A kind of polyurethane microwave absorbing porous material and its preparation process

By adding fiber-graphene composite and nickel-loaded aramid fibers to polyurethane materials, and using the reaction of polyacrylic acid and phosphoric acid solutions, the problem of unstable absorption performance of traditional polyurethane absorbing materials is solved, achieving a wider range of Improved wave absorption performance to meet the needs of various engineering applications.

CN118580551BActive Publication Date: 2024-11-15CHANGZHOU RONGXIN COMPOSITE MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410742058.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-11-15
Estimated Expiration
2044-06-11

AI Technical Summary

Technical Problem

Traditional polyurethane absorbing materials have problems such as unstable wave absorption performance, narrow frequency range and low wave absorption peak, which is difficult to meet the needs of various engineering applications.

Method used

Polyurethane is used as the matrix material, fiber-graphene composite is added, and the material is reinforced by the bonding of polyacrylic acid with zinc oxide-graphene composite and nickel-loaded aramid fibers. Wave absorption performance.

Benefits of technology

It significantly improves the wave absorption performance of polyurethane absorbing porous materials, enhances its absorption capacity in different frequency ranges, and meets the needs of a variety of engineering applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004885139430000101
    Figure BDA0004885139430000101
Patent Text Reader

Abstract

The present invention relates to the technical field of porous materials, specifically a polyurethane wave-absorbing porous material and a preparation process thereof. The present invention adopts polyurethane as the matrix material of the wave-absorbing material, and the polyurethane material has good mechanical properties and porosity, and can reduce the reflection of electromagnetic waves on the surface of the material. The present invention adds a fiber-graphene composite to the polyurethane, and uses a cohesive polyacrylic acid to bond the zinc oxide-graphene composite and the aramid fiber loaded with nickel to prepare the fiber-graphene composite. The polyacrylic acid also has a carboxyl group, which can react with the terminal hydroxyl group of the polyether polyol to enhance the dispersibility of the fiber-graphene composite in the matrix, and improve the wave-absorbing performance of the polyurethane wave-absorbing porous material. The present invention also uses pyrrole monomer to load polypyrrole on aramid fiber, and the load of polypyrrole can improve the wave-absorbing ability of aramid fiber. The porous material prepared by the method provided by the present invention has excellent wave-absorbing performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of porous materials, in particular to a polyurethane wave-absorbing porous material and a preparation process thereof. Background Art

[0002] With the continuous development of electronic technology and communication technology, the demand for electromagnetic wave absorbing materials is increasing. Polyurethane materials have attracted much attention in the field of absorbing materials due to their high porosity, easy adjustment, excellent heat resistance and chemical stability. However, traditional polyurethane absorbing materials often have problems such as unstable absorbing performance, narrow frequency range, and low absorption peak. Therefore, a new type of polyurethane absorbing porous material is urgently needed to meet the needs of various engineering applications.

[0003] In order to solve the above problems and improve the wave absorbing performance, the present invention provides a polyurethane wave absorbing porous material and a preparation process thereof. Summary of the invention

[0004] The purpose of the present invention is to provide a polyurethane absorbing porous material and a preparation process thereof to solve the problems raised in the above background technology.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A preparation process of a polyurethane microwave absorbing porous material comprises the following steps:

[0007] Step 1: Take polyacrylic acid and deionized water, stir evenly to obtain a polyacrylic acid solution; add zinc oxide-graphene composite and nickel-loaded aramid fiber, ultrasonically disperse, react for 3-4 hours, filter and dry to obtain a fiber-graphene composite;

[0008] Step 2: Take polyether polyol, dispersant, fiber-graphene composite, disperse them by ultrasonic, add polyisocyanate, stir evenly, foam, and ripen to obtain polyurethane absorbing porous material.

[0009] More optimally, the polyurethane absorbing porous material comprises the following components, by weight: 20-22% of polyether polyol, 4-5% of dispersant, 7-9% of polyisocyanate, and the rest being fiber-graphene composite.

[0010] More optimally, in step 1, the mass ratio of the zinc oxide-graphene composite to the nickel-loaded aramid fiber is (1-2): (3-5).

