably, the silicone rubber in step S4 comprises the following raw materials in parts by weight: 58-65 parts of methyl vinyl silicone rubber, 32-40 parts of thermoplastic polyurethane elastomer, 16-20 parts of trioctyl phosphate, 4-5 parts of dibutyl malonate, 1-3 parts of L-cyclohexylglycine, 2-4 parts of diethylene glycol butyl ether acetate, 0.6-0.8 parts of accelerator and 3-5 parts of vulcanizing agent.

[0017] The preparation method of the silicone rubber comprises the following steps:

[0018] Step M1, adding methyl vinyl silicone rubber raw rubber, thermoplastic polyurethane elastomer, trioctyl phosphate, dibutyl malonate, L-cyclohexylglycine and diethylene glycol butyl ether acetate into a kneader by weight, mixing at 80-100° C. for 2-3 hours, maintaining the temperature unchanged, mixing in vacuum for 3-5 hours, cooling to room temperature, and obtaining a vulcanizing agent-free mixed rubber; then, the vulcanizing agent-free mixed rubber, accelerator and vulcanizing agent are thinly passed on a double-roll mill for 3-5 times to obtain a vulcanizing agent-containing mixed rubber;

[0019] Step M2, forming the mixed rubber containing the vulcanizing agent prepared in step M1, and vulcanizing it on a flat vulcanizer at a pressure of 8-15 MPa and a temperature of 160-180° C. for 10-20 minutes to obtain a primary vulcanized silicone rubber;

[0020] Step M3, subjecting the primary vulcanized silicone rubber to secondary vulcanization at 160-240° C. for 3-7 hours to obtain silicone rubber.

[0021] Preferably, in step M1, the accelerator is accelerator TMTD.

[0022] Preferably, in step M1, the vulcanizing agent is 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane or 2,4-dichlorobenzoyl peroxide.

[0023] Preferably, in step M1, the vacuum degree of the vacuum mixing is -0.1 MPa.

[0024] Preferably, the repair enhancer is prepared by the following steps:

[0025] Step A1, uniformly mix urea, formaldehyde aqueous solution and deionized water, adjust the pH to 8-9, heat to 65-75°C, keep warm for 1-2h, cool to room temperature, and obtain urea-formaldehyde prepolymer solution, wherein the mass ratio of urea, formaldehyde aqueous solution and deionized water is 5-6:12-16:42-46;

[0026] Step A2, adding sodium dodecylbenzene sulfonate and functional monomers into deionized water, heating to 35-45° C., and continuously stirring to form an emulsion, wherein the mass ratio of sodium dodecylbenzene sulfonate, functional monomers and deionized water is 0.8-1.2:12-14:100-120;

[0027] Step A3, adding the urea-formaldehyde prepolymer solution dropwise to the emulsion prepared in step A2 while stirring, then adding ammonium chloride and a water-resistant modifier, continuing stirring for 4-8 minutes, adding n-octanol dropwise, adjusting the pH to 2.8-3.2 after the addition, heating to 58-62°C, keeping warm and stirring for 2.6-3.2 hours, filtering, washing, and drying to obtain a repair enhancer. In the above process, ammonium chloride is used as a curing agent, and an in-situ polymerization method is used to prepare a repair enhancer with a microcapsule structure, wherein the mass ratio of the urea-formaldehyde prepolymer solution, the emulsion, ammonium chloride, the water-resistant modifier and n-octanol is 20-22:110-130:0.3-0.6:1.6-2.0:0.04-0.06.

[0028] Preferably, in step A1, the mass fraction of the formaldehyde aqueous solution is 32-36%.

[0029] Preferably, the water-resistant modifier is prepared by the following steps:

[0030] Step B1, under nitrogen protection, adding p-hydroxydiphenylamine and acryloyl chloride to anhydrous ethanol, stirring evenly, then adding triethylamine, heating to reflux, stirring and reacting for 4-6 hours, after the reaction is completed, extracting, and concentrating the organic phase under reduced pressure to obtain a hydroxyl monomer, wherein the mass ratio of p-hydroxydiphenylamine, acryloyl chloride, anhydrous ethanol and triethylamine is 2.6-2.8:1.2-1.4:45-65:0.02-0.04. In the above reaction process, anhydrous ethanol is used as a solvent, triethylamine is used as an acid binding agent, and p-hydroxydiphenylamine and acryloyl chloride undergo an amidation reaction to obtain a hydroxyl monomer;

[0031] The structural formula of the hydroxyl monomer is shown below:

[0032]

[0033] Step B2, adding hydroxyl monomer, 2-mercaptonicotinic acid and benzoin dimethyl ether to anhydrous ethanol, stirring evenly, maintaining a constant speed, placing under ultraviolet irradiation for 15-25 minutes while stirring, and controlling the irradiation temperature to be 35-45° C. After the reaction is completed, removing anhydrous ethanol, and then washing and drying to obtain a pyridine compound, wherein the mass ratio of hydroxyl monomer, 2-mercaptonicotinic acid, benzoin dimethyl ether and anhydrous ethanol is 2.1-2.5:1.1-1.5:0.02-0.04:35-45;

[0034] The structural formula of the pyridine compound is shown below:

[0035]

[0036] In the above process, anhydrous ethanol is used as a solvent, benzoin dimethyl ether is used as a photoinitiator, and the unsaturated double bond on the hydroxyl monomer and the thiol group on 2-mercaptonicotinic acid undergo a click reaction to obtain a pyridine compound;

[0037] Step B3, adding a pyridyl compound and 4,6-diaminopyrimidine to anhydrous DMF, stirring evenly, adding dropwise a mixed solution a of N,N'-dicyclohexylcarbodiimide, 4-dimethylaminopyridine and anhydrous DMF while stirring, heating to 65-75°C, stirring for reaction for 2-3h, cooling to room temperature after the reaction, filtering by suction, washing and drying the filter cake to obtain a water-resistant modifier, wherein the mass ratio of the pyridyl compound, 4,6-diaminopyrimidine, anhydrous DMF and the mixed solution a is 3.6-4.0:0.8-1.2:40-50:10, and the mass ratio of N,N'-dicyclohexylcarbodiimide, 4-dimethylaminopyridine and anhydrous DMF in the mixed solution a is 1.8-2.2:1.4-1.6:15;

[0038] The structural formula of the water-resistant modifier is as follows:

[0039]

[0040] In the above reaction process, N, N'-dicyclohexylcarbodiimide is used as a dehydrating agent and 4-dimethylaminopyridine is used as an acylating agent to cause the carboxyl group of the pyridine compound and the amino group on 4,6-diaminopyrimidine to undergo an amidation reaction to obtain a water-resistant modifier.

[0041] Preferably, the peak wavelength of the irradiation in step B2 is 365nm and the intensity is 80mw / cm 2 .

[0042] Preferably, the functional monomer is prepared by the following steps:

[0043] Step C1, ultrasonically dispersing 3,3'-dithiodipropionic acid in anhydrous DMF, dripping tetrabutylammonium bromide, allyl glycidyl ether and anhydrous DMF mixed solution b, heating to 95-105°C after the dripping is completed, stirring and reacting for 2-3h, centrifuging, washing and drying to obtain an allyl monomer, wherein the mass ratio of 3,3'-dithiodipropionic acid, anhydrous DMF and mixed solution b is 4-5:45-55:14, and the mass ratio of tetrabutylammonium bromide, allyl glycidyl ether and anhydrous DMF in the mixed solution b is 0.02-0.04:2.2-2.6:12-14. In the above process, using anhydrous DMF as solvent, 3,3'-dithiodipropionic acid and allyl glycidyl ether undergo a ring-opening esterification reaction to obtain an allyl monomer;

[0044] The structural formula of allyl monomer is as follows:

[0045]

[0046] Step C2, under nitrogen protection, add allyl monomer and Custer catalyst to toluene, heat to 35-45°C, stir evenly, then add triethoxysilane, continue to heat to 65-75°C, stir and react for 18-24h, remove toluene after the reaction, and obtain a functional monomer, wherein the mass ratio of allyl monomer, Custer catalyst, toluene and triethoxysilane is 2.2-2.6:0.25-0.35:30-40:0.9-1.3;

[0047] The structural formula of the functional monomer is as follows:

[0048]

[0049] In the above process, toluene is used as a solvent, and the unsaturated double bonds on the allyl monomer and the active hydrogen on the triethoxysilane undergo a hydrosilylation reaction to obtain a functional monomer.

