Method for forming LDMOS device

By integrating NPN and PNP tube structures in LDMOS devices, improving the surface electric field, solving the problem of on-resistance and shutdown breakdown voltage increase in the prior art, achieving higher performance.

CN118571762BActive Publication Date: 2024-11-22HANGZHOU HFC SEMICONDUCTOR CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411044906.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-22
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

Existing high-voltage LDMOS devices are already close to their limits in reducing on-resistance and increasing the shutdown breakdown voltage, and are difficult to further improve.

Method used

By forming a light doped ion region, a sacrificial oxide layer and a P-type silicon structure in the LDMOS device, several NPN and PNP tubes are integrated to improve the surface electric field, reduce the on-resistance and increase the shutdown breakdown voltage.

Benefits of technology

It effectively reduces the on-resistance, improves the shutdown breakdown voltage, and improves the device performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118571762B_ABST
    Figure CN118571762B_ABST
Patent Text Reader

Abstract

The present invention provides a method for forming an LDMOS device, comprising: sequentially forming a P-type body region and an N-type drift region located in the P-type body region in a substrate, wherein the surfaces of the substrate, the P-type body region and the N-type drift region are all flush; forming a gate structure, wherein the gate structure covers a portion of the surface of the P-type body region and a portion of the surface of the N-type drift region; forming a lightly doped ion region in the P-type body region, wherein the lightly doped ion region is located on a side of the gate structure opposite to the N-type drift region; forming a sacrificial oxide layer on the surface of the gate structure, the surface of the P-type body region and the surface of the N-type drift region; forming P-type silicon in the N-type drift region, wherein the P-type silicon extends radially along the gate structure; and forming a plurality of spaced N-type silicons in the P-type silicon. The present invention improves the surface electric field close to the silicon surface, reduces the on-resistance, and increases the off-breakdown voltage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a method for forming an LDMOS device. Background Art

[0002] High-voltage LDMOS has always been a core device in power integrated circuits due to its high input impedance, low loss, fast switching speed, wide safe operating area and easy integration. It is widely used in various fields such as mobile communications, automotive electronics, and LED lighting.

[0003] The performance of high-voltage LDMOS often requires the ability to withstand high voltage while minimizing the specific on-resistance. To achieve this goal, commonly used technologies include lateral superjunction and surface field reduction (RESURF) technology. Both of them introduce opposite charge compensation layers in the drift region, which deplete each other with the drift region in the off state to achieve the purpose of optimizing the electric field and increasing the doping concentration of the drift region, thereby reducing the specific on-resistance in the on state.

[0004] However, the drift regions of conventional super junction and surface field reduction technologies in the prior art only have auxiliary depletion from charge compensation layers on both sides, and their improvement on device performance is approaching the limit. Summary of the invention

[0005] The object of the present invention is to provide a method for forming an LDMOS device, which can improve the surface electric field close to the silicon surface, reduce the on-resistance, and increase the off-breakdown voltage.

[0006] In order to achieve the above object, the present invention provides a method for forming an LDMOS device, comprising:

[0007] Providing a substrate, sequentially forming a P-type body region and an N-type drift region located in the P-type body region in the substrate, wherein surfaces of the substrate, the P-type body region and the N-type drift region are all flush;

[0008] A gate structure is formed on the surface of the P-type body region and the surface of the N-type drift region, wherein the gate structure covers a portion of the surface of the P-type body region and a portion of the surface of the N-type drift region;

[0009] forming a lightly doped ion region in the P-type body region, wherein the lightly doped ion region is located on a side of the gate structure opposite to the N-type drift region;

[0010] forming a sacrificial oxide layer on the surface of the gate structure, the surface of the P-type body region, and the surface of the N-type drift region;

[0011] Forming P-type silicon in the N-type drift region, wherein the P-type silicon extends along the radial direction of the gate structure;

[0012] A plurality of N-type silicons are formed in the P-type silicon.

[0013] Optionally, in the method for forming the LDMOS device, ions are implanted into the P-type body region to form an N-type drift region.

[0014] Optionally, in the method for forming the LDMOS device, the amount of implanted ions is 1.0e 12 ~1.0e 14 .

