A method for extracting keratin
By combining degreasing and enzymatic dissolution technology, combined with the oxidative dissolution step, the problem of difficult removal of harmful substances and high impurity content in the keratin extraction process in the existing technology is solved, and efficient and pure keratin extraction is achieved, which is suitable for the field of cosmetics.
Patent Information
- Application Number
- CN202411056514.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-08-02
AI Technical Summary
Existing technology cannot meet the purity and efficiency requirements of the cosmetics field when extracting keratin. The extraction process often contains harmful substances and has high impurity content, resulting in a low extraction rate.
Using a method that combines degreasing and enzyme dissolution, the ratio of surfactant, hydrochloric acid and adsorbent is adjusted, combined with the oxidation and dissolution step, using immobilized protease and saturated calcium hydroxide solution, and freeze-drying to obtain high purity angle. protein.
The extraction rate and purity of keratin are improved, and the generation of impurities is reduced. The obtained keratin is suitable for use in cosmetics, has a stable structure and high safety, and is suitable as a wetting agent and sunscreen repair ingredient.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of keratin extraction, and in particular to a method for extracting keratin. Background Art
[0002] Keratin is an important component of the keratin of birds, mammals and reptiles. Horns, nails, feathers, hair, etc. all contain keratin. Keratin is abundant and low in cost. About 7 million tons of it are discarded every year in the world, which not only brings huge pollution to the environment, but also causes waste of resources.
[0003] Keratin itself is non-toxic and harmless, has good biocompatibility, is degradable and renewable, and is an environmentally friendly resource. Its effective utilization is in line with the concept of circular economy.
[0004] Keratin recovered by existing technologies is mostly used to make textile fibers. The extracted keratin has a large molecular weight, and harmful substances added during the extraction process are difficult to remove. There are few applications of keratin in the cosmetics field. At the same time, the general keratin extraction method cannot meet the requirements of the cosmetics field due to the high content of harmful substances, while the harmless extraction method has a low extraction rate and a high impurity content. Summary of the invention
[0005] The present application aims to overcome at least one of the defects of the prior art and provide a method for extracting keratin. By combining a specific degreasing method with enzyme dissolution and oxidative dissolution, the keratin extraction rate can be improved while reducing the generation of impurities. No harmful substances are used in the extraction process, and the prepared keratin is suitable for use in the cosmetics field.
[0006] In a first aspect, the present invention provides a method for extracting keratin, which is achieved by the following technical solutions:
[0007] A method for extracting keratin, comprising the following steps:
[0008] (1) After washing the animal hair, cut it into fiber segments, add a degreasing agent to pre-treat it at a temperature of 60-80°C, and filter it to obtain degreased hair;
[0009] (2) adding the degreased hair to a saturated calcium hydroxide solution, treating for 2 hours, adding protease to dissolve the hair, and centrifuging for the first time to obtain a first solution and hair residue;
[0010] (3) adding the hair residue to an oxidizing agent, oxidizing and dissolving the hair residue, and centrifuging the hair residue for a second time to obtain a second solution;
[0011] (4) mixing the first dissolving solution and the second dissolving solution to precipitate, and then freeze-drying the precipitate to obtain keratin;
[0012] Wherein, the degreasing agent comprises a surfactant, hydrochloric acid and an adsorbent;
[0013] The amounts of the surfactant, the hydrochloric acid and the adsorbent are in a weight ratio of 1:(5-15):(0.5-2);
[0014] The raw materials for preparing the adsorbent include volcanic mud, sodium metaaluminate and coconut shell activated carbon in a weight ratio of 1:(2-4):(0.5-2);
[0015] The surfactant is selected from at least one of a plant surfactant and an amino acid surfactant;
[0016] The protease is prepared by embedding and immobilization;
[0017] The preparation method of the protease comprises the following steps: mixing magnesium sulfate and beta-cyclodextrin in a weight ratio of 1:(1-2), adding to an acidic buffer solution, adding protease powder, and then adding glutaraldehyde solution, mixing evenly, reacting for 4 hours, adding dropwise to a CaCl2 solution, fixing at 30-80°C for 0.5-7.5 hours, filtering; after replacing a new CaCl2 solution, standing at 0-6°C for hardening for 1-3 hours; then washing with a NaCl solution, and drying.
[0018] A method for extracting keratin according to an embodiment of the present application has at least the following beneficial effects:
[0019] The method of the present application first uses a degreasing agent to treat the hair fiber, which can make the hair fiber swell. There is a lipid layer on the fiber surface of animal hair, and the lipid layer is formed by covalent bonding of lipids and proteins. The use of a degreasing agent can destroy the bonding and remove the hydrophobic lipid substances on the surface of animal hair, thereby improving the hydrophilicity and chemical reactivity of the fiber surface, which is beneficial for the alkali solution and protease in the subsequent steps to directly act on keratin, thereby improving the extraction efficiency of keratin; using an alkali method for treatment, on the one hand, can destroy the disulfide bonds in the molecular structure of keratin, which is beneficial to the hydrolysis of keratin, and on the other hand, can further loosen the molecular structure of keratin, improve the extraction rate of protease extraction, and reduce the amount of protease added.