[0050] In summary, the present application has the following beneficial effects: in order to improve the weather resistance and waterproofness of environmentally friendly and antioxidant wires and cables, the present invention adds a repair enhancer, the outer layer of the repair enhancer is a urea-formaldehyde resin structure in which urea and formaldehyde are chemically cross-linked and then modified by a water-resistant modifier, the inner core contains functional monomers, and the water-resistant modifier contains phenyl, pyridyl, pyrimidine, amide, amino and hydroxyl groups. The presence of phenyl, pyridyl and pyrimidine groups, on the one hand, gives polyethylene excellent corrosion resistance and ultraviolet radiation resistance, and on the other hand, pyridyl and pyrimidine groups can hydrogen bond with amino groups in silicone rubber, thereby improving the compatibility of functionalized polyethylene with silicone rubber and strengthening the intermolecular binding force. Water molecules are not easy to enter the interior of the molecule through the coating, thereby improving the waterproof performance of wires and cables. The presence of amino and hydroxyl groups can hydrogen bond with amide groups in urea-formaldehyde resin, thereby further improving the waterproofness of wires and cables. The functional monomer is prepared by chemically bonding 3,3'-dithiodipropionic acid with allyl glycidyl ether, and then chemically cross-linking with triethoxysilane. Triethoxysilane contains -Si-O-Me- bonds. The presence of -Si-O-Me- bonds improves the compatibility between functionalized polyethylene and silicone rubber on the one hand, and on the other hand, it has the hydrophobicity and antioxidant properties of organic siloxane. 3,3'-dithiodipropionic acid contains disulfide bonds and flexible long alkyl chains. The self-repairing properties of functionalized polyethylene are improved through dynamic disulfide bonds and hydrogen bonds between functionalized polyethylene and urea-formaldehyde resin, and the antioxidant properties and mechanical properties of wires and cables are further improved. The presence of flexible long alkyl chains can work together with -Si-O-Me- bonds to introduce them into functionalized polyethylene, and can work together with water-resistant modifiers to improve the antioxidant properties and mechanical properties of wires and cables. DETAILED DESCRIPTION

[0051] In order to make the implementation methods of the present application easier to understand, the present application will be described in detail below in conjunction with specific examples. These examples are only for illustration and are not limited to the scope of application of the present application.

[0052] The contents of the main raw materials and their components used in the examples are as follows:

[0053] Thermoplastic polyurethane elastomer is thermoplastic polyester elastomer rubber produced by DuPont Company of the United States, with the brand name TPEETPC-ET G3548; methyl vinyl silicone rubber raw rubber is XIAMETERTM RBG-0730 rubber produced by Dow Corning, with a vinyl content of 3%, a molecular weight of 650,000, and VOC<1.2%; cross-linked polyethylene is CP350 cross-linked polyethylene plastic raw material with the product number CP355; high-density polyethylene is extrusion-grade high-density polyethylene with the brand name DGDA3485 produced by Dow of the United States; maleic anhydride grafted polyethylene is extrusion-grade maleic anhydride grafted polyethylene with the brand name E226 produced by DuPont (Comar) Company of the United States; and Castel catalyst is a platinum catalyst produced by Platinum Corporation with the CAS number 68478-92-2.

[0054] Preparation Examples 1-3 and Comparative Preparation Examples 1-2 provide methods for preparing functional monomers.

[0055] Preparation Example 1

[0056] The functional monomer is prepared by the following steps:

[0057] Step C1, ultrasonically dispersing 3,3'-dithiodipropionic acid in anhydrous DMF, controlling the ultrasonic frequency to 40kHz, the ultrasonic power to 600w, and ultrasonicating for 30min, dripping tetrabutylammonium bromide, allyl glycidyl ether and anhydrous DMF mixed solution b, and controlling the dripping to be completed within 30min. After the dripping is completed, the temperature is raised to 95°C, and the stirring reaction is controlled at a speed of 600rpm for 2h. After the reaction is completed, centrifugation is performed, and then washed with anhydrous ethanol and deionized water for 3 times in sequence, and dried at 50°C to constant weight to obtain an allyl monomer, wherein the mass ratio of 3,3'-dithiodipropionic acid, anhydrous DMF and mixed solution b is 4:45:14, and the mass ratio of tetrabutylammonium bromide, allyl glycidyl ether and anhydrous DMF in the mixed solution b is 0.02:2.2:12;

[0058] Step C2, under nitrogen protection, add allyl monomer and Custer catalyst to toluene, heat to 35°C, stir at 400 rpm for 40 min until uniform, then add triethoxysilane, continue to heat to 65°C, maintain the speed unchanged, continue stirring to react for 18 h, after the reaction is completed, remove toluene by reduced pressure distillation to obtain a functional monomer, wherein the mass ratio of allyl monomer, Custer catalyst, toluene and triethoxysilane is 2.2:0.25:30:0.9.

[0059] Preparation Example 2

[0060] The functional monomer is prepared by the following steps:

[0061] Step C1, ultrasonically dispersing 3,3'-dithiodipropionic acid in anhydrous DMF, controlling the ultrasonic frequency to 35kHz, the ultrasonic power to 550w, and ultrasonicating for 35min, dripping tetrabutylammonium bromide, allyl glycidyl ether and anhydrous DMF mixed solution b, and controlling the dripping to be completed within 30min. After the dripping is completed, the temperature is raised to 100°C, and the stirring reaction is controlled at a speed of 500rpm for 2.5h. After the reaction is completed, centrifugation is performed, and then washed with anhydrous ethanol and deionized water for 4 times in sequence, and dried at 55°C to constant weight to obtain an allyl monomer, wherein the mass ratio of 3,3'-dithiodipropionic acid, anhydrous DMF and mixed solution b is 4.5:50:14, and the mass ratio of tetrabutylammonium bromide, allyl glycidyl ether and anhydrous DMF in the mixed solution b is 0.03:2.4:13;

[0062] Step C2, under nitrogen protection, add allyl monomer and Custer catalyst to toluene, heat to 40°C, stir at 500 rpm for 30 min until uniform, add triethoxysilane, continue to heat to 70°C, maintain the speed unchanged, continue to stir and react for 21 h, after the reaction is completed, remove toluene by reduced pressure distillation to obtain a functional monomer, wherein the mass ratio of allyl monomer, Custer catalyst, toluene and triethoxysilane is 2.4:0.3:35:1.1.

[0063] Preparation Example 3

[0064] The functional monomer is prepared by the following steps:

[0065] Step C1, ultrasonically dispersing 3,3'-dithiodipropionic acid in anhydrous DMF, controlling the ultrasonic frequency to 30kHz, the ultrasonic power to 500w, and ultrasonicating for 40min, dripping tetrabutylammonium bromide, allyl glycidyl ether and anhydrous DMF mixed solution b, and controlling the dripping to be completed within 30min. After the dripping is completed, the temperature is raised to 105°C, and the speed is controlled to be 400rpm and stirred for reaction for 3h. After the reaction is completed, centrifugation is performed, and then washed with anhydrous ethanol and deionized water for 5 times in sequence, and dried at 60°C to constant weight to obtain an allyl monomer, wherein the mass ratio of 3,3'-dithiodipropionic acid, anhydrous DMF and mixed solution b is 5:55:14, and the mass ratio of tetrabutylammonium bromide, allyl glycidyl ether and anhydrous DMF in the mixed solution b is 0.04:2.6:14;

[0066] Step C2, under nitrogen protection, add allyl monomer and Custer catalyst to toluene, heat to 45°C, stir at 600 rpm for 10 min until uniform, then add triethoxysilane, continue to heat to 75°C, maintain the speed unchanged, continue stirring to react for 24 h, after the reaction is completed, remove toluene by reduced pressure distillation to obtain a functional monomer, wherein the mass ratio of allyl monomer, Custer catalyst, toluene and triethoxysilane is 2.6:0.35:40:1.3.

[0067] Comparative Preparation Example 1

[0068] The functional monomer is prepared by the following steps:

[0069] Step C1, ultrasonically dispersing malonic acid in anhydrous DMF, controlling the ultrasonic frequency to 40kHz, the ultrasonic power to 600w, ultrasonicating for 30min, dripping tetrabutylammonium bromide, allyl glycidyl ether and anhydrous DMF mixed solution b, controlling the dripping to be completed within 30min, heating to 95°C, controlling the speed to 600rpm and stirring to react for 2h, after the reaction is completed, centrifuging, and then washing with anhydrous ethanol and deionized water for 3 times in sequence, and drying at 50°C to constant weight to obtain an allyl monomer, wherein the mass ratio of malonic acid, anhydrous DMF and mixed solution b is 4:45:14, and the mass ratio of tetrabutylammonium bromide, allyl glycidyl ether and anhydrous DMF in the mixed solution b is 0.02:2.2:12;

[0070] Step C2, under nitrogen protection, add allyl monomer and Custer catalyst to toluene, heat to 35°C, stir at 400 rpm for 40 min until uniform, then add triethoxysilane, continue to heat to 65°C, maintain the speed unchanged, continue stirring to react for 18 h, after the reaction is completed, remove toluene by reduced pressure distillation to obtain a functional monomer, wherein the mass ratio of allyl monomer, Custer catalyst, toluene and triethoxysilane is 2.2:0.25:30:0.9.

