A piezoelectric crystal processing method

By adopting a multi-step method of orientation, cutting and grinding in piezoelectric crystal processing, the problem of crystal orientation deviation in the existing technology is solved, high-precision piezoelectric crystal processing is achieved, and the precision and application performance of the crystal rod are improved. .

CN118578532BActive Publication Date: 2024-10-22TDG HLDG CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411075476.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-22
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

Existing piezoelectric crystal processing technology has crystal orientation deviation problems during the orientation and cutting processes, resulting in insufficient precision and accuracy and affecting the application performance of the device.

Method used

A piezoelectric crystal processing method is adopted, including the steps of orientation, head and tail cutting, end face grinding and cylindrical grinding. The crystal orientation deviation in the direction A and B of the crystal end face is measured with an orientation meter, and a special cutting fixture and a single wire cutting machine are used for precise cutting. The crystal orientation is corrected based on geometric calculations, and grinding is performed on a surface grinder and a cylindrical grinder to ensure that the crystal accurate orientation and outer circle smoothness.

Benefits of technology

It achieves high-precision orientation and cutting of the crystal, controls the crystal direction deviation within 12′, reduces line marks and missing angles, improves the cylindricity and straightness of the crystal, and ensures high-precision processing of crystal rods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118578532B_ABST
    Figure CN118578532B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of crystal processing, and specifically to a piezoelectric crystal processing method, comprising the following steps: a) orientation: placing a crystal vertically on an orientation instrument, finding the crystal direction of a crystal end face direction A, marking a horizontal reference line on the crystal X face, and then placing the crystal horizontally on a special cutting fixture, adjusting the crystal inclination angle, obtaining the crystal direction of a crystal end face direction B, and accurately orienting; b) head and tail cutting: adjusting the position of a cutting line to align it with a horizontal reference line, and then translating a special cutting fixture to align the cutting line with a minimum diameter point at the end of the crystal, and cutting the head and tail ends of the crystal respectively, with high cutting accuracy; c) end face grinding: grinding the head and tail end faces of the crystal flat, and then correcting the end face crystal direction, realizing one-time correction by calculating the crystal direction deviation, and achieving high efficiency; d) external cylindrical grinding: grinding the outer circle of the crystal according to a target diameter, and obtaining a crystal rod with a smooth appearance, no scratches or cracks, a more standardized appearance, and a small crystal direction deviation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of crystal processing, and specifically to a piezoelectric crystal processing method. Background Art

[0002] Piezoelectric crystals can be widely used in mobile phones, multimedia data broadcasting systems (such as VOD, etc.), automotive electronics, wireless LAN and digital TV filters, oscillators and other components. Due to the miniaturization of various devices, the internal components are required to be made more precisely, and the precision requirements for piezoelectric crystal processing are increased, especially the accuracy requirements for the crystal orientation of the applied wafers are also getting higher and higher, which has an important impact on the application performance of the device. This requires more accurate crystal rod orientation, cutting and grinding during the piezoelectric crystal processing.

[0003] In order to solve this problem, the patent with the announcement number CN211930601U discloses an orientation fixture for a crystal rod for a surface acoustic wave filter. This utility model invents an orientation fixture, which uses a universal wheel to enable the upper turntable to deflect within a certain angle range, and bolts are used for angle adjustment and mutual support between the two turntables. When the crystal is oriented by this structure, the directions A and B need to be adjusted by the universal wheel respectively, which is prone to deviation; the patent with the publication number CN108000291A discloses an automatic orientation auxiliary device for c-plane correction of a sapphire crystal rod. In order to realize the rapid and accurate determination of the crystal orientation deviation of the sapphire end face, this invention patent uses the crystal orientation deviation determined by an XRD ray diffractometer, and uses a nozzle to automatically mark the crystal orientation deviation direction on the arc surface of the crystal rod. The crystal orientation deviation point is positioned by the nozzle method in this invention, but the position accuracy is not high, and it is easy to have a large best crystal orientation deviation. Summary of the invention

[0004] To solve the above problems, the present invention aims to provide a piezoelectric crystal processing method.