[0020] The dosage ratio of the surfactant, hydrochloric acid and adsorbent in the degreasing agent raw material of the present application can adjust the balance between the degreasing and oil removal effect and the impurity removal effect of the degreasing agent, enhance the degreasing and oil removal ability of the degreasing agent, and thus enhance the keratin extraction effect. If the dosage of the adsorbent is too little, the impurity removal enhancement effect is not obvious. If the dosage of the adsorbent is too much, the effect of removing the keratin lipid layer will be affected. If the dosage of the hydrochloric acid is too little, it will also affect the effect of removing the keratin lipid layer. If the dosage of the hydrochloric acid is too much, it will cause the loss of part of the keratin, affecting the yield of the keratin.
[0021] The volcanic mud of the present application is combined with sodium aluminate and coconut shell activated carbon to fully utilize the electrostatic attraction effect of volcanic mud, the cohesion effect of sodium aluminate, and the porous adsorption effect of coconut shell activated carbon to effectively absorb odors, grease, and stains on the surface of animal hair, thereby enhancing the deep cleaning effect of the degreasing agent on the hair.
[0022] The present application adds a saturated calcium hydroxide solution for treatment, so that the residual acid reacts with the saturated calcium hydroxide solution, neutralizes the residual acid in the pretreatment process, avoids the residual acid from damaging the structure of the protease, and ensures the efficient enzymatic hydrolysis process; utilizes the low solubility of calcium hydroxide to control the alkalinity of the enzymatic hydrolysis solution and avoid a large excess of residual alkali; after the keratin is hydrolyzed, the small amount of residual alkali solution can react with carbon dioxide in the air to generate calcium carbonate; calcium carbonate is insoluble in water, and the generated calcium carbonate has a small particle size and will be wrapped on the surface of the protein structure, preventing the continuous hydrolysis of keratin and maintaining the stability of the keratin structure.
[0023] The present application encapsulates the protease in a gel polymer grid or a polymer semipermeable membrane. This method can effectively protect the enzyme molecules from the influence of the external environment while maintaining its catalytic activity. Immobilized protease can significantly improve its stability in different environments (such as temperature, pH value, organic solvent, etc.); compared with free enzymes, immobilized protease is easier to separate and recover from the reaction system, thereby achieving multiple reuses, which not only reduces production costs, but also reduces environmental pollution; by optimizing the immobilization conditions and methods, the distribution and conformation of the protease on the carrier can be adjusted, thereby further improving its catalytic efficiency.
[0024] The oxidation method for extracting keratin in the present application is to oxidize the disulfide bonds of keratin in the remaining animal hair residues into water-soluble sulfonic acid groups, further extract keratin, and increase the keratin yield.
[0025] According to some embodiments of the present application, the average length of the fiber segment in step (1) is 1 cm-1.5 cm.
[0026] According to some embodiments of the present application, the amount of the degreasing agent added in step (1) is 30%-50% of the weight of the animal hair.
[0027] According to some embodiments of the present application, the pretreatment time in step (1) is 3-5 hours.
[0028] According to some embodiments of the present application, the method for preparing the adsorbent comprises the following steps:
[0029] A1. Mix volcanic mud, sodium aluminate and coconut shell activated carbon according to the weight ratio, and then dry and grind to obtain a powder;
[0030] A2. The powder prepared in step A1 was calcined at 110-150 ℃ for 30-40min;
[0031] A3. Then heat to 650-700℃ and calcine for 20-30min;
[0032] A4. After cooling and magnetization, grinding to a size of 100 mesh or more is performed to obtain the adsorbent.
[0033] Step A1: firstly mix the volcanic mud, sodium aluminate and coconut shell activated carbon, so that the sodium aluminate and coconut shell activated carbon can be fully mixed, and it is not easy to separate in the subsequent granulation process, so that the magnetism of the sodium aluminate is evenly distributed in the coconut shell activated carbon, thereby making the adsorption performance of the prepared adsorbent more stable.
[0034] The preparation method of the adsorbent includes a two-step roasting process. The first stage of the two-stage roasting is pre-activation, and the second stage of roasting is activation. The two-stage roasting gradually destroys the lattice, making it easier to form an amorphous active material, thereby improving the adsorption effect on impurities.