[0071] Comparative Preparation Example 2

[0072] The functional monomer is prepared by the following steps:

[0073] Step C1, ultrasonically dispersing 3,3'-dithiodipropionic acid in anhydrous DMF, controlling the ultrasonic frequency to 40kHz, the ultrasonic power to 600w, and ultrasonicating for 30min, dripping tetrabutylammonium bromide, isopropyl glycidyl ether and anhydrous DMF mixed solution b, and controlling the dripping to be completed within 30min. After the dripping is completed, the temperature is raised to 95°C, and the stirring reaction is controlled at a speed of 600rpm for 2h. After the reaction is completed, centrifugation is performed, and then washed with anhydrous ethanol and deionized water for 3 times in sequence, and dried at 50°C to constant weight to obtain an allyl monomer, wherein the mass ratio of 3,3'-dithiodipropionic acid, anhydrous DMF and mixed solution b is 4:45:14, and the mass ratio of tetrabutylammonium bromide, isopropyl glycidyl ether and anhydrous DMF in the mixed solution b is 0.02:2.2:12;

[0074] Step C2, under nitrogen protection, add allyl monomer and Custer catalyst to toluene, heat to 35°C, stir at 400 rpm for 40 min until uniform, then add triethoxysilane, continue to heat to 65°C, maintain the speed unchanged, continue stirring to react for 18 h, after the reaction is completed, remove toluene by reduced pressure distillation to obtain a functional monomer, wherein the mass ratio of allyl monomer, Custer catalyst, toluene and triethoxysilane is 2.2:0.25:30:0.9.

[0075] Preparation Examples 4-6 and Comparative Preparation Example 3 provide methods for preparing water-resistant modifiers.

[0076] Preparation Example 4

[0077] The water-resistant modifier is prepared by the following steps:

[0078] Step B1, under nitrogen protection, add p-hydroxydiphenylamine and acryloyl chloride to anhydrous ethanol, control the speed to 500 rpm and stir for 35 minutes until uniform, then add triethylamine, raise the temperature to reflux, maintain the speed unchanged, stir and react for 4 hours, after the reaction is completed, extract with water and dichloromethane in a volume ratio of 1:5, and concentrate the organic phase under reduced pressure to obtain a hydroxyl monomer, wherein the mass ratio of p-hydroxydiphenylamine, acryloyl chloride, anhydrous ethanol and triethylamine is 2.6:1.2:45:0.02;

[0079] Step B2: Add hydroxyl monomer, 2-mercaptonicotinic acid and benzoin dimethyl ether to anhydrous ethanol, stir at 500 rpm for 40 min until uniform, maintain the speed unchanged, and place at a wavelength peak of 365 nm and an intensity of 80 mw / cm 2 The mixture was irradiated under ultraviolet light for 15 min, and the irradiation temperature was controlled to be 35°C. After the reaction was completed, the anhydrous ethanol was removed by rotary evaporation, and then washed with anhydrous ethanol and deionized water for 3 times, and dried at 45°C to constant weight to obtain a pyridine compound, wherein the mass ratio of hydroxyl monomer, 2-mercaptonicotinic acid, benzoin dimethyl ether and anhydrous ethanol was 2.1:1.1:0.02:35;

[0080] Step B3, add the pyridine compound and 4,6-diaminopyrimidine to anhydrous DMF, stir at a speed of 600 rpm for 20 minutes until uniform, and add a mixture of N, N'-dicyclohexylcarbodiimide, 4-dimethylaminopyridine and anhydrous DMF dropwise while stirring. After the dropwise addition, heat to 65 ° C, stir and react for 2 hours. After the reaction is completed, cool to room temperature, filter, wash the filter cake with anhydrous ethanol and deionized water for 3 times, and dry at 50 ° C to constant weight to obtain a water-resistant modifier, wherein the mass ratio of the pyridine compound, 4,6-diaminopyrimidine, anhydrous DMF and the mixture a is 3.6:0.8:40:10, and the mass ratio of N, N'-dicyclohexylcarbodiimide, 4-dimethylaminopyridine and anhydrous DMF in the mixture a is 1.8:1.4:15.

[0081] Preparation Example 5

[0082] The water-resistant modifier is prepared by the following steps:

[0083] Step B1, under nitrogen protection, add p-hydroxydiphenylamine and acryloyl chloride to anhydrous ethanol, control the speed to 550 rpm and stir for 30 minutes until uniform, then add triethylamine, raise the temperature to reflux, maintain the speed unchanged, continue stirring and react for 5 hours, after the reaction is completed, extract with water and dichloromethane in a volume ratio of 1:6, and concentrate the organic phase under reduced pressure to obtain a hydroxyl monomer, wherein the mass ratio of p-hydroxydiphenylamine, acryloyl chloride, anhydrous ethanol and triethylamine is 2.7:1.3:55:0.03;

[0084] Step B2: Add hydroxyl monomer, 2-mercaptonicotinic acid and benzoin dimethyl ether to anhydrous ethanol, stir at 550 rpm for 35 min until uniform, maintain the speed unchanged, and place at a wavelength peak of 365 nm and an intensity of 80 mw / cm 2 The mixture was irradiated under ultraviolet light for 20 minutes, and the irradiation temperature was controlled to be 40°C. After the reaction was completed, the anhydrous ethanol was removed by rotary evaporation, and then washed with anhydrous ethanol and deionized water for 4 times, and dried at 50°C to constant weight to obtain a pyridine compound, wherein the mass ratio of hydroxyl monomer, 2-mercaptonicotinic acid, benzoin dimethyl ether and anhydrous ethanol was 2.3:1.3:0.03:40;

[0085] Step B3, add the pyridine compound and 4,6-diaminopyrimidine to anhydrous DMF, stir at a speed of 650rpm for 25min until uniform, and add a mixed solution a of N,N'-dicyclohexylcarbodiimide, 4-dimethylaminopyridine and anhydrous DMF dropwise while stirring, and control the dripping to be completed within 30min. After the dripping is completed, the temperature is raised to 70°C, and the reaction is stirred for 2.5h. After the reaction is completed, it is cooled to room temperature, filtered, and the filter cake is washed with anhydrous ethanol and deionized water 4 times, and dried at 55°C to constant weight to obtain a water-resistant modifier, wherein the mass ratio of the pyridine compound, 4,6-diaminopyrimidine, anhydrous DMF and the mixed solution a is 3.8:1.0:45:10, and the mass ratio of N,N'-dicyclohexylcarbodiimide, 4-dimethylaminopyridine and anhydrous DMF in the mixed solution a is 2.0:1.5:15.

[0086] Preparation Example 6

[0087] The water-resistant modifier is prepared by the following steps:

[0088] Step B1, under nitrogen protection, add p-hydroxydiphenylamine and acryloyl chloride to anhydrous ethanol, control the speed to 600 rpm and stir for 25 minutes until uniform, then add triethylamine, raise the temperature to reflux, continue stirring and react for 6 hours, after the reaction is completed, extract with water and dichloromethane in a volume ratio of 1:7, and concentrate the organic phase under reduced pressure to obtain a hydroxyl monomer, wherein the mass ratio of p-hydroxydiphenylamine, acryloyl chloride, anhydrous ethanol and triethylamine is 2.8:1.4:65:0.04;

[0089] Step B2: Add hydroxyl monomer, 2-mercaptonicotinic acid and benzoin dimethyl ether to anhydrous ethanol, stir at 600 rpm for 30 min until uniform, maintain the speed unchanged, and place at a wavelength peak of 365 nm and an intensity of 80 mw / cm 2 The mixture was irradiated under ultraviolet light for 25 minutes, and the irradiation temperature was controlled to be 45°C. After the reaction was completed, the anhydrous ethanol was removed by rotary evaporation, and then washed with anhydrous ethanol and deionized water for 5 times, and dried at 55°C to constant weight to obtain a pyridyl compound, wherein the mass ratio of hydroxyl monomer, 2-mercaptonicotinic acid, benzoin dimethyl ether and anhydrous ethanol was 2.5:1.5:0.04:45;

[0090] Step B3, add the pyridine compound and 4,6-diaminopyrimidine to anhydrous DMF, stir at a speed of 700 rpm for 20 minutes until uniform, and add a mixed solution a of N, N'-dicyclohexylcarbodiimide, 4-dimethylaminopyridine and anhydrous DMF dropwise while stirring, and control the dripping within 30 minutes. After the dripping is completed, the temperature is raised to 75°C, and the reaction is stirred for 3 hours. After the reaction is completed, it is cooled to room temperature and filtered. The filter cake is washed with anhydrous ethanol and deionized water for 5 times, and dried at 60°C to constant weight to obtain a water-resistant modifier, wherein the mass ratio of the pyridine compound, 4,6-diaminopyrimidine, anhydrous DMF and the mixed solution a is 4.0:1.2:50:10, and the mass ratio of N, N'-dicyclohexylcarbodiimide, 4-dimethylaminopyridine and anhydrous DMF in the mixed solution a is 2.2:1.6:15.