[0011] More optimally, the preparation method of the zinc oxide-graphene composite is: take zinc oxide, graphene oxide, and deionized water, ultrasonically disperse for 1-2 hours, add hydrazine hydrate solution, heat to 95° C. and stir to react for 2-4 hours, wash and dry to obtain the zinc oxide-graphene composite.

[0012] More optimally, the mass ratio of zinc oxide to graphene oxide is (4-6):0.1.

[0013] More optimally, the preparation method of zinc oxide is: take deionized water, add zinc acetate dihydrate and polyvinyl pyrrolidone, stir evenly, heat to 75-85° C., wash, filter, and obtain zinc oxide.

[0014] More optimally, the preparation method of the nickel-loaded aramid fiber is as follows: take aramid fiber and deionized water, ultrasonically disperse for 3-4 hours to obtain an aramid fiber dispersion; add pyrrole monomer and phosphoric acid solution, stir evenly to obtain a mixed solution; take nickel dichloride hexahydrate and deionized water, stir evenly, add phosphoric acid, sodium dodecylbenzene sulfonate, and the mixed solution, heat to 55-65°C, stir evenly, add ammonia water, adjust the pH value, stir for 1-1.5 hours, add KH-550, heat to 70-75°C, react for 1-1.5 hours, filter and dry to obtain nickel-loaded aramid fiber.

[0015] More optimally, ammonia water is added dropwise to adjust the pH value to 11.

[0016] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0017] (1) The present invention uses polyurethane as the base material of the absorbing material. The polyurethane material has good mechanical properties and good impact resistance. At the same time, the polyurethane material is porous, which can reduce the reflection of electromagnetic waves on the surface of the material. The present invention adds a fiber-graphene composite to the polyurethane to improve the absorbing performance of the polyurethane.

[0018] (2) The present invention uses adhesive polyacrylic acid to bond zinc oxide-graphene composites and nickel-loaded aramid fibers together to prepare fiber-graphene composites. The polyacrylic acid also has carboxyl groups that can react with the terminal hydroxyl groups of polyether polyols to enhance the dispersibility of the fiber-graphene composite in the matrix and improve the absorbing performance of the polyurethane absorbing porous material.

[0019] (3) The present invention first uses pyrrole monomer to load polypyrrole on aramid fiber. The loading of polypyrrole can improve the wave absorption capacity of aramid fiber. The present invention also adds phosphoric acid solution. The addition of phosphoric acid solution can react with polypyrrole and nickel phosphate at the same time, making the polypyrrole particles denser and also making the generated nickel oxide particle size smaller. The present invention uses nickel dichloride hexahydrate as an oxidant to participate in the reaction, and can also generate nickel oxide in an alkaline environment, further enhancing the wave absorption performance. DETAILED DESCRIPTION

[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] There are no special restrictions on the purchase manufacturers and models of all raw materials involved in the present invention, and exemplary examples include: dispersant: can be purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., model: XFZ36; polyether polyol: can be purchased from Hubei Qifei Pharmaceutical Chemical Co., Ltd., model: QF0568; polyisocyanate: can be purchased from Beijing Haibeisi Company; aramid fiber: can be purchased from Shanghai Kefeng Chemical Reagent Co., Ltd., specification: 23tex, length 3-5mm; graphene oxide: model: 763705, can be purchased from Merck.

[0022] Embodiment 1: A process for preparing a polyurethane microwave absorbing porous material, comprising the following steps:

[0023] Step 1: Preparation of nickel-loaded aramid fibers:

[0024] Take 1g of aramid fiber and 200mL of deionized water, and ultrasonically disperse for 3.5h to obtain an aramid fiber dispersion; add 1.2g of pyrrole monomer and 1mL of 0.01M phosphoric acid solution, stir evenly to obtain a mixed solution; take 12g of nickel dichloride hexahydrate and 50mL of deionized water, stir evenly, add 10mL of phosphoric acid, 5g of sodium dodecylbenzene sulfonate, and the mixed solution, heat to 60°C, stir evenly, add ammonia water, adjust the pH value to 11, stir for 1.2h, add 10mL of KH-550, heat to 73°C, react for 1.2h, filter and dry to obtain nickel-loaded aramid fiber;