[0005] A piezoelectric crystal processing method comprises the following steps:

[0006] a) Orientation: The processed crystal is a Y-axis biased Z-axis crystal. The crystal is placed vertically on a fixed fixture and placed on an orientator with the positive X-face of the crystal facing forward. The crystal direction of the crystal end face direction A is found. Then a horizontal reference line is marked in the middle of the crystal X-face. After removing the crystal, it is placed horizontally on the resin strip of the special cutting fixture and placed on the orientator with the positive X-face of the crystal facing upward. The special cutting fixture is equipped with an azimuth adjustment component that can adjust the crystal tilt angle to find the crystal X-face crystal direction. The vertical direction is the crystal direction of the crystal end face direction B. Then the crystal, resin strip and special cutting fixture are fixed at this angle and moved as a whole to the single-wire saw for head-to-tail cutting.

[0007] b) Cutting the head and tail: adjust the position of the cutting line to align it with the horizontal reference line, then translate the special cutting fixture to align the cutting line with the minimum diameter point at the end of the crystal, and cut the head and tail of the crystal respectively;

[0008] c) End face grinding: remove the crystal from the resin strip, grind the end faces of the crystal head and tail, and then correct the end face crystal direction. The correction method is: first use an orientation instrument to measure the crystal direction deviation of the crystal end face direction A and the crystal end face direction B of one end face of the crystal, draw two straight lines representing the crystal end face direction A and the crystal end face direction B on the end face, the two straight lines pass through the center of the end face, and draw a rectangle with the center point as an angle and the two straight lines as sides. The lengths of the two rectangular sides are required to be proportional to the crystal direction deviation values ​​of the crystal end face direction A and the crystal end face direction B, respectively. Connect the diagonal of the rectangle corresponding to the center point, and extend the intersection of the diagonal line and the edge of the end face to be the crystal direction correction padding point. According to the geometric relationship between the crystal end face diameter and the rectangular side, calculate the padding height required for the crystal end face direction A and the crystal end face direction B corresponding to the crystal direction deviation. After padding the padding point to a corresponding height, place it on a surface grinder for crystal direction correction;

[0009] d) External cylindrical grinding: After the crystal end face crystal orientation is corrected, the outer circle of the crystal is ground according to the target diameter to obtain a crystal rod.

[0010] Wherein, in step a), the processed crystal is a Y-axis-biased Z-axis crystal, and the reference edge is the X-axis, such as Y42°, Y46°, Y50°, etc.

[0011] Preferably, the processed crystal is lithium tantalate, lithium niobate, quartz, barium titanate or gallium arsenide.

[0012] Among them, in step a), the orientation instrument mainly measures the diffraction angle of the crystal end face direction A and the diffraction angle of the crystal end face direction B by emitting X-rays, and determines the crystal directions in two directions respectively. The crystal direction of the crystal end face direction A is the crystal direction angle of the Y axis offset from the Z axis, and the crystal direction of the crystal end face direction B is the X-axis direction of the crystal end face.

[0013] Among them, in step a), the orientation adjustment component in the special cutting fixture is a structure with adjustable tilt angle such as an adjusting nut and an angle meter. Changing the orientation of the crystal on the vertical plane through this component helps to find the diffraction angle of the crystal X plane.

[0014] Among them, in step a), the crystal end face direction A and the crystal end face direction B are oriented twice respectively, and the orientation is accurate. If the traditional fixture is used for one-time orientation, when the crystal end face direction A is adjusted and then the crystal end face direction B is oriented, when the crystal tilt position is adjusted, it is easy to cause the crystal to move slightly on the adjusted crystal end face direction A, thereby causing the crystal direction deviation of the crystal end face direction A.

[0015] In step b), when cutting the head and tail of the crystal, a single-wire diamond wire cutting machine is used for cutting. This is because if inner circle cutting is used, the position of the minimum processable diameter of the crystal cannot be accurately aligned, which is prone to waste or repeated cutting.

[0016] Preferably, in step c), the head and tail end faces of the crystal are firstly ground flat using a coarse grinding wheel, and then the end face crystal orientation is corrected using a fine grinding wheel;

[0017] Preferably, in step c), the crystal orientation deviations of the crystal end face direction A and the crystal end face direction B of one end face of the crystal are respectively recorded as a and b , the diameter of the crystal end face is recorded as L Through geometric conversion, the required height of the pad corresponding to the crystal orientation deviation in the crystal end face direction A and the crystal end face direction B is obtained. H 1 and H 2, among which, H 1= L × sin( a / 60), H 2= L × sin( b / 60), the actual height of the pad .