[0091] Comparative Preparation Example 3

[0092] The water-resistant modifier is prepared by the following steps:

[0093] Step B1, under nitrogen protection, add p-hydroxydiphenylamine and acryloyl chloride to anhydrous ethanol, control the speed to 500 rpm and stir for 35 minutes until uniform, then add triethylamine, raise the temperature to reflux, maintain the speed unchanged, stir and react for 4 hours, after the reaction is completed, extract with water and dichloromethane in a volume ratio of 1:5, and concentrate the organic phase under reduced pressure to obtain a hydroxyl monomer, wherein the mass ratio of p-hydroxydiphenylamine, acryloyl chloride, anhydrous ethanol and triethylamine is 2.6:1.2:45:0.02;

[0094] Step B2: Add hydroxyl monomer, nicotinic acid and benzoin dimethyl ether to anhydrous ethanol, stir at 500 rpm for 40 min until uniform, maintain the speed unchanged, and place at a wavelength peak of 365 nm and an intensity of 80 mw / cm 2 The mixture was irradiated under ultraviolet light for 15 min, and the irradiation temperature was controlled at 35°C. After the reaction was completed, the anhydrous ethanol was removed by rotary evaporation, and then washed with anhydrous ethanol and deionized water for 3 times, and dried at 45°C to constant weight to obtain a pyridine compound, wherein the mass ratio of hydroxyl monomer, nicotinic acid, benzoin dimethyl ether and anhydrous ethanol was 2.1:1.1:0.02:35;

[0095] Step B3, add the pyridine compound and 4,6-diaminopyrimidine to anhydrous DMF, stir at a speed of 600 rpm for 20 minutes until uniform, and add a mixture of N, N'-dicyclohexylcarbodiimide, 4-dimethylaminopyridine and anhydrous DMF dropwise while stirring. After the dropwise addition, heat to 65 ° C, stir and react for 2 hours. After the reaction is completed, cool to room temperature, filter, wash the filter cake with anhydrous ethanol and deionized water for 3 times, and dry at 50 ° C to constant weight to obtain a water-resistant modifier, wherein the mass ratio of the pyridine compound, 4,6-diaminopyrimidine, anhydrous DMF and the mixture a is 3.6:0.8:40:10, and the mass ratio of N, N'-dicyclohexylcarbodiimide, 4-dimethylaminopyridine and anhydrous DMF in the mixture a is 1.8:1.4:15.

[0096] Preparation Examples 7-9 and Comparative Preparation Examples 4-6 provide methods for preparing the repair enhancer.

[0097] Preparation Example 7

[0098] The repair enhancer is prepared by the following steps:

[0099] Step A1, stirring urea, a 32% formaldehyde aqueous solution and deionized water at a speed of 500 rpm for 20 minutes until uniform, adjusting the pH to 8 with a 1M sodium hydroxide solution, heating to 65°C, keeping the temperature for reaction for 1 hour, cooling to room temperature, and obtaining a urea-formaldehyde prepolymer solution, wherein the mass ratio of urea, a 32% formaldehyde aqueous solution and deionized water is 5:12:42;

[0100] Step A2, adding sodium dodecylbenzene sulfonate and the functional monomer prepared in Preparation Example 1 into deionized water, heating to 35° C., and stirring for 20 min at a controlled speed of 1000 rpm to obtain an emulsion, wherein the mass ratio of sodium dodecylbenzene sulfonate, the functional monomer prepared in Preparation Example 1, and deionized water is 0.8:12:100;

[0101] Step A3, at a speed of 500 rpm, add the urea-formaldehyde prepolymer solution dropwise to the emulsion prepared in step A2 while stirring, then add ammonium chloride and the water-resistant modifier prepared in Preparation Example 4, continue stirring for 4 minutes, add n-octanol dropwise, after the dropwise addition, adjust the pH to 2.8, heat to 58°C, keep stirring for 2.6 hours, filter, wash with anhydrous ethanol and deionized water for 3 times, and dry at 50°C to constant weight to obtain a repair enhancer, wherein the mass ratio of urea-formaldehyde prepolymer solution, emulsion, ammonium chloride, water-resistant modifier prepared in Preparation Example 4 and n-octanol is 20:110:0.3:1.6:0.04.

[0102] Preparation Example 8

[0103] The repair enhancer is prepared by the following steps:

[0104] Step A1, stirring urea, a 34% formaldehyde aqueous solution and deionized water at a speed of 550 rpm for 15 min until uniform, adjusting the pH to 8.5 with a 1M sodium hydroxide solution, heating to 70°C, keeping the temperature for reaction for 1.5 h, cooling to room temperature, and obtaining a urea-formaldehyde prepolymer solution, wherein the mass ratio of urea, a 34% formaldehyde aqueous solution and deionized water is 5.5:14:44;

[0105] Step A2, adding sodium dodecylbenzene sulfonate and the functional monomer prepared in Preparation Example 2 to deionized water, heating to 40° C., stirring for 15 min at a controlled speed of 1100 rpm to obtain an emulsion, wherein the mass ratio of sodium dodecylbenzene sulfonate, the functional monomer prepared in Preparation Example 2 and deionized water is 1.0:11:110;

[0106] Step A3, at a rotation speed of 550rpm, add the urea-formaldehyde prepolymer solution dropwise to the emulsion prepared in step A2 while stirring, then add ammonium chloride and the water-resistant modifier prepared in Preparation Example 5, continue stirring for 6min, add n-octanol dropwise, after the dropwise addition, adjust the pH to 3.0, heat to 60°C, keep stirring for 3.0h, filter, wash with anhydrous ethanol and deionized water 4 times, and dry at 55°C to constant weight to obtain a repair enhancer, wherein the mass ratio of urea-formaldehyde prepolymer solution, emulsion, ammonium chloride, water-resistant modifier prepared in Preparation Example 5 and n-octanol is 21:120:0.45:1.8:0.05.

[0107] Preparation Example 9

[0108] The repair enhancer is prepared by the following steps:

[0109] Step A1, stirring urea, a 36% formaldehyde aqueous solution and deionized water at a speed of 600 rpm for 10 min until uniform, adjusting the pH to 9 with a 1M sodium hydroxide solution, heating to 75°C, keeping the temperature for reaction for 2 h, cooling to room temperature, and obtaining a urea-formaldehyde prepolymer solution, wherein the mass ratio of urea, a 36% formaldehyde aqueous solution and deionized water is 6:16:46;

[0110] Step A2, adding sodium dodecylbenzene sulfonate and the functional monomer prepared in Preparation Example 3 into deionized water, heating to 45° C., and stirring for 10 min at a controlled speed of 1200 rpm to obtain an emulsion, wherein the mass ratio of sodium dodecylbenzene sulfonate, the functional monomer prepared in Preparation Example 3, and deionized water is 1.2:14:120;

[0111] Step A3, at a speed of 600 rpm, add the urea-formaldehyde prepolymer solution dropwise to the emulsion prepared in step A2 while stirring, then add ammonium chloride and the water-resistant modifier prepared in Preparation Example 6, continue stirring for 8 minutes, add n-octanol dropwise, after the dropwise addition, adjust the pH to 3.2, raise the temperature to 62°C, keep stirring for 3.2 hours, filter, and then wash with anhydrous ethanol and deionized water 5 times, and dry at 60°C to constant weight to obtain a repair enhancer, wherein the mass ratio of urea-formaldehyde prepolymer solution, emulsion, ammonium chloride, water-resistant modifier prepared in Preparation Example 6 and n-octanol is 22:130:0.6:2.0:0.06.