[0015] Optionally, in the method for forming the LDMOS device, the method for forming the gate structure includes:

[0016] A gate oxide layer is formed on the surface of the P-type body region and the surface of the N-type drift region, and a gate is formed on the surface of the gate oxide layer.

[0017] Optionally, in the method for forming the LDMOS device, after sequentially forming a P-type body region and an N-type drift region located in the P-type body region in the substrate, the method further includes:

[0018] The N-type drift region is annealed.

[0019] Optionally, in the method for forming the LDMOS device, after a sacrificial oxide layer is formed on the surface of the gate structure, the surface of the P-type body region and the surface of the N-type drift region, it also includes: forming a hard mask layer on the surface of the sacrificial oxide layer.

[0020] Optionally, in the method for forming the LDMOS device, a method for forming P-type silicon in the N-type drift region, and extending the P-type silicon along the radial direction of the gate structure includes:

[0021] Etching the sacrificial oxide layer and the N-type drift region to form a trench in the N-type drift region;

[0022] P-type silicon is formed in the trench by epitaxial growth.

[0023] Optionally, in the method for forming the LDMOS device, the method for forming a plurality of spaced N-type silicons in the P-type silicon includes:

[0024] Etching the P-type silicon to form a plurality of spaced grooves in the P-type silicon;

[0025] N-type silicon is formed in the groove by epitaxial growth.

[0026] Optionally, in the method for forming the LDMOS device, the method for forming a plurality of spaced N-type silicons in the P-type silicon includes:

[0027] forming a photoresist layer having a plurality of spaced through holes on the surface of the sacrificial oxide layer and the surface of the P-type silicon;

[0028] Ions are implanted into the P-type silicon through the through hole to form a plurality of N-type silicons in the P-type silicon.

[0029] Optionally, in the method for forming the LDMOS device, after forming a plurality of spaced N-type silicons in the P-type silicon, the method further includes:

[0030] Sidewall spacers are formed on both sides of the gate, and the sidewall spacers are separated from the sides of the gate by a sacrificial oxide layer.

[0031] The method for forming an LDMOS device provided by the present invention includes: providing a substrate, sequentially forming a P-type body region and an N-type drift region located in the P-type body region in the substrate, and the surfaces of the substrate, the P-type body region and the N-type drift region are all flush; forming a gate structure, the gate structure covers a part of the surface of the P-type body region and a part of the surface of the N-type drift region; forming a lightly doped ion region in the P-type body region, the lightly doped ion region is located on the side of the gate structure opposite to the N-type drift region; forming a sacrificial oxide layer on the surface of the gate structure, the surface of the P-type body region and the surface of the N-type drift region; forming P-type silicon in the N-type drift region, the P-type silicon extends radially along the gate structure; forming a plurality of spaced N-type silicon in the P-type silicon. The present invention integrates N-type silicon and P-type silicon together to form a plurality of NPN tubes and PNP tubes. Thereby, the surface electric field close to the silicon surface is improved, the on-resistance is reduced, and the off-breakdown voltage is increased. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 is a flow chart of a method for forming an LDMOS device according to an embodiment of the present invention;

[0033] Figure 2 is a schematic structural diagram of an LDMOS device after forming an N-type drift region according to an embodiment of the present invention;

[0034] Figure 3 is a schematic structural diagram of an LDMOS device after forming a sacrificial oxide layer according to an embodiment of the present invention;

[0035] Figure 4 is a schematic structural diagram of an LDMOS device after a hard mask layer is formed according to an embodiment of the present invention;

[0036] Figure 5 is a schematic structural diagram of an LDMOS device after forming P-type silicon according to an embodiment of the present invention;

[0037] Figure 6 is a schematic structural diagram of an LDMOS device after forming N-type silicon according to an embodiment of the present invention;

[0038] Figure 7 is a schematic structural diagram of an LDMOS device after forming a drain region according to an embodiment of the present invention;

[0039] In the figure: 210-P type body region, 220-N type drift region, 230-gate oxide layer, 240-gate, 250-sacrificial oxide layer, 260-lightly doped ion region, 270-hard mask layer, 280-P type silicon, 290-N type silicon, 300-side wall, 310-source region, 320-drain region. DETAILED DESCRIPTION

[0040] The specific implementation of the present invention will be described in more detail below in conjunction with the schematic diagram. The advantages and features of the present invention will become clearer based on the following description. It should be noted that the drawings are all in a very simplified form and are not in exact proportions, and are only used to facilitate and clearly assist in explaining the purpose of the embodiments of the present invention.