[0025] Step 2: Preparation of zinc oxide-graphene composite:

[0026] Take 250 mL of deionized water, add 30 mL of zinc acetate dihydrate and 20 mL of polyvinyl pyrrolidone, stir evenly, heat to 80°C, wash and filter to obtain zinc oxide;

[0027] Take 4g zinc oxide, 0.1g graphene oxide, and 50mL deionized water, and ultrasonically disperse them for 1.5h, add 8mL of 40% hydrazine hydrate solution, heat to 95°C and stir to react for 3h, wash and dry to obtain a zinc oxide-graphene composite;

[0028] Step 3: Preparation of fiber-graphene composite:

[0029] Take 3 g of polyacrylic acid and 50 mL of deionized water, stir evenly to obtain a polyacrylic acid solution; add 1.5 g of zinc oxide-graphene composite and 4 g of nickel-loaded aramid fiber, ultrasonically disperse, react for 3.5 h, filter and dry to obtain a fiber-graphene composite;

[0030] The mass ratio of zinc oxide-graphene composite and nickel-loaded aramid fiber is 1.5:4;

[0031] Step 4: Preparation of polyurethane absorbing porous material:

[0032] Taking polyether polyol, dispersant, and fiber-graphene composite, dispersing by ultrasonic, adding polyisocyanate, stirring evenly, foaming, and ripening, to obtain polyurethane absorbing porous material;

[0033] The polyurethane wave-absorbing porous material includes the following components, by weight: 21% of polyether polyol, 4.5% of dispersant, 8% of polyisocyanate, and the rest is fiber-graphene composite.

[0034] Embodiment 2: A process for preparing a polyurethane microwave absorbing porous material, comprising the following steps:

[0035] Step 1: Preparation of nickel-loaded aramid fibers:

[0036] Take 1g of aramid fiber and 200mL of deionized water, and ultrasonically disperse for 3h to obtain an aramid fiber dispersion; add 1.2g of pyrrole monomer and 1mL of 0.01M phosphoric acid solution, stir evenly to obtain a mixed solution; take 12g of nickel dichloride hexahydrate and 50mL of deionized water, stir evenly, add 10mL of phosphoric acid, 5g of sodium dodecylbenzene sulfonate, and the mixed solution, heat to 55°C, stir evenly, add ammonia water dropwise, adjust the pH value to 11, stir for 1.5h, add 10mL of KH-550, heat to 70°C, react for 1.5h, filter and dry to obtain nickel-loaded aramid fiber;

[0037] Step 2: Preparation of zinc oxide-graphene composite:

[0038] Take 250 mL of deionized water, add 30 mL of zinc acetate dihydrate and 20 mL of polyvinyl pyrrolidone, stir evenly, heat to 75°C, wash and filter to obtain zinc oxide;

[0039] Take 4g zinc oxide, 0.1g graphene oxide, and 50mL deionized water, and ultrasonically disperse for 1h, add 8mL of 40% hydrazine hydrate solution, heat to 95°C and stir for 2h, wash and dry to obtain a zinc oxide-graphene composite;

[0040] Step 3: Preparation of fiber-graphene composite:

[0041] Take 3g of polyacrylic acid and 50mL of deionized water, stir evenly to obtain a polyacrylic acid solution; add 1g of zinc oxide-graphene composite and 3g of nickel-loaded aramid fiber, ultrasonically disperse, react for 3h, filter and dry to obtain a fiber-graphene composite;

[0042] The mass ratio of zinc oxide-graphene composite and nickel-loaded aramid fiber is 1:3;

[0043] Step 4: Preparation of polyurethane absorbing porous material:

[0044] Taking polyether polyol, dispersant, and fiber-graphene composite, dispersing by ultrasonic, adding polyisocyanate, stirring evenly, foaming, and ripening, to obtain polyurethane absorbing porous material;

[0045] The polyurethane wave-absorbing porous material comprises the following components, by weight: 20% of polyether polyol, 4% of dispersant, 7% of polyisocyanate, and the rest being a fiber-graphene composite.