[0112] Comparative Preparation Example 4

[0113] The repair enhancer is prepared by the following steps:

[0114] Step A1, stirring urea, a 32% formaldehyde aqueous solution and deionized water at a speed of 500 rpm for 20 minutes until uniform, adjusting the pH to 8 with a 1M sodium hydroxide solution, heating to 65°C, keeping the temperature for reaction for 1 hour, cooling to room temperature, and obtaining a urea-formaldehyde prepolymer solution, wherein the mass ratio of urea, a 32% formaldehyde aqueous solution and deionized water is 5:12:42;

[0115] Step A2, adding sodium dodecylbenzene sulfonate and the functional monomer prepared in Comparative Preparation Example 1 into deionized water, heating to 35° C., stirring for 20 min at a controlled speed of 1000 rpm to obtain an emulsion, wherein the mass ratio of sodium dodecylbenzene sulfonate, the functional monomer prepared in Comparative Preparation Example 1 and deionized water is 0.8:12:100;

[0116] Step A3, at a speed of 500 rpm, add the urea-formaldehyde prepolymer solution dropwise to the emulsion prepared in step A2 while stirring, then add ammonium chloride and the water-resistant modifier prepared in Preparation Example 4, continue stirring for 4 minutes, add n-octanol dropwise, after the dropwise addition, adjust the pH to 2.8, heat to 58°C, keep stirring for 2.6 hours, filter, wash with anhydrous ethanol and deionized water for 3 times, and dry at 50°C to constant weight to obtain a repair enhancer, wherein the mass ratio of urea-formaldehyde prepolymer solution, emulsion, ammonium chloride, water-resistant modifier prepared in Preparation Example 4 and n-octanol is 20:110:0.3:1.6:0.04.

[0117] Comparative Preparation Example 5

[0118] The repair enhancer is prepared by the following steps:

[0119] Step A1, stirring urea, a 32% formaldehyde aqueous solution and deionized water at a speed of 500 rpm for 20 minutes until uniform, adjusting the pH to 8 with a 1M sodium hydroxide solution, heating to 65°C, keeping the temperature for reaction for 1 hour, cooling to room temperature, and obtaining a urea-formaldehyde prepolymer solution, wherein the mass ratio of urea, a 32% formaldehyde aqueous solution and deionized water is 5:12:42;

[0120] Step A2, adding sodium dodecylbenzene sulfonate and the functional monomer prepared in Comparative Preparation Example 2 to deionized water, heating to 35° C., and stirring for 20 min at a controlled speed of 1000 rpm to obtain an emulsion, wherein the mass ratio of sodium dodecylbenzene sulfonate, the functional monomer prepared in Comparative Preparation Example 2, and deionized water is 0.8:12:100;

[0121] Step A3, at a speed of 500 rpm, add the urea-formaldehyde prepolymer solution dropwise to the emulsion prepared in step A2 while stirring, then add ammonium chloride and the water-resistant modifier prepared in Preparation Example 4, continue stirring for 4 minutes, add n-octanol dropwise, after the dropwise addition, adjust the pH to 2.8, heat to 58°C, keep stirring for 2.6 hours, filter, wash with anhydrous ethanol and deionized water for 3 times, and dry at 50°C to constant weight to obtain a repair enhancer, wherein the mass ratio of urea-formaldehyde prepolymer solution, emulsion, ammonium chloride, water-resistant modifier prepared in Preparation Example 4 and n-octanol is 20:110:0.3:1.6:0.04.

[0122] Comparative Preparation Example 6

[0123] The repair enhancer is prepared by the following steps:

[0124] Step A1, stirring urea, a 32% formaldehyde aqueous solution and deionized water at a speed of 500 rpm for 20 minutes until uniform, adjusting the pH to 8 with a 1M sodium hydroxide solution, heating to 65°C, keeping the temperature for reaction for 1 hour, cooling to room temperature, and obtaining a urea-formaldehyde prepolymer solution, wherein the mass ratio of urea, a 32% formaldehyde aqueous solution and deionized water is 5:12:42;

[0125] Step A2, adding sodium dodecylbenzene sulfonate and the functional monomer prepared in Preparation Example 1 into deionized water, heating to 35° C., and stirring for 20 min at a controlled speed of 1000 rpm to obtain an emulsion, wherein the mass ratio of sodium dodecylbenzene sulfonate, the functional monomer prepared in Preparation Example 1, and deionized water is 0.8:12:100;

[0126] Step A3, at a speed of 500 rpm, add the urea-formaldehyde prepolymer solution dropwise to the emulsion prepared in step A2 while stirring, then add ammonium chloride and the water-resistant modifier prepared in comparative preparation example 3, continue stirring for 4 minutes, add n-octanol dropwise, after the dropwise addition, adjust the pH to 2.8, raise the temperature to 58°C, keep stirring for 2.6 hours, filter, and then wash with anhydrous ethanol and deionized water for 3 times, and dry at 50°C to constant weight to obtain a repair enhancer, wherein the mass ratio of urea-formaldehyde prepolymer solution, emulsion, ammonium chloride, water-resistant modifier prepared in comparative preparation example 3 and n-octanol is 20:110:0.3:1.6:0.04.

[0127] Examples 1-3 and Comparative Examples 1-3 provide environmentally friendly and antioxidant wires and cables and their processing technology.

[0128] Example 1

[0129] This embodiment provides an environmentally friendly and anti-oxidation wire and cable, which is provided with a conductor, an isolation layer, an inner sheath and a covering layer in sequence from the inside to the outside;

[0130] The processing technology of the environmentally friendly and anti-oxidation wire and cable comprises the following steps:

[0131] Step S1, preparing a conductor: selecting 3 galvanized copper wires and 3 tinned copper wires with a diameter of 0.25 mm respectively, arranging the galvanized copper wires and the tinned copper wires in sequence at intervals, and twisting them tightly together to obtain a conductor;

[0132] Step S2, preparing an isolation layer: extruding cross-linked polyethylene to initially form a tube with a thickness of 3 mm matching the conductor, and further stretching it to tightly cover the conductor to form an isolation layer;

[0133] Step S3, preparing an inner protective layer: after wrapping the isolation layer with a silicon-germanium alloy mesh with a thickness of 1 mm, the functionalized polyethylene is directly extruded on the isolation layer wrapped by the silicon-germanium alloy mesh to form an inner protective layer with a compact structure;

[0134] Step S4, preparing wires and cables: finally, extruding the silicone rubber outside the inner sheath to form a compact covering layer, thereby obtaining environmentally friendly and anti-oxidation wires and cables;

[0135] The functionalized polyethylene is prepared by uniformly blending 100 parts of high-density polyethylene, 22 parts of maleic anhydride grafted polyethylene, 14 parts of aluminum hydroxide, 26 parts of the repair enhancer prepared in Preparation Example 7, 3 parts of carbon black masterbatch, 2 parts of calcium stearate and 2 parts of fluoroalkyl polyether modified polysiloxane, and then extruding and molding through a twin-screw extruder, wherein the extrusion process of the twin-screw extruder is: zone 1 170°C, zone 2 180°C, zone 3 185°C, zone 4 190°C, zone 5 195°C, die head temperature 200°C; screw speed 200rpm;

[0136] The silicone rubber comprises the following raw materials in parts by weight: 58 parts of methyl vinyl silicone rubber, 32 parts of thermoplastic polyurethane elastomer, 16 parts of trioctyl phosphate, 4 parts of dibutyl malonate, 1 part of L-cyclohexylglycine, 2 parts of diethylene glycol butyl ether acetate, 0.6 parts of accelerator TMTD and 3 parts of 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane;

[0137] The preparation method of the silicone rubber comprises the following steps:

[0138] Step M1, adding methyl vinyl silicone rubber raw rubber, thermoplastic polyurethane elastomer, trioctyl phosphate, dibutyl malonate, L-cyclohexylglycine and diethylene glycol butyl ether acetate into a kneader by weight, mixing at 80° C. for 2 hours, maintaining the temperature unchanged, continuing to mix at a vacuum degree of -0.1 MPa for another 3 hours, cooling to room temperature, and obtaining a vulcanizing agent-free mixed rubber; then, the vulcanizing agent-free mixed rubber, accelerator TMTD and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane are thinly passed on a double-roll mill for 3 times to obtain a vulcanizing agent-containing mixed rubber;

[0139] Step M2, forming the mixed rubber containing the vulcanizing agent prepared in step M1, and vulcanizing it on a flat vulcanizer at a pressure of 8 MPa and a temperature of 160° C. for 10 minutes to obtain a primary vulcanized silicone rubber;

[0140] Step M3, subjecting the primary vulcanized silicone rubber to secondary vulcanization at 160° C. for 3 h to obtain silicone rubber.