[0035] Grinding to a size of 100 mesh or more can make the adsorbent particles smaller, enhance the dispersibility of the adsorbent, and facilitate rapid and uniform mixing with other components in the subsequent preparation of the degreasing agent. It also increases the fineness of the prepared degreasing agent when used and is not easy to damage animal hair.
[0036] Furthermore, the step A3 further includes adding a pore-forming agent and mixing before heating. Adding a pore-forming agent can increase the porosity of the granulation.
[0037] Furthermore, the pore forming agent includes carboxymethyl cellulose and polyvinyl alcohol. Polyvinyl alcohol has good bonding strength with the powder, is more likely to improve dispersibility, and forms micropores after sintering to improve porosity. Carboxymethyl cellulose further improves porosity to avoid affecting adsorption effect due to blockage of adsorbent pores.
[0038] According to some embodiments of the present application, the amount of the saturated calcium hydroxide solution added in step (2) is 20%-30% of the weight of the degreased hair.
[0039] According to some embodiments of the present application, the amount of the protease added in step (2) is 1%-5% of the weight of the degreased hair.
[0040] Furthermore, the added amount of the protease is 2%-3% of the weight of the degreased hair, for example, the added amount of the protease is 3% of the weight of the degreased hair.
[0041] According to some embodiments of the present application, the time for dissolving the protease in step (2) is 2-3 hours.
[0042] According to some embodiments of the present application, the centrifugal speed of the first centrifugal separation in step (2) is 4000-6000 r / min.
[0043] Furthermore, the centrifugation time of the first centrifugation in step (2) is 20 min-30 min.
[0044] According to some embodiments of the present application, the amount of the oxidant added in step (3) is 10%-20% of the weight of the hair residue.
[0045] According to some embodiments of the present application, the oxidant in step (3) includes at least one of hydrogen peroxide, performic acid, peracetic acid, sodium hypochlorite, and potassium persulfate.
[0046] According to some embodiments of the present application, the time for oxidative dissolution in step (3) is 1-2 hours.
[0047] According to some embodiments of the present application, the centrifugal speed of the second centrifugal separation in step (3) is 6000-8000 r / min.
[0048] Furthermore, the centrifugation time of the second centrifugation in step (3) is 40 min-60 min.
[0049] According to some embodiments of the present application, the freeze-drying process in step (4) comprises the following steps:
[0050] S1. Fill the precipitate into a sample bottle and cover it with a rubber stopper to allow air to circulate freely inside and outside the bottle. Place the sample bottle in a low-temperature environment of -50°C for 4 hours;
[0051] S2. Primary drying: The frozen sample bottle is placed under a vacuum of 10-30 Pa, the temperature is raised to -20°C, and the drying is continued for 18-24 hours, and the ice crystals in the sample bottle are sublimated into water vapor and discharged;
[0052] S3. Secondary drying: After the primary drying is completed, the partition temperature is raised to 30°C and the drying is continued for 6-12h;
[0053] S4. After drying, fill the sample bottle with nitrogen and tighten the rubber stopper; lower the ambient temperature to room temperature or below, and cover the rubber stopper with an aluminum cap and clamp it in place.
[0054] The purpose of freezing is to make the water in the protein solution exist in the form of ice crystals to prepare for subsequent drying; the purpose of primary drying is to remove most of the water in the protein through sublimation drying while maintaining its original structure and activity; the purpose of secondary drying is to remove the residual bound water in the sample through desorption drying; the purpose of sealed storage is to prevent keratin from moisture, oxidation or contamination during storage.
[0055] Furthermore, the protective gas is selected from one of nitrogen, helium, neon and argon.
[0056] According to some embodiments of the present application, the precipitation method in step (4) is: placing the collected keratin solution in a 3500-7000Da dialysis bag, and placing it in a container filled with pure water for dialysis purification and desalination, wherein the volume ratio of the keratin solution to the volume of pure water is 1:(50-100), the water change interval is 2-12h, and after changing the water 5-10 times, the retentate in the dialysis bag is recovered.
[0057] In a second aspect, an embodiment of the present application provides keratin obtained by using the above-mentioned method for extracting keratin.
[0058] The keratin according to the embodiment of the present application has at least the following beneficial effects:
[0059] The keratin obtained in the present application is safe and pollution-free, has a stable structure, strong water absorption, is easy to store and transport, has a small molecular weight, and is suitable for use in making cosmetics.
[0060] In a third aspect, the embodiments of the present application provide the application of the above keratin in cosmetics. The keratin of the present application is used in the preparation of cosmetics and can be used as a moisturizer for cosmetics. The molecular structure of keratin can lock in moisture, thereby keeping the skin moisturized and full of vitality. At the same time, keratin can accelerate the regeneration of damaged skin tissues, has sun protection and repair functions, and keratin is a natural ingredient with high safety and low irritation to the skin. DETAILED DESCRIPTION
[0061] To make the purpose, technical solution and advantages of the present application clearer, the following will be further described in detail in conjunction with specific embodiments. The embodiments described here are only part of the embodiments of the present application and cannot be understood as limiting the scope of protection of the present application.