[0046] Embodiment 3: A process for preparing a polyurethane absorbing porous material, comprising the following steps:

[0047] Step 1: Preparation of nickel-loaded aramid fibers:

[0048] Take 1g of aramid fiber and 200mL of deionized water, and ultrasonically disperse for 4h to obtain an aramid fiber dispersion; add 1.2g of pyrrole monomer and 1mL of 0.01M phosphoric acid solution, stir evenly to obtain a mixed solution; take 12g of nickel dichloride hexahydrate and 50mL of deionized water, stir evenly, add 10mL of phosphoric acid, 5g of sodium dodecylbenzene sulfonate, and the mixed solution, heat to 65°C, stir evenly, add ammonia water, adjust the pH value to 11, stir for 1h, add 10mL of KH-550, heat to 75°C, react for 1h, filter and dry to obtain nickel-loaded aramid fiber;

[0049] Step 2: Preparation of zinc oxide-graphene composite:

[0050] Take 250 mL of deionized water, add 30 mL of zinc acetate dihydrate and 20 mL of polyvinyl pyrrolidone, stir evenly, heat to 85°C, wash and filter to obtain zinc oxide;

[0051] Take 4g zinc oxide, 0.1g graphene oxide, and 50mL deionized water, ultrasonically disperse for 2h, add 8mL of 40% hydrazine hydrate solution, heat to 95°C and stir for 4h, wash and dry to obtain a zinc oxide-graphene composite;

[0052] Step 3: Preparation of fiber-graphene composite:

[0053] Take 3g of polyacrylic acid and 50mL of deionized water, stir evenly to obtain a polyacrylic acid solution; add 2g of zinc oxide-graphene composite and 5g of nickel-loaded aramid fiber, ultrasonically disperse, react for 4h, filter and dry to obtain a fiber-graphene composite;

[0054] The mass ratio of zinc oxide-graphene composite and nickel-loaded aramid fiber is 2:5;

[0055] Step 4: Preparation of polyurethane absorbing porous material:

[0056] Taking polyether polyol, dispersant, and fiber-graphene composite, dispersing by ultrasonic, adding polyisocyanate, stirring evenly, foaming, and ripening, to obtain polyurethane absorbing porous material;

[0057] The polyurethane wave-absorbing porous material comprises the following components, by weight: 22% of polyether polyol, 5% of dispersant, 9% of polyisocyanate, and the rest being a fiber-graphene composite.

[0058] Comparative Example 1: The zinc oxide-graphene composite and the nickel-loaded aramid fiber are bonded together without using polyacrylic acid, and the rest is the same as Example 1:

[0059] A preparation process of a polyurethane microwave absorbing porous material comprises the following steps:

[0060] Step 1: Preparation of nickel-loaded aramid fibers:

[0061] Take 1g of aramid fiber and 200mL of deionized water, and ultrasonically disperse for 3.5h to obtain an aramid fiber dispersion; add 1.2g of pyrrole monomer and 1mL of 0.01M phosphoric acid solution, stir evenly to obtain a mixed solution; take 12g of nickel dichloride hexahydrate and 50mL of deionized water, stir evenly, add 10mL of phosphoric acid, 5g of sodium dodecylbenzene sulfonate, and the mixed solution, heat to 60°C, stir evenly, add ammonia water, adjust the pH value to 11, stir for 1.2h, add 10mL of KH-550, heat to 73°C, react for 1.2h, filter and dry to obtain nickel-loaded aramid fiber;

[0062] Step 2: Preparation of zinc oxide-graphene composite:

[0063] Take 250 mL of deionized water, add 30 mL of zinc acetate dihydrate and 20 mL of polyvinyl pyrrolidone, stir evenly, heat to 80°C, wash and filter to obtain zinc oxide;