[0141] Example 2

[0142] This embodiment provides an environmentally friendly and anti-oxidation wire and cable, which is provided with a conductor, an isolation layer, an inner sheath and a covering layer in sequence from the inside to the outside;

[0143] The processing technology of the environmentally friendly and anti-oxidation wire and cable comprises the following steps:

[0144] Step S1, preparing a conductor: selecting 4 galvanized copper wires and 4 tinned copper wires with a diameter of 0.35 mm, arranging the galvanized copper wires and the tinned copper wires in sequence, and twisting them tightly to obtain a conductor;

[0145] Step S2, preparing an isolation layer: extruding cross-linked polyethylene to initially form a tube with a thickness of 4 mm matching the conductor, and further stretching it to tightly cover the conductor to form an isolation layer;

[0146] Step S3, preparing an inner protective layer: after wrapping the isolation layer with a silicon-germanium alloy mesh with a thickness of 1.3 mm, the functionalized polyethylene is directly extruded on the isolation layer wrapped by the silicon-germanium alloy mesh to form an inner protective layer with a compact structure;

[0147] Step S4, preparing wires and cables: finally, extruding the silicone rubber outside the inner sheath to form a compact covering layer, thereby obtaining environmentally friendly and anti-oxidation wires and cables;

[0148] The functionalized polyethylene is prepared by uniformly blending 110 parts of high-density polyethylene, 25 parts of maleic anhydride grafted polyethylene, 22 parts of aluminum hydroxide, 29 parts of the repair enhancer prepared in Preparation Example 8, 4 parts of carbon black masterbatch, 3 parts of zinc stearate and 2.5 parts of fluoroalkyl polyether modified polysiloxane, and then extruding and molding through a twin-screw extruder;

[0149] The extrusion process of the twin-screw extruder is as follows: zone 1 175°C, zone 2 182°C, zone 3 187°C, zone 4 192°C, zone 5 197°C, die head temperature 200°C; screw speed 200rpm;

[0150] The silicone rubber comprises the following raw materials in parts by weight: 61.5 parts of methyl vinyl silicone rubber, 36 parts of thermoplastic polyurethane elastomer, 18 parts of trioctyl phosphate, 4.5 parts of dibutyl malonate, 2 parts of L-cyclohexylglycine, 3 parts of diethylene glycol butyl ether acetate, 0.8 parts of accelerator TMTD and 4 parts of 2,4-dichlorobenzoyl peroxide;

[0151] The preparation method of the silicone rubber comprises the following steps:

[0152] Step M1, adding methyl vinyl silicone rubber, thermoplastic polyurethane elastomer, trioctyl phosphate, dibutyl malonate, L-cyclohexylglycine and diethylene glycol butyl ether acetate into a kneader by weight, mixing at 90° C. for 2.5 hours, maintaining the temperature unchanged, continuing to mix at a vacuum degree of -0.1 MPa for another 4 hours, cooling to room temperature, and obtaining a vulcanizer-free mixed rubber; then, the vulcanizer-free mixed rubber, accelerator TMTD and 2,4-dichlorobenzoyl peroxide are thinly passed on a double-roll mill for 4 times to obtain a vulcanizer-containing mixed rubber;

[0153] Step M2, forming the mixed rubber containing the vulcanizing agent prepared in step M1, and vulcanizing it on a flat vulcanizer at a pressure of 12 MPa and a temperature of 170° C. for 15 minutes to obtain a primary vulcanized silicone rubber;

[0154] Step M3, subjecting the primary vulcanized silicone rubber to secondary vulcanization at 200° C. for 5 h to obtain silicone rubber.

[0155] Example 3

[0156] This embodiment provides an environmentally friendly and anti-oxidation wire and cable, which is provided with a conductor, an isolation layer, an inner sheath and a covering layer in sequence from the inside to the outside;

[0157] The processing technology of the environmentally friendly and anti-oxidation wire and cable comprises the following steps:

[0158] Step S1, preparing a conductor: selecting 5 galvanized copper wires and 5 tinned copper wires with a diameter of 0.45 mm, respectively, arranging the galvanized copper wires and the tinned copper wires in sequence at intervals, and twisting them tightly together to obtain a conductor;

[0159] Step S2, preparing an isolation layer: extruding cross-linked polyethylene to initially form a tube with a thickness of 5 mm matching the conductor, and further stretching it to tightly cover the conductor to form an isolation layer;

[0160] Step S3, preparing an inner protective layer: after wrapping the isolation layer with a silicon-germanium alloy mesh with a thickness of 1.5 mm, the functionalized polyethylene is directly extruded on the isolation layer wrapped by the silicon-germanium alloy mesh to form an inner protective layer with a compact structure;

[0161] Step S4, preparing wires and cables: finally, extruding the silicone rubber outside the inner protective layer to form a compact covering layer to obtain environmentally friendly and anti-oxidation wires and cables.

[0162] The functionalized polyethylene is prepared by uniformly blending 120 parts of high-density polyethylene, 28 parts of maleic anhydride grafted polyethylene, 30 parts of aluminum hydroxide, 32 parts of the repair enhancer prepared in Preparation Example 9, 5 parts of carbon black masterbatch, 4 parts of barium stearate and 3 parts of fluoroalkyl polyether modified polysiloxane, and then extruding and molding through a twin-screw extruder.

[0163] The extrusion process of the twin-screw extruder is as follows: zone 1 180°C, zone 2 185°C, zone 3 190°C, zone 4 195°C, zone 5 200°C, die head temperature 200°C; screw speed 200rpm;

[0164] The silicone rubber comprises the following raw materials in parts by weight: 65 parts of methyl vinyl silicone rubber, 40 parts of thermoplastic polyurethane elastomer, 20 parts of trioctyl phosphate, 5 parts of dibutyl malonate, 3 parts of L-cyclohexylglycine, 4 parts of diethylene glycol butyl ether acetate, 0.8 parts of accelerator TMTD and 5 parts of 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane;

[0165] The preparation method of the silicone rubber comprises the following steps:

[0166] Step M1, adding methyl vinyl silicone rubber raw rubber, thermoplastic polyurethane elastomer, trioctyl phosphate, dibutyl malonate, L-cyclohexylglycine and diethylene glycol butyl ether acetate into a kneader by weight, mixing at 100° C. for 3 hours, maintaining the temperature unchanged, continuing to mix at a vacuum degree of -0.1 MPa for another 5 hours, cooling to room temperature, and obtaining a vulcanizing agent-free mixed rubber; then, the vulcanizing agent-free mixed rubber, accelerator TMTD and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane are thinly passed on a double-roll mill for 5 times to obtain a vulcanizing agent-containing mixed rubber;

[0167] Step M2, forming the mixed rubber containing the vulcanizing agent prepared in step M1, and vulcanizing it on a flat vulcanizer at a pressure of 15 MPa and a temperature of 180° C. for 20 minutes to obtain a primary vulcanized silicone rubber;

[0168] Step M3, subjecting the primary vulcanized silicone rubber to secondary vulcanization at 240° C. for 7 h to obtain silicone rubber.

[0169] Comparative Example 1

[0170] This comparative example provides an environmentally friendly and anti-oxidation wire and cable, which is provided with a conductor, an isolation layer, an inner sheath and a covering layer in sequence from the inside to the outside;

[0171] The processing technology of the environmentally friendly and anti-oxidation wire and cable comprises the following steps:

[0172] Step S1, preparing a conductor: selecting 3 galvanized copper wires and 3 tinned copper wires with a diameter of 0.25 mm respectively, arranging the galvanized copper wires and the tinned copper wires in sequence at intervals, and twisting them tightly together to obtain a conductor;

[0173] Step S2, preparing an isolation layer: extruding cross-linked polyethylene to initially form a tube with a thickness of 3 mm matching the conductor, and further stretching it to tightly cover the conductor to form an isolation layer;

[0174] Step S3, preparing an inner protective layer: after wrapping the isolation layer with a silicon-germanium alloy mesh with a thickness of 1 mm, the functionalized polyethylene is directly extruded on the isolation layer wrapped by the silicon-germanium alloy mesh to form an inner protective layer with a compact structure;

[0175] Step S4, preparing wires and cables: finally, extruding the silicone rubber outside the inner sheath to form a compact covering layer, thereby obtaining environmentally friendly and anti-oxidation wires and cables;

[0176] The functionalized polyethylene is prepared by uniformly blending 100 parts of high-density polyethylene, 22 parts of maleic anhydride grafted polyethylene, 14 parts of aluminum hydroxide, 26 parts of the repair enhancer prepared in Comparative Preparation Example 4, 3 parts of carbon black masterbatch, 2 parts of calcium stearate and 2 parts of fluoroalkyl polyether modified polysiloxane, and then extruding and molding through a twin-screw extruder, wherein the extrusion process of the twin-screw extruder is: zone 1 170°C, zone 2 180°C, zone 3 185°C, zone 4 190°C, zone 5 195°C, die head temperature 200°C; screw speed 200rpm;

[0177] The silicone rubber comprises the following raw materials in parts by weight: 58 parts of methyl vinyl silicone rubber, 32 parts of thermoplastic polyurethane elastomer, 16 parts of trioctyl phosphate, 4 parts of dibutyl malonate, 1 part of L-cyclohexylglycine, 2 parts of diethylene glycol butyl ether acetate, 0.6 parts of accelerator TMTD and 3 parts of 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane;

[0178] The preparation method of the silicone rubber comprises the following steps:

[0179] Step M1, adding methyl vinyl silicone rubber raw rubber, thermoplastic polyurethane elastomer, trioctyl phosphate, dibutyl malonate, L-cyclohexylglycine and diethylene glycol butyl ether acetate into a kneader by weight, mixing at 80° C. for 2 hours, maintaining the temperature unchanged, continuing to mix at a vacuum degree of -0.1 MPa for another 3 hours, cooling to room temperature, and obtaining a vulcanizing agent-free mixed rubber; then, the vulcanizing agent-free mixed rubber, accelerator TMTD and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane are thinly passed on a double-roll mill for 3 times to obtain a vulcanizing agent-containing mixed rubber;

[0180] Step M2, forming the mixed rubber containing the vulcanizing agent prepared in step M1, and vulcanizing it on a flat vulcanizer at a pressure of 8 MPa and a temperature of 160° C. for 10 minutes to obtain a primary vulcanized silicone rubber;

[0181] Step M3, subjecting the primary vulcanized silicone rubber to secondary vulcanization at 160° C. for 3 h to obtain silicone rubber.