[0062] Protease Preparation Example 1
[0063] Preparation of protease: Mix magnesium sulfate and β-cyclodextrin in a weight ratio of 1:2, add to an acidic buffer solution, add protease powder, then add glutaraldehyde solution, mix well, react for 4 hours, add dropwise to a CaCl2 solution, fix at 80°C for 5 hours, filter; after replacing a new CaCl2 solution, let it stand at 4°C for 1 hour to harden; then wash with NaCl solution and dry.
[0064] Protease Preparation Example 2
[0065] Preparation of protease: Mix magnesium sulfate and β-cyclodextrin in a weight ratio of 1:1, add to an acidic buffer solution, add protease powder, then add glutaraldehyde solution, mix well, react for 4 hours, add dropwise to a CaCl2 solution, fix at 30°C for 7.5 hours, and filter; after replacing a new CaCl2 solution, let it stand at 0°C for 3 hours to harden; then wash with NaCl solution and dry.
[0066] Degreasing agent preparation example 1
[0067] Preparation of degreasing agent: mix surfactant, hydrochloric acid and adsorbent in a weight ratio of 1:10:1.5;
[0068] Wherein, the preparation of adsorbent:
[0069] A1. Mix 10 parts by weight of volcanic mud, 20 parts of sodium aluminate powder and 5 parts of coconut shell activated carbon powder, and then dry and grind to obtain a powder;
[0070] A2. The powder prepared in step A1 was calcined at 110 ° C for 30 min;
[0071] A3. Add 2 parts of carboxymethyl cellulose and 2 parts of polyvinyl alcohol by weight, and then heat to 700 ℃ and calcine for 20min;
[0072] A4. After cooling, grinding to 100 mesh to obtain an adsorbent;
[0073] The surfactants are prepared by mixing disodium cocoyl glutamate and sodium lauroyl methyl alanine in a weight ratio of 1:1.
[0074] Degreasing agent comparative example 1
[0075] Preparation of degreasing agent: Mix surfactant and hydrochloric acid in a weight ratio of 1:10;
[0076] Among them, the surfactants disodium cocoyl glutamate and sodium lauroyl methyl alanine are mixed in a weight ratio of 1:1. Example 1
[0077] Keratin extraction:
[0078] (1) Wash the animal hair and cut it into fiber segments with an average length of 1.5 cm. Add the degreasing agent prepared in Preparation Example 1 to pretreat the hair at 70° C. for 4 h. The amount of the degreasing agent added is 40% of the weight of the animal hair. Filter the hair to obtain degreased hair.
[0079] (2) adding the defatted animal hair to a saturated calcium hydroxide solution, wherein the amount of the saturated calcium hydroxide solution added is 25% of the weight of the defatted hair. After treating for 2 hours, adding the protease prepared in Protease Preparation Example 1 to dissolve for 3 hours, wherein the amount of the protease added is 3% of the weight of the defatted hair. Centrifuging for the first time at a speed of 5000 r / min for 25 minutes to obtain a first dissolved solution and hair residues.
[0080] (3) adding the hair residue to a 25% by mass hydrogen peroxide solution, where the amount of hydrogen peroxide solution added is 15% of the weight of the hair residue, oxidatively dissolving for 2 h, and centrifuging for a second time at a speed of 7000 r / min for 50 min to obtain a second dissolved solution;
[0081] (4) mixing the first dissolving solution and the second dissolving solution to precipitate, and then freeze-drying the precipitate to obtain keratin;
[0082] Wherein, freeze drying process comprises the following steps:
[0083] S1. Fill the precipitate into a sample bottle and cover it with a rubber stopper to allow air to circulate freely inside and outside the bottle. Place the sample bottle in a low-temperature environment of -50°C for 4 hours;
[0084] S2. Primary drying: The frozen sample bottle is placed under a vacuum of 10-30 Pa, the temperature is raised to -20°C, and the drying is continued for 20 hours, and the ice crystals in the sample bottle are sublimated into water vapor and discharged;
[0085] S3. Secondary drying: After the primary drying is completed, the partition temperature is raised to 30 ° C and continued to dry for 8h;
[0086] S4. After drying, fill the sample bottle with nitrogen and tighten the rubber stopper; lower the ambient temperature to room temperature or below, and cover the rubber stopper with an aluminum cap and clamp it;
[0087] The precipitation method is as follows: the collected keratin solution is placed in a 3500-7000Da dialysis bag, and then placed in a container filled with pure water for dialysis purification and desalination, wherein the volume ratio of the keratin solution to the volume of pure water is 1:80, the water change interval is 8 hours, and after changing the water 8 times, the retentate in the dialysis bag is recovered. Example 2
[0088] Keratin extraction:
[0089] (1) Wash the animal hair, cut it into fiber segments with an average length of 1 cm, add the degreasing agent prepared in Preparation Example 1, and pretreat it at 80° C. for 3 h. The amount of the degreasing agent added is 50% of the weight of the animal hair. Filter and obtain degreased hair.