[0041] Hereinafter, the terms "first", "second", etc. are used to distinguish between similar elements and are not necessarily used to describe a particular order or chronological sequence. It is to be understood that these terms used in this manner are interchangeable where appropriate. Similarly, if the method described herein includes a series of steps, the order of these steps presented herein is not necessarily the only order in which these steps can be performed, and some of the steps described may be omitted and / or some other steps not described herein may be added to the method.

[0042] Furthermore, it should be understood that when a layer (or film), region, pattern or structure is referred to as being "on" a substrate, layer (or film), region and / or pattern, it can be directly on another layer or substrate, and / or there can be intervening layers. In addition, it should be understood that when a layer is referred to as being "under" another layer, it can be directly under another layer, and / or there can be one or more intervening layers. In addition, references to being "on" and "under" each layer can be made based on the accompanying drawings.

[0043] Please refer to Figure 1 The present invention provides a method for forming an LDMOS device, comprising:

[0044] S11: providing a substrate, and sequentially forming a P-type body region and an N-type drift region located in the P-type body region in the substrate, wherein surfaces of the substrate, the P-type body region, and the N-type drift region are all flush;

[0045] S12: forming a gate structure, where the gate structure covers a portion of the surface of the P-type body region and a portion of the surface of the N-type drift region;

[0046] S13: forming a lightly doped ion region in the P-type body region, wherein the lightly doped ion region is located on a side of the gate structure opposite to the N-type drift region;

[0047] S14: forming a sacrificial oxide layer on the surface of the gate structure, the surface of the P-type body region, and the surface of the N-type drift region;

[0048] S15: forming P-type silicon in the N-type drift region, and the P-type silicon extends along the radial direction of the gate structure;

[0049] S16: forming a plurality of spaced N-type silicons in the P-type silicon.

[0050] For details, please refer to Figure 2 First, a substrate is provided. The substrate may be a silicon substrate, for example, a wafer. In other embodiments of the present invention, it may also be other types of substrates, such as a germanium substrate. A P-type body region 210 is formed in the substrate by ion implantation. The P-type body region 210 is close to the surface of the substrate, and the surface of the P-type body region 210 is flush with the surface of the substrate. Next, ions are implanted in the P-type body region 210 to form an N-type drift region 220. The N-type drift region 220 is close to the surface of the P-type body region 210, and the surface of the N-type drift region 220 is flush with the surface of the P-type body region 210. The dose of ion implantation to form the N-type drift region 220 may be 1.0e 12 ~1.0e 14 Next, the N-type drift region 220 is annealed.

[0051] Next, please refer to Figure 3 , an oxide layer is formed on the surface of the P-type body region 210 and the surface of the N-type drift region 220, which can be formed by depositing silicon dioxide. A gate polysilicon layer is formed on the surface of the oxide layer, and part of the gate polysilicon and part of the oxide layer are etched to form a gate 240 and a gate oxide layer 230. The gate oxide layer 230 covers part of the surface of the P-type body region 210 and part of the surface of the N-type drift region 220, that is, part of the surface of the P-type body region 210 and part of the surface of the N-type drift region 220 are exposed. The gate 240 is located on the surface of the gate oxide layer 230, and the gate oxide layer 230 and the gate 240 form a gate structure. Next, a sacrificial oxide layer 250 is formed on the gate 240 and the exposed surface of the part of the P-type body region 210 and the surface of the part of the N-type drift region 220. The material of the sacrificial oxide layer 250 can be silicon dioxide, and the sacrificial oxide layer 250 can be formed by depositing silicon dioxide.

[0052] Next, please refer to Figure 4, a photoresist layer is formed on the surface of the sacrificial oxide layer 250, and a portion of the photoresist layer is removed to expose the sacrificial oxide layer 250 on the surface of a portion of the P-type body region 210 on one side of the gate 240. Ions are injected into the P-type body region 210 starting from the surface of the sacrificial oxide layer 250 not covered by the photoresist layer, thereby forming a lightly doped ion (LDD) region 260 in the P-type body region 210. Next, the photoresist layer is removed, and a hard mask layer 270 is formed on the surface of the sacrificial oxide layer 250. The material of the hard mask layer 270 is silicon nitride, so it can be formed by depositing silicon nitride. Forming the hard mask layer 270 is an optional step, so in other embodiments of the present invention, the hard mask layer 270 may not be formed.