[0182] Comparative Example 2

[0183] This comparative example provides an environmentally friendly and anti-oxidation wire and cable, which is provided with a conductor, an isolation layer, an inner sheath and a covering layer in sequence from the inside to the outside;

[0184] The processing technology of the environmentally friendly and anti-oxidation wire and cable comprises the following steps:

[0185] Step S1, preparing a conductor: selecting 3 galvanized copper wires and 3 tinned copper wires with a diameter of 0.25 mm respectively, arranging the galvanized copper wires and the tinned copper wires in sequence at intervals, and twisting them tightly together to obtain a conductor;

[0186] Step S2, preparing an isolation layer: extruding cross-linked polyethylene to initially form a tube with a thickness of 3 mm matching the conductor, and further stretching it to tightly cover the conductor to form an isolation layer;

[0187] Step S3, preparing an inner protective layer: after wrapping the isolation layer with a silicon-germanium alloy mesh with a thickness of 1 mm, the functionalized polyethylene is directly extruded on the isolation layer wrapped by the silicon-germanium alloy mesh to form an inner protective layer with a compact structure;

[0188] Step S4, preparing wires and cables: finally, extruding the silicone rubber outside the inner sheath to form a compact covering layer, thereby obtaining environmentally friendly and anti-oxidation wires and cables;

[0189] The functionalized polyethylene is prepared by uniformly blending 100 parts of high-density polyethylene, 22 parts of maleic anhydride grafted polyethylene, 14 parts of aluminum hydroxide, 26 parts of the repair enhancer prepared in Comparative Preparation Example 5, 3 parts of carbon black masterbatch, 2 parts of calcium stearate and 2 parts of fluoroalkyl polyether modified polysiloxane, and then extruding and molding through a twin-screw extruder, wherein the extrusion process of the twin-screw extruder is: zone 1 170°C, zone 2 180°C, zone 3 185°C, zone 4 190°C, zone 5 195°C, die head temperature 200°C; screw speed 200rpm;

[0190] The silicone rubber comprises the following raw materials in parts by weight: 58 parts of methyl vinyl silicone rubber, 32 parts of thermoplastic polyurethane elastomer, 16 parts of trioctyl phosphate, 4 parts of dibutyl malonate, 1 part of L-cyclohexylglycine, 2 parts of diethylene glycol butyl ether acetate, 0.6 parts of accelerator TMTD and 3 parts of 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane;

[0191] The preparation method of the silicone rubber comprises the following steps:

[0192] Step M1, adding methyl vinyl silicone rubber raw rubber, thermoplastic polyurethane elastomer, trioctyl phosphate, dibutyl malonate, L-cyclohexylglycine and diethylene glycol butyl ether acetate into a kneader by weight, mixing at 80° C. for 2 hours, maintaining the temperature unchanged, continuing to mix at a vacuum degree of -0.1 MPa for another 3 hours, cooling to room temperature, and obtaining a vulcanizing agent-free mixed rubber; then, the vulcanizing agent-free mixed rubber, accelerator TMTD and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane are thinly passed on a double-roll mill for 3 times to obtain a vulcanizing agent-containing mixed rubber;

[0193] Step M2, forming the mixed rubber containing the vulcanizing agent prepared in step M1, and vulcanizing it on a flat vulcanizer at a pressure of 8 MPa and a temperature of 160° C. for 10 minutes to obtain a primary vulcanized silicone rubber;

[0194] Step M3, subjecting the primary vulcanized silicone rubber to secondary vulcanization at 160° C. for 3 h to obtain silicone rubber.

[0195] Comparative Example 3

[0196] This comparative example provides an environmentally friendly and anti-oxidation wire and cable, which is provided with a conductor, an isolation layer, an inner sheath and a covering layer in sequence from the inside to the outside;

[0197] The processing technology of the environmentally friendly and anti-oxidation wire and cable comprises the following steps:

[0198] Step S1, preparing a conductor: selecting 3 galvanized copper wires and 3 tinned copper wires with a diameter of 0.25 mm respectively, arranging the galvanized copper wires and the tinned copper wires in sequence at intervals, and twisting them tightly together to obtain a conductor;

[0199] Step S2, preparing an isolation layer: extruding cross-linked polyethylene to initially form a tube with a thickness of 3 mm matching the conductor, and further stretching it to tightly cover the conductor to form an isolation layer;

[0200] Step S3, preparing an inner protective layer: after wrapping the isolation layer with a silicon-germanium alloy mesh with a thickness of 1 mm, the functionalized polyethylene is directly extruded on the isolation layer wrapped by the silicon-germanium alloy mesh to form an inner protective layer with a compact structure;

[0201] Step S4, preparing wires and cables: finally, extruding the silicone rubber outside the inner sheath to form a compact covering layer, thereby obtaining environmentally friendly and anti-oxidation wires and cables;

[0202] The functionalized polyethylene is prepared by uniformly blending 100 parts of high-density polyethylene, 22 parts of maleic anhydride grafted polyethylene, 14 parts of aluminum hydroxide, 26 parts of the repair enhancer prepared in Comparative Preparation Example 6, 3 parts of carbon black masterbatch, 2 parts of calcium stearate and 2 parts of fluoroalkyl polyether modified polysiloxane, and then extruding and molding through a twin-screw extruder, wherein the extrusion process of the twin-screw extruder is: zone 1 170°C, zone 2 180°C, zone 3 185°C, zone 4 190°C, zone 5 195°C, die head temperature 200°C; screw speed 200rpm;

[0203] The silicone rubber comprises the following raw materials in parts by weight: 58 parts of methyl vinyl silicone rubber, 32 parts of thermoplastic polyurethane elastomer, 16 parts of trioctyl phosphate, 4 parts of dibutyl malonate, 1 part of L-cyclohexylglycine, 2 parts of diethylene glycol butyl ether acetate, 0.6 parts of accelerator TMTD and 3 parts of 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane;

[0204] The preparation method of the silicone rubber comprises the following steps:

[0205] Step M1, adding methyl vinyl silicone rubber raw rubber, thermoplastic polyurethane elastomer, trioctyl phosphate, dibutyl malonate, L-cyclohexylglycine and diethylene glycol butyl ether acetate into a kneader by weight, mixing at 80° C. for 2 hours, maintaining the temperature unchanged, continuing to mix at a vacuum degree of -0.1 MPa for another 3 hours, cooling to room temperature, and obtaining a vulcanizing agent-free mixed rubber; then, the vulcanizing agent-free mixed rubber, accelerator TMTD and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane are thinly passed on a double-roll mill for 3 times to obtain a vulcanizing agent-containing mixed rubber;

[0206] Step M2, forming the mixed rubber containing the vulcanizing agent prepared in step M1, and vulcanizing it on a flat vulcanizer at a pressure of 8 MPa and a temperature of 160° C. for 10 minutes to obtain a primary vulcanized silicone rubber;

[0207] Step M3, subjecting the primary vulcanized silicone rubber to secondary vulcanization at 160° C. for 3 h to obtain silicone rubber.

[0208] Performance Testing

[0209] The inner sheaths of the wires and cables prepared in Examples 1-3 and Comparative Examples 1-3 were tested for tensile strength and environmental stress cracking resistance according to GB / T1040 "Determination of tensile properties of plastics" and GB / T1842-2008 "Test method for environmental stress cracking of plastic polyethylene"; the water absorption rate of the inner sheath was determined according to GB / T 11547-2008; the antioxidant properties: at a wavelength of 365nm and a light intensity of 6000μw / cm 2 The samples were exposed to ultraviolet light for 30 days. The elongation at break retention of each group of samples after exposure for 30 days was measured according to GB / T1040 "Determination of tensile properties of plastics". The test results are shown in Table 1:

[0210] Table 1 Mechanical properties, waterproofness and oxidation resistance test of the inner sheath of wires and cables

[0211]

[0212] It can be seen from Table 1 that, compared with Comparative Examples 1-3, the cable inner sheath prepared in Examples 1-3 has higher tensile strength and lower absorption rate, and the elongation at break is higher during ultraviolet treatment. Therefore, the wires and cables prepared in the present invention have excellent mechanical properties, waterproofness and oxidation resistance.