[0064] Take 4g zinc oxide, 0.1g graphene oxide, and 50mL deionized water, and ultrasonically disperse them for 1.5h, add 8mL of 40% hydrazine hydrate solution, heat to 95°C and stir to react for 3h, wash and dry to obtain a zinc oxide-graphene composite;

[0065] Step 3: Preparation of fiber-graphene composite:

[0066] Take 50 mL of deionized water, add 1.5 g of zinc oxide-graphene composite and 4 g of nickel-loaded aramid fiber, ultrasonically disperse, react for 3.5 h, filter and dry to obtain a fiber-graphene composite;

[0067] The mass ratio of zinc oxide-graphene composite and nickel-loaded aramid fiber is 1.5:4;

[0068] Step 4: Preparation of polyurethane absorbing porous material:

[0069] Taking polyether polyol, dispersant, and fiber-graphene composite, dispersing by ultrasonic, adding polyisocyanate, stirring evenly, foaming, and ripening, to obtain polyurethane absorbing porous material;

[0070] The polyurethane wave-absorbing porous material includes the following components, by weight: 21% of polyether polyol, 4.5% of dispersant, 8% of polyisocyanate, and the rest is fiber-graphene composite.

[0071] Comparative Example 2: Polypyrrole is not loaded on the aramid fiber, and the rest is the same as Example 1:

[0072] A preparation process of a polyurethane microwave absorbing porous material comprises the following steps:

[0073] Step 1: Preparation of nickel-loaded aramid fibers:

[0074] Take 1g of aramid fiber and 200mL of deionized water, and ultrasonically disperse for 3.5h to obtain an aramid fiber dispersion; take 12g of nickel dichloride hexahydrate and 50mL of deionized water, stir evenly, add 10mL of phosphoric acid, 5g of sodium dodecylbenzene sulfonate, and aramid fiber dispersion, heat to 60°C, stir evenly, drop ammonia water, adjust the pH value to 11, stir for 1.2h, add 10mL of KH-550, heat to 73°C, react for 1.2h, filter and dry to obtain nickel-loaded aramid fiber;

[0075] Step 2: Preparation of zinc oxide-graphene composite:

[0076] Take 250 mL of deionized water, add 30 mL of zinc acetate dihydrate and 20 mL of polyvinyl pyrrolidone, stir evenly, heat to 80°C, wash and filter to obtain zinc oxide;

[0077] Take 4g zinc oxide, 0.1g graphene oxide, and 50mL deionized water, and ultrasonically disperse them for 1.5h, add 8mL of 40% hydrazine hydrate solution, heat to 95°C and stir to react for 3h, wash and dry to obtain a zinc oxide-graphene composite;

[0078] Step 3: Preparation of fiber-graphene composite:

[0079] Take 3 g of polyacrylic acid and 50 mL of deionized water, stir evenly to obtain a polyacrylic acid solution; add 1.5 g of zinc oxide-graphene composite and 4 g of nickel-loaded aramid fiber, ultrasonically disperse, react for 3.5 h, filter and dry to obtain a fiber-graphene composite;

[0080] The mass ratio of zinc oxide-graphene composite and nickel-loaded aramid fiber is 1.5:4;

[0081] Step 4: Preparation of polyurethane absorbing porous material:

[0082] Taking polyether polyol, dispersant, and fiber-graphene composite, dispersing by ultrasonic, adding polyisocyanate, stirring evenly, foaming, and ripening, to obtain polyurethane absorbing porous material;

[0083] The polyurethane wave-absorbing porous material includes the following components, by weight: 21% of polyether polyol, 4.5% of dispersant, 8% of polyisocyanate, and the rest is fiber-graphene composite.