[0053] Next, please refer to Figure 5 , a photoresist layer is formed on the surface of the hard mask layer 270, and the photoresist layer is patterned, and the patterned photoresist layer exposes the hard mask layer 270 on the surface of a portion of the N-type drift region 220. In other embodiments of the present invention, if the hard mask layer 270 is not formed, the sacrificial oxide layer 250 on the surface of a portion of the N-type drift region 220 is exposed. Next, a portion of the hard mask layer 270, the sacrificial oxide layer 250 and the N-type drift region 220 are etched to form a groove in the N-type drift region 220. In other embodiments of the present invention, if the hard mask layer 270 is not formed, a portion of the sacrificial oxide layer 250 and the N-type drift region 220 are etched to form a groove in the N-type drift region 220. Next, the photoresist layer is removed. Next, a P-type silicon 280 is formed in the groove by epitaxial growth, and the surface of the P-type silicon 280 is flush with the surface of the N-type drift region 220. The P-type silicon 280 extends along the radial direction of the gate 240.

[0054] Next, please refer to Figure 6 , a photoresist layer is formed on the surface of the hard mask layer 270 and the surface of the P-type silicon 280, and the photoresist layer is patterned so that the patterned photoresist layer forms a plurality of spaced through holes, and the surface of the P-type silicon 280 is exposed in the through holes. A partial thickness of the P-type silicon 280 is etched from the through holes, thereby forming a plurality of spaced grooves in the P-type silicon 280. Then, a plurality of spaced N-type silicon 290 are formed in the P-type silicon 280 by epitaxial growth in the grooves. The surfaces of all N-type silicon 290 are flush with the surfaces of the P-type silicon 280. In other embodiments of the present invention, ions can also be injected into the P-type silicon 280 through the through holes of the patterned photoresist layer to form a plurality of N-type silicon 290 in the P-type silicon 280. The surfaces of all N-type silicon 290 are flush with the surfaces of the P-type silicon 280.

[0055] Next, please refer to Figure 7, remove the photoresist layer, if there is no hard mask layer 270, the surface of the sacrificial oxide layer 250 is exposed. If there is a hard mask layer 270, the hard mask layer 270 is also removed to expose the surface of the sacrificial oxide layer 250. Next, the lightly doped ion region 260 is annealed.

[0056] Next, please continue to refer to Figure 7 , remove part of the sacrificial oxide layer 250, and only retain the sacrificial oxide layer 250 on both sides of the gate 240. Next, a sidewall 300 is formed on both sides of the gate 240, and the sidewall 300 is separated from the side of the gate 240 by the sacrificial oxide layer 250. The sidewall 300 is spaced a certain distance from both the N-type silicon 290 and the P-type silicon 280.

[0057] Next, please continue to refer to Figure 7 Ions are implanted into the lightly doped ion region 260 and the N-type drift region 220 to form a source region 310 and a drain region 320. The source region 310 or the drain region 320 in the N-type drift region 220 is spaced a certain distance from the N-type silicon 290 and the P-type silicon 280.

[0058] The embodiment of the present invention integrates N-type silicon 290 and P-type silicon 280 together, and forms a plurality of NPN tubes and PNP tubes, which are cross-formed on the surface close to the N-type drift region 220 and the surface of the substrate. This improves the surface electric field close to the silicon surface, reduces the on-resistance, and increases the off-breakdown voltage.

[0059] Therefore, the LDMOS device formed by the LDMOS device forming method of the embodiment of the present invention includes: a substrate, a P-type body region located in the substrate and an N-type drift region located in the P-type body region; a gate structure located on the surface of the P-type body region and the surface of the N-type drift region; P-type silicon located in the N-type drift region, the P-type silicon being separated from the gate structure by a sidewall and a sacrificial oxide layer; and a plurality of spaced N-type silicons located in the P-type silicon.