[0018] Among them, in step d), the crystal with the end face crystal orientation corrected is placed on a horizontal table, the minimum diameter position of the crystal outer ring is marked on the upward end face, and the target diameter circle is drawn within the marked position range. Then the crystal is mounted on an external cylindrical grinder, the drawn target diameter circle coincides with the external cylindrical grinder top rod and concentric, the grinding fluid is turned on, and the outer circle of the crystal is rough-machined using a coarse grinding wheel. When it is close to the target diameter of 1-2 mm, the fine grinding wheel is replaced to fine-machine the outer circle of the crystal.

[0019] Preferably, if the process of the present invention is used to process lithium tantalate or lithium niobate crystals, in step c), the rough grinding wheel mesh number is #150-200, and the grinding rate is 5-10um / min; the fine grinding wheel mesh number is #400-500, and the grinding rate is 1-2um / min; in step d), the rough grinding wheel mesh number of the cylindrical grinder is #150-200, and the grinding rate is 0.05-0.06mm / min; the fine grinding wheel mesh number is #400-500, and the grinding rate is 0.01-0.02mm / min, and the roughness of the outer peripheral surface of the crystal is controlled at 0.5-0.8um, which can effectively reduce the chipping and edge defects in the subsequent slicing process.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) In the orientation process of the present invention, different fixtures are used to orient and fix the crystal end face direction A and the crystal end face direction B, and they do not interfere with each other during the process. The crystal orientation deviation can be controlled within 12'. At the same time, the cutting is carried out after orientation, which increases the accuracy of the cut end face;

[0022] (2) The present invention adopts a single-wire cutting process, which can effectively reduce the line marks on the crystal end face and ensure the consistency of the crystal orientation of the end face cutting. At the same time, the special cutting fixture has a simple structure and is easy to achieve high-precision alignment cutting in the single-wire cutting process;

[0023] (3) In the crystal end face orientation correction process of the present invention, a correction is achieved once by calculating the maximum deviation value of the crystal orientation. If the crystal end face direction A and the crystal end face direction B are directional corrected separately, the efficiency is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic diagram of the orientation of the crystal end face direction A;

[0025] Figure 2 It is a schematic diagram of the orientation of the crystal end face direction B;

[0026] Figure 3 This is a schematic diagram of the crystal orientation correction of the crystal end face;

[0027] Figure 4 A schematic diagram of the crystal direction in the crystal end face direction;

[0028] Figure 5 It is a schematic diagram of the crystal direction B in the crystal end face direction;

[0029] Among them, 1-directional x-ray, 2-diffraction point in the direction A of the crystal end face, 3-crystal positive X-plane, 4-horizontal reference line, 5-fixed clamp, 6-diffraction point in the direction B of the crystal end face, 7-lithium tantalate crystal, 8-resin strip, 9-adjusting nut, 10-special clamp for cutting, 11-crystal end face direction A, 12-rectangular side corresponding to the crystal end face direction B, 13-rectangular side corresponding to the crystal end face direction A, 14-crystal direction correction heightening point, 15-crystal end face direction B, 16-diffraction angle in the direction A of the crystal end face, 17 diffraction angle in the direction B of the crystal end face, 18-space coordinate system. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1 is as follows:

[0032] A piezoelectric crystal processing method comprises the following steps:

[0033] a) Orientation: A 4-inch Y38° lithium tantalate crystal was used for the experiment, and the goal was to process it into a Y42° crystal rod. Figure 1 FIG. 1 is a schematic diagram of orientation of the crystal end face direction A. A lithium tantalate crystal 7 is vertically placed on a fixing fixture 5 and placed on an orientation instrument, with the positive X-plane 3 of the crystal facing forward. The orientation instrument emits directional X-rays 1 to the crystal, and at the same time, the crystal is rotated left and right by about 4 degrees. Diffraction occurs at the diffraction point 2 in the crystal end face direction A, and the crystal diffraction angle in the crystal end face direction A11 is found. The diffraction angle 16 in the crystal end face direction A is 33°21′. Figure 4 Schematic diagram of crystal end face direction A. In the spatial coordinate system 18, the crystal end face direction A is the crystal direction angle of the Y axis offset from the Z axis. After finding the crystal end face direction A, use a marker to make a horizontal reference line 4 in the middle of the crystal X plane. Figure 2 FIG. 1 is a schematic diagram of orientation of the crystal end face direction B. After the crystal is removed, it is laid horizontally on the resin strip 8 of the special cutting fixture 10 and placed on the orientation instrument, with the positive X face of the crystal facing upward and the head facing right or left. An adjusting nut 9 is provided in the special cutting fixture. By adjusting the nut, the crystal tilt angle can be adjusted. Diffraction occurs at the diffraction point 6 in the crystal end face direction B, thereby finding the crystal X face diffraction angle of 17°25′. Since the X face and the crystal end face direction B are in a vertical relationship, when the horizontal crystal direction of the crystal X face is found, the vertical direction is the crystal end face direction B15. In the spatial coordinate system 18, the crystal end face direction B is the X-axis direction on the cutting target end face. The crystal end face direction B diffraction angle 17 is 24°17′. See FIG. Figure 5 The crystal end face direction B is shown in the figure; then glue is used to fix the crystal, resin strip and fixture at this angle; after solidification, the whole is moved to the single-wire cutting machine for head and tail cutting;

[0034] b) Cutting the head and tail: After the crystal is oriented, place the crystal on the single-wire cutting machine, adjust the position of the diamond wire, use 0.12mm diamond wire to cut, align with the horizontal reference line made during orientation, and then translate the special cutting fixture to align the cutting line with the minimum diameter point at the end of the crystal. The feed speed is 1.0mm / min, and the cutting fluid circulation is turned on to cut the head end of the crystal. After the cutting is completed, rotate 180° to cut the tail end of the crystal;

[0035] c) End face grinding: Remove the crystal from the resin strip and place it on a surface grinder to grind the end faces of the cut head and tail with a #200 rough grinding wheel at a feed rate of 8um / min. After the grinding is completed, use a #500 fine grinding wheel to correct the end face crystal orientation at a feed rate of 1um / min. Figure 3The schematic diagram of the crystal end face crystal orientation correction is as follows: first, use an orientation instrument to measure the crystal end face direction A and crystal end face direction B of one end face of the crystal, and record them as a and b , the diameter of the crystal end face is recorded as L , draw two straight lines on the end face in the direction of the crystal end face A and the direction of the crystal end face B, the two straight lines pass through the center of the end face, and draw a rectangle with the center point as an angle and the two straight lines as sides. The lengths of the rectangular side 13 corresponding to the crystal end face direction A and the rectangular side 12 corresponding to the crystal end face direction B are required to be proportional to the crystal direction deviation values ​​of the crystal end face direction A and the crystal end face direction B, respectively. Connect the diagonal line of the rectangle corresponding to the center point, and extend the intersection of the diagonal line and the edge of the end face to be the crystal direction correction padding point 14. The padding height required for the crystal direction deviation corresponding to the crystal end face direction A and the crystal end face direction B is obtained through geometric conversion. H 1 and H 2, among which, H 1= L × sin( a / 60), H 2= L × sin( b / 60), the actual height of the pad , after raising the height to a certain level at the raising point and placing it on a surface grinder for crystal orientation correction, the target crystal orientation can be achieved;

[0036] d) External cylindrical grinding: Place the crystal with the corrected end face on a horizontal table, mark the minimum diameter position of the crystal outer ring on the upward end face, draw the target diameter circle within the marked position range, and then install the crystal on the external cylindrical grinder. The drawn target circle coincides with the external cylindrical grinder top rod, turn on the grinding fluid, and use the #150 coarse grinding wheel to rough-process the outer circle of the crystal. The rough grinding feed rate is 0.05mm / min. When it is close to the target diameter of 1-2mm, replace the #500 fine grinding wheel for fine processing of the crystal outer circle. The fine grinding feed rate is 0.01mm / min. The roughness of the outer peripheral surface of the crystal is controlled at 0.5-0.8um, which can effectively reduce the chipping and edge bursting in the subsequent slicing process.