[0084] Comparative Example 3: Phosphoric acid is not added to nickel dichloride hexahydrate, and the rest is the same as Example 1:

[0085] A preparation process of a polyurethane microwave absorbing porous material comprises the following steps:

[0086] Step 1: Preparation of nickel-loaded aramid fibers:

[0087] Take 1g of aramid fiber and 200mL of deionized water, and perform ultrasonic dispersion for 3.5h to obtain an aramid fiber dispersion; add 1.2g of pyrrole monomer and 1mL of 0.01M phosphoric acid solution, stir evenly to obtain a mixed solution; take 12g of nickel dichloride hexahydrate and 50mL of deionized water, stir evenly, add 5g of sodium dodecylbenzene sulfonate and the mixed solution, heat to 60°C, stir evenly, add ammonia water dropwise, adjust the pH value to 11, stir for 1.2h, add 10mL of KH-550, heat to 73°C, react for 1.2h, filter and dry to obtain nickel-loaded aramid fiber;

[0088] Step 2: Preparation of zinc oxide-graphene composite:

[0089] Take 250 mL of deionized water, add 30 mL of zinc acetate dihydrate and 20 mL of polyvinyl pyrrolidone, stir evenly, heat to 80°C, wash and filter to obtain zinc oxide;

[0090] Take 4g zinc oxide, 0.1g graphene oxide, and 50mL deionized water, and ultrasonically disperse them for 1.5h, add 8mL of 40% hydrazine hydrate solution, heat to 95°C and stir to react for 3h, wash and dry to obtain a zinc oxide-graphene composite;

[0091] Step 3: Preparation of fiber-graphene composite:

[0092] Take 3 g of polyacrylic acid and 50 mL of deionized water, stir evenly to obtain a polyacrylic acid solution; add 1.5 g of zinc oxide-graphene composite and 4 g of nickel-loaded aramid fiber, ultrasonically disperse, react for 3.5 h, filter and dry to obtain a fiber-graphene composite;

[0093] The mass ratio of zinc oxide-graphene composite and nickel-loaded aramid fiber is 1.5:4;

[0094] Step 4: Preparation of polyurethane absorbing porous material:

[0095] Taking polyether polyol, dispersant, and fiber-graphene composite, dispersing by ultrasonic, adding polyisocyanate, stirring evenly, foaming, and ripening, to obtain polyurethane absorbing porous material;

[0096] The polyurethane wave-absorbing porous material includes the following components, by weight: 21% of polyether polyol, 4.5% of dispersant, 8% of polyisocyanate, and the rest is fiber-graphene composite.

[0097] Comparative Example 4: The mass ratio of the zinc oxide-graphene composite to the nickel-loaded aramid fiber is 0.5:3, and the rest is the same as in Example 1:

[0098] A preparation process of a polyurethane microwave absorbing porous material comprises the following steps:

[0099] Step 1: Preparation of nickel-loaded aramid fibers:

[0100] Take 1g of aramid fiber and 200mL of deionized water, and ultrasonically disperse for 3.5h to obtain an aramid fiber dispersion; add 1.2g of pyrrole monomer and 1mL of 0.01M phosphoric acid solution, stir evenly to obtain a mixed solution; take 12g of nickel dichloride hexahydrate and 50mL of deionized water, stir evenly, add 10mL of phosphoric acid, 5g of sodium dodecylbenzene sulfonate, and the mixed solution, heat to 60°C, stir evenly, add ammonia water, adjust the pH value to 11, stir for 1.2h, add 10mL of KH-550, heat to 73°C, react for 1.2h, filter and dry to obtain nickel-loaded aramid fiber;

[0101] Step 2: Preparation of zinc oxide-graphene composite:

[0102] Take 250 mL of deionized water, add 30 mL of zinc acetate dihydrate and 20 mL of polyvinyl pyrrolidone, stir evenly, heat to 80°C, wash and filter to obtain zinc oxide;

[0103] Take 4g zinc oxide, 0.1g graphene oxide, and 50mL deionized water, and ultrasonically disperse them for 1.5h, add 8mL of 40% hydrazine hydrate solution, heat to 95°C and stir to react for 3h, wash and dry to obtain a zinc oxide-graphene composite;

[0104] Step 3: Preparation of fiber-graphene composite:

[0105] Take 3 g of polyacrylic acid and 50 mL of deionized water, stir evenly to obtain a polyacrylic acid solution; add 0.79 g of zinc oxide-graphene composite and 4.74 g of nickel-loaded aramid fiber, ultrasonically disperse, react for 3.5 h, filter and dry to obtain a fiber-graphene composite;