[0090] (2) adding the defatted animal hair to a saturated calcium hydroxide solution, wherein the amount of the saturated calcium hydroxide solution added is 30% of the weight of the defatted hair. After treating for 2 hours, adding the protease prepared in Protease Preparation Example 1 to dissolve for 2 hours, wherein the amount of the protease added is 5% of the weight of the defatted hair. Centrifuging for the first time at a speed of 6000 r / min for 20 minutes to obtain a first dissolved solution and hair residues.
[0091] (3) adding the hair residue to a 25% sodium hypochlorite solution, wherein the amount of the sodium hypochlorite solution added is 20% of the weight of the hair residue, oxidizing and dissolving for 1 hour, and centrifuging for a second time at a speed of 8000 r / min for 40 minutes to obtain a second solution;
[0092] (4) mixing the first dissolving solution and the second dissolving solution to precipitate, and then freeze-drying the precipitate to obtain keratin;
[0093] Wherein, freeze drying process comprises the following steps:
[0094] S1. Fill the precipitate into a sample bottle and cover it with a rubber stopper to allow air to circulate freely inside and outside the bottle. Place the sample bottle in a low-temperature environment of -50°C for 4 hours;
[0095] S2. Primary drying: The frozen sample bottle is placed under a vacuum of 10-30 Pa, the temperature is raised to -20°C, and the drying is continued for 24 hours to sublimate the ice crystals in the sample bottle into water vapor and discharge it;
[0096] S3. Secondary drying: After the primary drying is completed, the partition temperature is raised to 30 ° C and continued to dry for 6h;
[0097] S4. After drying, fill the sample bottle with nitrogen and tighten the rubber stopper; lower the ambient temperature to room temperature or below, and cover the rubber stopper with an aluminum cap and clamp it;
[0098] The precipitation method is as follows: the collected keratin solution is placed in a 3500-7000Da dialysis bag, and then placed in a container filled with pure water for dialysis purification and desalination, wherein the volume ratio of the keratin solution to the volume of pure water is 1:80, the water change interval is 8 hours, and after changing the water 8 times, the retentate in the dialysis bag is recovered. Example 3
[0099] Keratin extraction:
[0100] (1) Wash the animal hair and cut it into fiber segments with an average length of 1.5 cm. Add the degreasing agent prepared in Preparation Example 1 to pretreat the hair at 60° C. for 5 h. The amount of the degreasing agent added is 30% of the weight of the animal hair. Filter the hair to obtain degreased hair.
[0101] (2) adding the defatted animal hair to a saturated calcium hydroxide solution, wherein the amount of the saturated calcium hydroxide solution added is 20% of the weight of the defatted hair. After treating for 2 hours, adding the protease prepared in Protease Preparation Example 1 to dissolve for 3 hours, wherein the amount of the protease added is 1% of the weight of the defatted hair. Centrifuging for the first time at a speed of 4000 r / min for 30 minutes to obtain a first dissolving solution and hair residues.
[0102] (3) adding the hair residue to a 25% by mass peroxyformic acid solution, wherein the amount of the peroxyformic acid solution added is 10% of the weight of the hair residue, oxidatively dissolving for 2 h, and centrifuging for a second time at a speed of 6000 r / min for 60 min to obtain a second dissolved solution;
[0103] (4) mixing the first dissolving solution and the second dissolving solution to precipitate, and then freeze-drying the precipitate to obtain keratin;
[0104] Wherein, freeze drying process comprises the following steps:
[0105] S1. Fill the precipitate into a sample bottle and cover it with a rubber stopper to allow air to circulate freely inside and outside the bottle. Place the sample bottle in a low-temperature environment of -50°C for 4 hours;
[0106] S2. Primary drying: The frozen sample bottle is placed under a vacuum of 10-30 Pa, the temperature is raised to -20°C, and the drying is continued for 18 hours, and the ice crystals in the sample bottle are sublimated into water vapor and discharged;
[0107] S3. Secondary drying: After the primary drying is completed, the partition temperature is raised to 30 ° C and continued to dry for 12h;
[0108] S4. After drying, fill the sample bottle with nitrogen and tighten the rubber stopper; lower the ambient temperature to room temperature or below, and cover the rubber stopper with an aluminum cap and clamp it;
[0109] The precipitation method is as follows: the collected keratin solution is placed in a 3500-7000Da dialysis bag, and then placed in a container filled with pure water for dialysis purification and desalination, wherein the volume ratio of the keratin solution to the volume of pure water is 1:80, the water change interval is 8 hours, and after changing the water 8 times, the retentate in the dialysis bag is recovered.