[0037] The lithium tantalate crystal rod produced in this embodiment has a smooth appearance without scratches or cracks, a crystal rod cylindricity of less than 0.1 mm, a straightness of ≤0.04 mm, a roundness of ≤0.1 mm / 100 mm, and a crystal orientation deviation of the crystal end face direction A and the crystal end face direction B within 6′.

[0038] In order to highlight the beneficial effects of the present invention, the following comparative example experiments were also carried out.

[0039] Comparative Example 1 is as follows:

[0040] A piezoelectric crystal processing method comprises the following steps:

[0041] a) Orientation: Place the lithium tantalate crystal vertically on the fixture, place it on the orienter, rotate the crystal rod, find the diffraction angle of the target crystal direction A of the crystal end face, turn the fixture 90 degrees, find the crystal direction of the crystal end face direction B, and fix the crystal and the fixture;

[0042] b) Cutting the head and tail: After the crystal is oriented, place the crystal on the single-wire cutting machine, adjust the position of the diamond wire, use 0.12mm diamond wire for cutting, and then translate the special cutting fixture to align the cutting line with the minimum diameter point at the end of the crystal. The feed speed is 1.0mm / min, and the cutting fluid circulation is turned on to cut the head end of the crystal. After the cutting is completed, rotate 180° to cut the tail end of the crystal;

[0043] c) End surface grinding: same as in Example 1;

[0044] d) External cylindrical grinding: same as in Example 1.

[0045] The lithium tantalate crystal rod produced in Comparative Example 1 had no abnormalities in the crystal rod, but during the end face crystal orientation correction process, the end face was ground off by 3 mm, which was mainly caused by large crystal orientation deviation during the orientation process and excessive correction.

[0046] Comparative Example 2 is as follows:

[0047] A piezoelectric crystal processing method comprises the following steps:

[0048] a) Orientation: same as in Example 1;

[0049] b) Cutting the head and tail: Use an internal circle cutting machine to cut the head and tail;

[0050] c) End surface grinding: same as in Example 1;

[0051] d) External cylindrical grinding: same as in Example 1.

[0052] The lithium tantalate crystal rods produced in Example 2 have no abnormalities. Although the efficiency of a single station of the inner circle cutting machine is higher than that of a single line cutting machine, the inner circle cutting machine has high requirements for manual operation in processes such as tool replacement, fixture clamping, and tool alignment, and the process is slow. In addition, two cuts are required to cut one surface (the first cut is for orientation and adjustment of the cutting direction, and the second cut is for accurate cutting). One operator can only operate one station. Compared with one person operating multiple stations on a single line cutting machine, the labor intensity and difficulty are high, and the efficiency is low.

[0053] Comparative Example 3 is as follows:

[0054] A piezoelectric crystal processing method comprises the following steps:

[0055] a) Orientation: same as in Example 1;

[0056] b) Cutting the head and tail: same as in Example 1;

[0057] c) Surface grinding: remove the crystal from the resin strip, place it on a surface grinder, and grind the two end faces of the cut head and tail with a rough grinding wheel. After grinding, remove the crystal and place it on a 7BD orientation tester to measure the crystal direction A of the crystal end face. After calculating the deviation, reinstall it on the surface grinder to correct the crystal direction. After correction, repeat the above steps to correct the crystal direction B of the crystal end face. The grinding parameters are the same as those in Example 1.

[0058] d) External cylindrical grinding: same as in Example 1.

[0059] The lithium tantalate crystal rod produced in Example 3 had no abnormalities, but during the end face crystal orientation correction process, two corrections were performed, and the operation time took 30 minutes longer. In addition, the crystal orientation deviation after correction was unstable and required repeated correction. It was judged that crystal orientation 1 and crystal orientation 2 were corrected separately, and interference occurred during the correction process.