[0106] The mass ratio of zinc oxide-graphene composite and nickel-loaded aramid fiber is 0.5:3;

[0107] Step 4: Preparation of polyurethane absorbing porous material:

[0108] Taking polyether polyol, dispersant, and fiber-graphene composite, dispersing by ultrasonic, adding polyisocyanate, stirring evenly, foaming, and ripening, to obtain polyurethane absorbing porous material;

[0109] The polyurethane wave-absorbing porous material includes the following components, by weight: 21% of polyether polyol, 4.5% of dispersant, 8% of polyisocyanate, and the rest is fiber-graphene composite.

[0110] Comparative Example 5: The mass ratio of the zinc oxide-graphene composite to the nickel-loaded aramid fiber is 1:1, and the rest is the same as in Example 1:

[0111] A preparation process of a polyurethane microwave absorbing porous material comprises the following steps:

[0112] Step 1: Preparation of nickel-loaded aramid fibers:

[0113] Take 1g of aramid fiber and 200mL of deionized water, and ultrasonically disperse for 3.5h to obtain an aramid fiber dispersion; add 1.2g of pyrrole monomer and 1mL of 0.01M phosphoric acid solution, stir evenly to obtain a mixed solution; take 12g of nickel dichloride hexahydrate and 50mL of deionized water, stir evenly, add 10mL of phosphoric acid, 5g of sodium dodecylbenzene sulfonate, and the mixed solution, heat to 60°C, stir evenly, add ammonia water, adjust the pH value to 11, stir for 1.2h, add 10mL of KH-550, heat to 73°C, react for 1.2h, filter and dry to obtain nickel-loaded aramid fiber;

[0114] Step 2: Preparation of zinc oxide-graphene composite:

[0115] Take 250 mL of deionized water, add 30 mL of zinc acetate dihydrate and 20 mL of polyvinyl pyrrolidone, stir evenly, heat to 80°C, wash and filter to obtain zinc oxide;

[0116] Take 4g zinc oxide, 0.1g graphene oxide, and 50mL deionized water, and ultrasonically disperse them for 1.5h, add 8mL of 40% hydrazine hydrate solution, heat to 95°C and stir to react for 3h, wash and dry to obtain a zinc oxide-graphene composite;

[0117] Step 3: Preparation of fiber-graphene composite:

[0118] Take 3 g of polyacrylic acid and 50 mL of deionized water, stir evenly to obtain a polyacrylic acid solution; add 2.75 g of zinc oxide-graphene composite and 2.75 g of nickel-loaded aramid fiber, ultrasonically disperse, react for 3.5 h, filter and dry to obtain a fiber-graphene composite;

[0119] The mass ratio of zinc oxide-graphene composite and nickel-loaded aramid fiber is 1:1;

[0120] Step 4: Preparation of polyurethane absorbing porous material:

[0121] Taking polyether polyol, dispersant, and fiber-graphene composite, dispersing by ultrasonic, adding polyisocyanate, stirring evenly, foaming, and ripening, to obtain polyurethane absorbing porous material;

[0122] The polyurethane wave-absorbing porous material includes the following components, by weight: 21% of polyether polyol, 4.5% of dispersant, 8% of polyisocyanate, and the rest is fiber-graphene composite.

[0123] experiment:

[0124] The performance of the polyurethane absorbing porous materials prepared in Examples 1 to 3 and Comparative Examples 1 to 5 was tested. The absorbing performance was tested using an N5230 vector network analyzer using the bow method. The electromagnetic parameter was the reflection loss at 10 GHz. The data obtained are shown in the following table:

[0125]