[0110] Comparative Example 1
[0111] Keratin extraction:
[0112] (1) Wash the animal hair and cut it into fiber segments with an average length of 1.5 cm. Add the degreasing agent prepared in Preparation Example 1 to pretreat the hair at 70° C. for 4 h. The amount of the degreasing agent added is 40% of the weight of the animal hair. Filter the hair to obtain degreased hair.
[0113] (2) adding the defatted animal hair to a saturated calcium hydroxide solution, wherein the amount of the saturated calcium hydroxide solution added is 25% of the weight of the defatted hair; after treating for 2 hours, adding a common protease to dissolve the hair for 3 hours, wherein the amount of the protease added is 3% of the weight of the defatted hair; and performing a first centrifugal separation at a speed of 5000 r / min for 25 minutes to obtain a first dissolving solution and hair residue;
[0114] (3) adding the hair residue to a 25% by mass hydrogen peroxide solution, where the amount of hydrogen peroxide solution added is 15% of the weight of the hair residue, oxidatively dissolving for 2 h, and centrifuging for a second time at a speed of 7000 r / min for 50 min to obtain a second dissolved solution;
[0115] (4) mixing the first dissolving solution and the second dissolving solution to precipitate, and then freeze-drying the precipitate to obtain keratin;
[0116] Wherein, freeze drying process comprises the following steps:
[0117] S1. Fill the precipitate into a sample bottle and cover it with a rubber stopper to allow air to circulate freely inside and outside the bottle. Place the sample bottle in a low-temperature environment of -50°C for 4 hours;
[0118] S2. Primary drying: The frozen sample bottle is placed under a vacuum of 10-30 Pa, the temperature is raised to -20°C, and the drying is continued for 20 hours, and the ice crystals in the sample bottle are sublimated into water vapor and discharged;
[0119] S3. Secondary drying: After the primary drying is completed, the partition temperature is raised to 30 ° C and continued to dry for 8h;
[0120] S4. After drying, fill the sample bottle with nitrogen and tighten the rubber stopper; lower the ambient temperature to room temperature or below, and cover the rubber stopper with an aluminum cap and clamp it;
[0121] The precipitation method is as follows: the collected keratin solution is placed in a 3500-7000Da dialysis bag, and then placed in a container filled with pure water for dialysis purification and desalination, wherein the volume ratio of the keratin solution to the volume of pure water is 1:80, the water change interval is 8 hours, and after changing the water 8 times, the retentate in the dialysis bag is recovered.
[0122] Comparative Example 2
[0123] Keratin extraction:
[0124] (1) After washing the animal hair, cut it into fiber segments with an average length of 1.5 cm, add the degreasing agent prepared in Comparative Example 1 for pretreatment at a temperature of 70° C. for 4 h, and add the degreasing agent in an amount of 40% of the weight of the animal hair. Filter and obtain degreased hair;
[0125] (2) adding the defatted animal hair to a saturated calcium hydroxide solution, wherein the amount of the saturated calcium hydroxide solution added is 25% of the weight of the defatted hair. After treating for 2 hours, adding the protease prepared in Protease Preparation Example 1 to dissolve for 3 hours, wherein the amount of the protease added is 3% of the weight of the defatted hair. Centrifuging for the first time at a speed of 5000 r / min for 25 minutes to obtain a first dissolved solution and hair residues.
[0126] (3) adding the hair residue to a 25% by mass hydrogen peroxide solution, where the amount of hydrogen peroxide solution added is 15% of the weight of the hair residue, oxidatively dissolving for 2 h, and centrifuging for a second time at a speed of 7000 r / min for 50 min to obtain a second dissolved solution;
[0127] (4) mixing the first dissolving solution and the second dissolving solution to precipitate, and then freeze-drying the precipitate to obtain keratin;
[0128] Wherein, freeze drying process comprises the following steps:
[0129] S1. Fill the precipitate into a sample bottle and cover it with a rubber stopper to allow air to circulate freely inside and outside the bottle. Place the sample bottle in a low-temperature environment of -50°C for 4 hours;
[0130] S2. Primary drying: The frozen sample bottle is placed under a vacuum of 10-30 Pa, the temperature is raised to -20°C, and the drying is continued for 20 hours, and the ice crystals in the sample bottle are sublimated into water vapor and discharged;
[0131] S3. Secondary drying: After the primary drying is completed, the partition temperature is raised to 30 ° C and continued to dry for 8h;
[0132] S4. After drying, fill the sample bottle with nitrogen and tighten the rubber stopper; lower the ambient temperature to room temperature or below, and cover the rubber stopper with an aluminum cap and clamp it;
[0133] The precipitation method is as follows: the collected keratin solution is placed in a 3500-7000Da dialysis bag, and then placed in a container filled with pure water for dialysis purification and desalination, wherein the volume ratio of the keratin solution to the volume of pure water is 1:80, the water change interval is 8 hours, and after changing the water 8 times, the retentate in the dialysis bag is recovered.