[0060] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A piezoelectric crystal processing method, characterized in that: The following steps are involved: a) Orientation: The processed crystal is a Y-axis-biased Z-axis crystal, and the reference side is the X-axis. The crystal is placed vertically on a fixed fixture and placed on an orientator, with the positive X-face of the crystal facing forward. The crystal direction of the crystal end face direction A is found, and then a horizontal reference line is marked in the middle of the crystal X-face. After removing the crystal, it is laid horizontally on the resin strip of the special cutting fixture and placed on the orientator, with the positive X-face of the crystal facing upward. The special cutting fixture is equipped with an azimuth adjustment component that can adjust the crystal tilt angle to find the crystal X-face crystal direction. The vertical direction is the crystal direction of the crystal end face direction B; then the crystal, resin strip and special cutting fixture are fixed at this angle and moved as a whole to the single-wire cutting machine for head-to-tail cutting; b) Cutting the head and tail: adjust the position of the cutting line to align it with the horizontal reference line, then translate the special cutting fixture to align the cutting line with the minimum diameter point at the end of the crystal, and cut the head and tail of the crystal respectively; c) End grinding: Remove the crystal from the resin strip, grind the end faces of the crystal head and tail, and then correct the end face crystal orientation. The correction method is: first use an orientation instrument to measure the crystal end face direction A and crystal end face direction B of one end face of the crystal, and record them as a and b , draw two straight lines on the end face representing the crystal end face direction A and the crystal end face direction B. The two straight lines pass through the center of the end face. Draw a rectangle with the center point as an angle and the two straight lines as sides. The lengths of the two rectangular sides are required to be proportional to the crystal direction deviation values ​​of the crystal end face direction A and the crystal end face direction B, respectively. Connect the diagonal lines of the rectangles corresponding to the center points, and extend the intersection of the diagonal lines and the edge of the end face to be the crystal direction correction padding point. The diameter of the crystal end face is recorded as L , through the geometric relationship between the crystal end face diameter and the rectangular side, calculate the required pad height for the crystal end face direction A and the crystal end face direction B corresponding to the crystal orientation deviation H 1 and H 2, among which, H 1= L × sin( a / 60), H 2= L × sin( b / 60), the actual height of the pad , after raising the height to a certain level at the raised point, place it on a surface grinder for crystal orientation correction; d) External cylindrical grinding: After the crystal end face crystal orientation is corrected, the outer circle of the crystal is ground according to the target diameter to obtain a crystal rod.

2. The processing method according to claim 1, characterized in that: The processed crystal is lithium tantalate, lithium niobate, quartz, barium titanate or gallium arsenide.

3. The processing method according to claim 1, characterized in that: In the step a), the orientation adjustment component in the special cutting fixture is an angle meter or an adjustment nut.

4. The processing method according to claim 1, characterized in that: In the step b), when cutting the head and tail of the crystal, a diamond wire single wire cutting machine is used for cutting.

5. The processing method according to claim 1, characterized in that: In the step c), the head and tail end faces of the crystal are firstly ground flat using a coarse grinding wheel, and then the end face crystal orientation is corrected using a fine grinding wheel.

6. The processing method according to claim 1, characterized in that: In the step d), the crystal with the corrected end face crystal orientation is placed on a horizontal table, the position of the minimum diameter of the outer ring of the crystal is marked on the upward end face, a target diameter circle is drawn within the marked position range, and then the crystal is mounted on an external cylindrical grinder, the drawn target diameter circle coincides and is concentric with the external cylindrical grinder top rod, the grinding fluid is turned on, and the outer circle of the crystal is rough-machined using a coarse grinding wheel. When it is close to the target diameter of 1-2 mm, the fine grinding wheel is replaced to fine-machine the outer circle of the crystal.

7. The processing method according to any one of claims 1 to 6, characterized in that: When the processed crystal is lithium tantalate or lithium niobate crystal, in the step c), the rough grinding wheel has a mesh number of #150-200, a grinding rate of 5-10um / min, and the fine grinding wheel has a mesh number of #400-500, a grinding rate of 1-2um / min.

8. The processing method according to any one of claims 1 to 6, characterized in that: When the processed crystal is lithium tantalate or lithium niobate crystal, in the step d), the rough grinding wheel of the cylindrical grinder has a mesh number of #150-200 and a grinding rate of 0.05-0.06 mm / min; the fine grinding wheel has a mesh number of #400-500 and a grinding rate of 0.01-0.02 mm / min.