[0060] In summary, the method for forming an LDMOS device provided in an embodiment of the present invention includes: providing a substrate, sequentially forming a P-type body region and an N-type drift region located in the P-type body region in the substrate, and the surfaces of the substrate, the P-type body region and the N-type drift region are all flush; forming a gate structure, the gate structure covers a portion of the surface of the P-type body region and a portion of the surface of the N-type drift region; forming a lightly doped ion region in the P-type body region, the lightly doped ion region is located on the side of the gate structure opposite to the N-type drift region; forming a sacrificial oxide layer on the surface of the gate structure, the surface of the P-type body region and the surface of the N-type drift region; forming P-type silicon in the N-type drift region, the P-type silicon extends radially along the gate structure; forming a number of spaced N-type silicon in the P-type silicon. The present invention integrates N-type silicon and P-type silicon together to form a number of NPN tubes and PNP tubes. Thereby, the surface electric field close to the silicon surface is improved, the on-resistance is reduced, and the off breakdown voltage is increased.

[0061] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any technician in the relevant technical field, without departing from the scope of the technical solution of the present invention, makes any form of equivalent replacement or modification to the technical solution and technical content disclosed in the present invention, which does not depart from the content of the technical solution of the present invention and still falls within the protection scope of the present invention.

Claims

1. A method for forming an LDMOS device, characterized in that: include: Providing a substrate, sequentially forming a P-type body region and an N-type drift region located in the P-type body region in the substrate, wherein surfaces of the substrate, the P-type body region and the N-type drift region are all flush; forming a gate structure, wherein the gate structure covers a portion of the surface of the P-type body region and a portion of the surface of the N-type drift region; forming a lightly doped ion region in the P-type body region, wherein the lightly doped ion region is located on a side of the gate structure opposite to the N-type drift region; forming a sacrificial oxide layer on the surface of the gate structure, the surface of the P-type body region, and the surface of the N-type drift region; Forming P-type silicon in the N-type drift region, wherein the P-type silicon extends along the radial direction of the gate structure; A plurality of N-type silicons are formed in the P-type silicon.

2. The method for forming an LDMOS device according to claim 1, wherein: Ions are implanted into the P-type body region to form an N-type drift region.

3. The method for forming an LDMOS device according to claim 2, wherein: The amount of implanted ions is 1.0e 12 ~1.0e 14 .

4. The method for forming an LDMOS device according to claim 1, wherein: The method of forming a gate structure includes: A gate oxide layer is formed on the surface of the P-type body region and the surface of the N-type drift region, and a gate is formed on the surface of the gate oxide layer.

5. The method for forming an LDMOS device according to claim 1, wherein: After sequentially forming a P-type body region and an N-type drift region located in the P-type body region in the substrate, the method further includes: The N-type drift region is annealed.

6. The method for forming an LDMOS device according to claim 1, wherein: After forming a sacrificial oxide layer on the surface of the gate structure, the surface of the P-type body region and the surface of the N-type drift region, the method further includes: forming a hard mask layer on the surface of the sacrificial oxide layer.

7. The method for forming an LDMOS device according to claim 1, wherein: A method for forming P-type silicon in the N-type drift region, wherein the P-type silicon extends radially along the gate structure, comprises: Etching the sacrificial oxide layer and the N-type drift region to form a trench in the N-type drift region; P-type silicon is formed in the trench by epitaxial growth.

8. The method for forming an LDMOS device according to claim 1, wherein: The method of forming a plurality of spaced N-type silicons in the P-type silicon comprises: Etching the P-type silicon to form a plurality of spaced grooves in the P-type silicon; N-type silicon is formed in the groove by epitaxial growth.

9. The method for forming an LDMOS device according to claim 1, wherein: The method of forming a plurality of spaced N-type silicons in the P-type silicon comprises: forming a photoresist layer having a plurality of spaced through holes on the surface of the sacrificial oxide layer and the surface of the P-type silicon; Ions are implanted into the P-type silicon through the through hole to form a plurality of N-type silicons in the P-type silicon.

10. The method for forming an LDMOS device according to claim 1, wherein: After forming a plurality of spaced N-type silicon in the P-type silicon, the method further comprises: Sidewall spacers are formed on both sides of the gate, and the sidewall spacers are separated from the sides of the gate by a sacrificial oxide layer.