[0213] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A processing technology for environmentally friendly and anti-oxidation wires and cables, characterized in that: The following steps are involved: Step S1, preparing a conductor: selecting galvanized copper wires and tinned copper wires with diameters of 0.25-0.45 mm respectively, arranging the galvanized copper wires and the tinned copper wires at intervals, and twisting them tightly together to obtain a conductor; Step S2, preparing an isolation layer: extruding cross-linked polyethylene to initially form a tube with a thickness of 3-5 mm matching the conductor, and further stretching it to tightly cover the conductor to form an isolation layer; Step S3, preparing an inner protective layer: after wrapping the isolation layer with an alloy mesh material having a thickness of 1-1.5 mm, the functionalized polyethylene is directly extruded on the isolation layer wrapped with the alloy mesh material to form an inner protective layer with a compact structure; Step S4, preparing wires and cables: finally, extruding the silicone rubber outside the inner sheath to form a compact covering layer, thereby obtaining environmentally friendly and anti-oxidation wires and cables; The functionalized polyethylene is prepared by uniformly blending 100-120 parts of high-density polyethylene, 22-28 parts of maleic anhydride grafted polyethylene, 14-30 parts of aluminum hydroxide, 26-32 parts of a repair enhancer, 3-5 parts of a carbon black masterbatch, 2-4 parts of a processing aid and 2-3 parts of a fluoroalkyl polyether modified polysiloxane, and then extruding and molding the mixture through a twin-screw extruder. The repair enhancer is prepared by the following steps: Step A1, uniformly mix urea, formaldehyde aqueous solution and deionized water, adjust the pH to 8-9, heat to 65-75°C, keep warm for 1-2h, cool to room temperature, and obtain urea-formaldehyde prepolymer solution; Step A2, adding sodium dodecylbenzene sulfonate and functional monomers into deionized water, heating to 35-45° C., and continuously stirring to form an emulsion; Step A3, adding the urea-formaldehyde prepolymer solution dropwise to the emulsion prepared in step A2 while stirring, then adding ammonium chloride and a water-resistant modifier, continuing stirring for 4-8 minutes, adding n-octanol dropwise, adjusting the pH to 2.8-3.2 after the addition, heating to 58-62° C., keeping the temperature and stirring for 2.6-3.2 hours, filtering, washing, and drying to obtain a repair enhancer; The water-resistant modifier is prepared by the following steps: Step B1, under nitrogen protection, add p-hydroxydiphenylamine and acryloyl chloride to anhydrous ethanol, stir evenly, then add triethylamine, heat to reflux, stir and react for 4-6 hours, after the reaction is completed, extract, and concentrate the organic phase under reduced pressure to obtain a hydroxyl monomer; Step B2, adding hydroxyl monomer, 2-mercaptonicotinic acid and benzoin dimethyl ether to anhydrous ethanol, stirring evenly, maintaining the rotation speed unchanged, placing under ultraviolet irradiation for 15-25 minutes while stirring, and controlling the irradiation temperature to be 35-45° C. After the reaction is completed, removing anhydrous ethanol, and then washing and drying to obtain a pyridine compound; Step B3, add the pyridine compound and 4,6-diaminopyrimidine to anhydrous DMF, stir evenly, and dropwise add a mixed solution a of N,N'-dicyclohexylcarbodiimide, 4-dimethylaminopyridine and anhydrous DMF while stirring. After the dropwise addition, heat to 65-75°C, stir to react for 2-3h, and after the reaction is completed, cool to room temperature, filter with suction, wash and dry the filter cake to obtain a water-resistant modifier; The functional monomer is prepared by the following steps: Step C1, ultrasonically dispersing 3,3'-dithiodipropionic acid in anhydrous DMF, adding tetrabutylammonium bromide, allyl glycidyl ether and anhydrous DMF mixed solution b dropwise, and after the addition is completed, heating to 95-105° C., stirring and reacting for 2-3 hours, and after the reaction is completed, centrifuging, washing, and drying to obtain an allyl monomer; Step C2, under nitrogen protection, add allyl monomer and Custer catalyst to toluene, heat to 35-45°C, stir evenly, then add triethoxysilane, continue to heat to 65-75°C, stir and react for 18-24h, remove toluene after the reaction is completed, and obtain functional monomer.

2. The processing technology of an environmentally friendly and anti-oxidation wire and cable according to claim 1 is characterized in that: In step A1, the mass ratio of urea, formaldehyde aqueous solution and deionized water is 5-6:12-16:42-46, in step A2, the mass ratio of sodium dodecylbenzene sulfonate, functional monomer and deionized water is 0.8-1.2:12-14:100-120, and in step A3, the mass ratio of urea-formaldehyde prepolymer solution, emulsion, ammonium chloride, water-resistant modifier and n-octanol is 20-22:110-130:0.3-0.6:1.6-2.0:0.04-0.

06.

3. The processing technology of an environmentally friendly and anti-oxidation wire and cable according to claim 1 is characterized in that: In the step B1, the mass ratio of p-hydroxydiphenylamine, acryloyl chloride, anhydrous ethanol and triethylamine is 2.6-2.8:1.2-1.4:45-65:0.02-0.04; in the step B2, the mass ratio of hydroxyl monomer, 2-mercaptonicotinic acid, benzoin dimethyl ether and anhydrous ethanol is 2.1-2.5:1.1-1.5:0.02-0.04:35-45; in the step B3, the mass ratio of pyridine compound, 4,6-diaminopyrimidine, anhydrous DMF and mixed solution a is 3.6-4.0:0.8-1.2:40-50:10; in the mixed solution a, the mass ratio of N,N'-dicyclohexylcarbodiimide, 4-dimethylaminopyridine and anhydrous DMF is 1.8-2.2:1.4-1.6:

15.

4. The processing technology of an environmentally friendly and anti-oxidation wire and cable according to claim 1 is characterized in that: In the step C1, the mass ratio of 3,3'-dithiodipropionic acid, anhydrous DMF and mixed solution b is 4-5:45-55:14, in the mixed solution b, the mass ratio of tetrabutylammonium bromide, allyl glycidyl ether and anhydrous DMF is 0.02-0.04:2.2-2.6:12-14, and in the step C2, the mass ratio of allyl monomer, Custer catalyst, toluene and triethoxysilane is 2.2-2.6:0.25-0.35:30-40:0.9-1.

3.

5. The processing technology of an environmentally friendly and anti-oxidation wire and cable according to claim 1 is characterized in that: The silicone rubber comprises the following raw materials in parts by weight: 58-65 parts of methyl vinyl silicone rubber, 32-40 parts of thermoplastic polyurethane elastomer, 16-20 parts of trioctyl phosphate, 4-5 parts of dibutyl malonate, 1-3 parts of L-cyclohexylglycine, 2-4 parts of diethylene glycol butyl ether acetate, 0.6-0.8 parts of accelerator and 3-5 parts of vulcanizer.

6. The processing technology of an environmentally friendly and anti-oxidation wire and cable according to claim 5 is characterized in that: The preparation method of silicone rubber comprises the following steps: Step M1, adding methyl vinyl silicone rubber raw rubber, thermoplastic polyurethane elastomer, trioctyl phosphate, dibutyl malonate, L-cyclohexylglycine and diethylene glycol butyl ether acetate into a kneader by weight, mixing at 80-100° C. for 2-3 hours, maintaining the temperature unchanged, mixing in vacuum for 3-5 hours, cooling to room temperature, and obtaining a vulcanizing agent-free mixed rubber; then, the vulcanizing agent-free mixed rubber, accelerator and vulcanizing agent are thinly passed on a double-roll mill for 3-5 times to obtain a vulcanizing agent-containing mixed rubber; Step M2, forming the mixed rubber containing the vulcanizing agent prepared in step M1, and vulcanizing it on a flat vulcanizer at a pressure of 8-15 MPa and a temperature of 160-180° C. for 10-20 minutes to obtain a primary vulcanized silicone rubber; Step M3, subjecting the primary vulcanized silicone rubber to secondary vulcanization at 160-240° C. for 3-7 hours to obtain silicone rubber.

7. An environmentally friendly, antioxidant wire and cable obtained by the processing technology described in any one of claims 1 to 6.