[0134] Comparative Example 3
[0135] Keratin extraction:
[0136] (1) Wash the animal hair and cut it into fiber segments with an average length of 1.5 cm. Add the degreasing agent prepared in Preparation Example 1 to pretreat the hair at 70° C. for 4 h. The amount of the degreasing agent added is 40% of the weight of the animal hair. Filter the hair to obtain degreased hair.
[0137] (2) adding the defatted animal hair to a saturated calcium hydroxide solution, wherein the amount of the saturated calcium hydroxide solution added is 25% of the weight of the defatted hair. After treating for 2 hours, adding the protease prepared in Protease Preparation Example 1 to dissolve for 3 hours, wherein the amount of the protease added is 3% of the weight of the defatted hair. Centrifuging for the first time at a speed of 5000 r / min for 25 minutes to obtain a first dissolved solution and hair residues.
[0138] (3) precipitating the first dissolving solution, and freeze-drying the precipitate to obtain keratin;
[0139] Wherein, freeze drying process comprises the following steps:
[0140] S1. Fill the precipitate into a sample bottle and cover it with a rubber stopper to allow air to circulate freely inside and outside the bottle. Place the sample bottle in a low-temperature environment of -50°C for 4 hours;
[0141] S2. Primary drying: The frozen sample bottle is placed under a vacuum of 10-30 Pa, the temperature is raised to -20°C, and the drying is continued for 20 hours, and the ice crystals in the sample bottle are sublimated into water vapor and discharged;
[0142] S3. Secondary drying: After the primary drying is completed, the partition temperature is raised to 30 ° C and continued to dry for 8h;
[0143] S4. After drying, fill the sample bottle with nitrogen and tighten the rubber stopper; lower the ambient temperature to room temperature or below, and cover the rubber stopper with an aluminum cap and clamp it;
[0144] The precipitation method is as follows: the collected keratin solution is placed in a 3500-7000Da dialysis bag, and then placed in a container filled with pure water for dialysis purification and desalination, wherein the volume ratio of the keratin solution to the volume of pure water is 1:80, the water change interval is 8 hours, and after changing the water 8 times, the retentate in the dialysis bag is recovered.
[0145] Experimental example
[0146] Keratin was extracted according to the methods of Examples 1-3 and Comparative Examples 1-3, and the extraction rate and the average molecular weight of keratin were measured. The obtained data are shown in Table 1 below:
[0147]
[0148] As can be seen from Table 1, the keratin extraction rate of the extraction methods of Examples 1-3 of the present application is high, and the average molecular weight of the obtained keratin is small, which is suitable for use in cosmetics.
[0149] The protease in the extraction method of Comparative Example 1 was not embedded, and the rest was the same as Example 1. The extraction rate of keratin extracted in Comparative Example 1 was significantly lower than that in Example 1, and the average molecular weight of keratin was also larger than that in Example 1, indicating that the embedding of the protease of the present application is very critical for the extraction of keratin. The embedded protease can not only improve the extraction efficiency, but also make the protein hydrolysis more complete.
[0150] The degreasing agent in the extraction method of Comparative Example 2 does not contain an adsorbent in the preparation raw materials, and the rest is the same as Example 1. The extraction rate of keratin extracted in Comparative Example 2 is significantly lower than that in Example 1, and the average molecular weight of keratin is also larger than that in Example 1, indicating that the addition of an adsorbent to the degreasing agent of the present application can significantly improve the removal effect of the lipid layer on the surface of animal fur, thereby improving the extraction efficiency of keratin and making the hydrolysis of keratin more complete.
[0151] The extraction method of Comparative Example 3 did not undergo oxidative dissolution, and the rest was the same as Example 1. The extraction rate of keratin extracted in Comparative Example 3 was significantly lower than that in Example 1, and the average molecular weight of keratin was also larger than that in Example 1, indicating that oxidative decomposition can further extract keratin from fur residues, thereby increasing the extraction rate of keratin. The oxidant can destroy the disulfide bonds and peptide bonds of keratin, and the average molecular weight of the extracted keratin is also smaller.
[0152] Although the embodiments of the present application have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions or variations may be made to the embodiments without departing from the principles and purpose of the present application, and that the technical solutions after these changes, modifications, substitutions or variations will fall within the scope of protection of the present application.