[0126] Conclusion: In Comparative Example 1, polyacrylic acid is not used to bond the zinc oxide-graphene composite and the nickel-loaded aramid fiber together, and the zinc oxide-graphene composite is easy to agglomerate in the matrix, affecting the wave absorption performance. In Comparative Example 2, polypyrrole is not loaded on the aramid fiber, and the wave absorption performance decreases. In Comparative Example 3, phosphoric acid is not added, and the particle size of nickel oxide is large, which affects the wave absorption performance. In Comparative Example 4, the mass ratio of zinc oxide-graphene composite and nickel-loaded aramid fiber is 0.5:3, and the amount of zinc oxide-graphene composite added is reduced. In Comparative Example 5, the mass ratio of zinc oxide-graphene composite and nickel-loaded aramid fiber is 1:1, and the amount of nickel-loaded aramid fiber added is reduced, and the wave absorption performance is reduced. In embodiments 1 to 3 of the present invention, a fiber-graphene composite is added to polyurethane, and a zinc oxide-graphene composite and a nickel-loaded aramid fiber are bonded together using adhesive polyacrylic acid to prepare a fiber-graphene composite. The polyacrylic acid also has a carboxyl group, which can react with the terminal hydroxyl group of the polyether polyol to enhance the dispersibility of the fiber-graphene composite in the matrix and improve the wave absorbing performance of the polyurethane wave absorbing porous material. The present invention uses pyrrole monomers to load polypyrrole on aramid fibers, and the loading of polypyrrole can improve the wave absorbing ability of aramid fibers. The present invention also adds a phosphoric acid solution, and the addition of the phosphoric acid solution can react with nickel phosphate at the same time, so that the generated nickel oxide has a smaller particle size, further enhancing the wave absorbing performance.

[0127] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A process for preparing a polyurethane microwave absorbing porous material, characterized in that: The following steps are involved: Step 1: Take polyacrylic acid and deionized water, stir evenly to obtain a polyacrylic acid solution; add zinc oxide-graphene composite and nickel-loaded aramid fiber, ultrasonically disperse, react for 3-4 hours, filter and dry to obtain a fiber-graphene composite; Step 2: taking polyether polyol, dispersant, fiber-graphene composite, ultrasonically dispersing, adding polyisocyanate, stirring evenly, foaming, and ripening to obtain polyurethane absorbing porous material; The polyurethane wave-absorbing porous material comprises the following components, by weight: 20-22% of polyether polyol, 4-5% of dispersant, 7-9% of polyisocyanate, and the remainder being a fiber-graphene composite; In step 1, the mass ratio of the zinc oxide-graphene composite and the nickel-loaded aramid fiber is (1-2): (3-5); The preparation method of the nickel-loaded aramid fiber is as follows: take aramid fiber and deionized water, perform ultrasonic dispersion for 3-4 hours, and obtain aramid fiber dispersion liquid; add pyrrole monomer and phosphoric acid solution, stir evenly, and obtain a mixed liquid; take nickel dichloride hexahydrate and deionized water, stir evenly, add phosphoric acid and sodium dodecylbenzene sulfonate, and the mixed liquid, heat it to 55-65° C., stir evenly, drop ammonia water, adjust the pH value, stir for 1-1.5 hours, add KH-550, heat it to 70-75° C., react for 1-1.5 hours, filter, and dry to obtain the nickel-loaded aramid fiber.

2. The process for preparing a polyurethane microwave absorbing porous material according to claim 1, characterized in that: The preparation method of the zinc oxide-graphene composite is as follows: taking zinc oxide, graphene oxide and deionized water, ultrasonically dispersing for 1-2 hours, adding hydrazine hydrate solution, heating to 95° C. and stirring for reaction for 2-4 hours, washing and drying to obtain the zinc oxide-graphene composite.

3. The process for preparing a polyurethane microwave absorbing porous material according to claim 2, characterized in that: The mass ratio of zinc oxide to graphene oxide is (4-6):0.

1.

4. The process for preparing a polyurethane absorbing porous material according to claim 2, characterized in that: The preparation method of zinc oxide is as follows: taking deionized water, adding zinc acetate dihydrate and polyvinyl pyrrolidone, stirring evenly, heating to 75-85° C., washing, filtering, and obtaining zinc oxide.

5. The process for preparing a polyurethane microwave absorbing porous material according to claim 1, characterized in that: Ammonia water was added dropwise to adjust the pH value to 11.