Claims
1. A method for extracting keratin, characterized in that: The following steps are involved: (1) After washing the animal hair, cut it into fiber segments, add a degreasing agent to pre-treat it at a temperature of 60-80°C, and filter it to obtain degreased hair; (2) adding the degreased hair to a saturated calcium hydroxide solution, treating for 2 hours, adding protease to dissolve the hair, and centrifuging for the first time to obtain a first solution and hair residue; (3) adding the hair residue to an oxidizing agent, oxidizing and dissolving the hair residue, and centrifuging the hair residue for a second time to obtain a second solution; (4) mixing the first dissolving solution and the second dissolving solution to precipitate, and then freeze-drying the precipitate to obtain keratin; Wherein, the degreasing agent in step (1) is composed of a surfactant, hydrochloric acid and an adsorbent; The amount of the surfactant, the hydrochloric acid and the adsorbent is 1:(5-15):(0.5-2) by weight ratio; The raw materials for preparing the adsorbent are composed of volcanic mud, sodium metaaluminate and coconut shell activated carbon in a weight ratio of 1:(2-4):(0.5-2); The surfactant is prepared by mixing disodium cocoyl glutamate and sodium lauroyl methyl alanine in a weight ratio of 1:1; The oxidant in step (3) is selected from a 25% by mass hydrogen peroxide solution, a 25% by mass sodium hypochlorite solution or a 25% by mass peroxyformic acid solution; The protease described in step (2) is prepared by embedding and immobilization; The preparation method of the protease comprises the following steps: mixing magnesium sulfate and beta-cyclodextrin in a weight ratio of 1:(1-2), adding to an acidic buffer solution, adding protease powder, and then adding glutaraldehyde solution, mixing evenly, reacting for 4 hours, adding dropwise to a CaCl2 solution, fixing at 30-80°C for 0.5-7.5 hours, filtering; after replacing a new CaCl2 solution, standing at 0-6°C for hardening for 1-3 hours; then washing with a NaCl solution, and drying.
2. A method for extracting keratin according to claim 1, characterized in that: The average length of the fiber segment in step (1) is 1 cm to 1.5 cm.
3. A method for extracting keratin according to claim 1, characterized in that: The amount of the degreasing agent added in step (1) is 30%-50% of the weight of the animal hair.
4. A method for extracting keratin according to claim 1, characterized in that: In step (2), the amount of the saturated calcium hydroxide solution added is 20%-30% of the weight of the degreased hair, and the amount of the protease added is 1%-5% of the weight of the degreased hair.
5. A method for extracting keratin according to claim 1, characterized in that: The amount of the oxidant added in step (3) is 10%-20% of the weight of the hair residue.
6. A method for extracting keratin according to claim 1, characterized in that: The preparation method of the adsorbent comprises the following steps: A1. Mix volcanic mud, sodium aluminate and coconut shell activated carbon according to the weight ratio, and then dry and grind to obtain a powder; A2. The powder prepared in step A1 was calcined at 110-150 ℃ for 30-40min; A3. Then heat to 650-700℃ and calcine for 20-30min; A4. After cooling and magnetization, grinding to a size of 100 mesh or more is performed to obtain the adsorbent.
7. A method for extracting keratin according to claim 1, characterized in that: The freeze-drying process in step (4) comprises the following steps: S1. Fill the precipitate into a sample bottle and cover it with a rubber stopper to allow air to circulate freely inside and outside the bottle. Place the sample bottle in a low-temperature environment of -50°C for 4 hours; S2. Primary drying: The frozen sample bottle is placed under a vacuum of 10-30 Pa, the temperature is raised to -20°C, and the drying is continued for 18-24 hours, and the ice crystals in the sample bottle are sublimated into water vapor and discharged; S3. Secondary drying: After the primary drying is completed, the partition temperature is raised to 30°C and the drying is continued for 6-12h; S4. After drying, fill the sample bottle with nitrogen and tighten the rubber stopper; lower the ambient temperature to room temperature or below, and cover the rubber stopper with an aluminum cap and clamp it in place.
8. A method for extracting keratin according to claim 1, characterized in that: The precipitation method in step (4) is as follows: placing the collected keratin solution in a 3500-7000Da dialysis bag, and placing it in a container filled with pure water for dialysis purification and desalination, wherein the volume ratio of the keratin solution to the volume of pure water is 1:(50-100), the water change interval is 2-12h, and after changing the water 5-10 times, the retentate in the dialysis bag is recovered.
Citation Information
Patent Citations
Preparation method of sheep horn protein peptide
CN103088095A
Novel extraction method of rabbit hair keratin and application thereof to cosmetics
CN109575119A
Method for extracting keratin and keratin extracted by method
CN116333085A