A rare earth element-added neodymium iron boron magnet and its preparation process

By adding lanthanum-copper alloy and samarium-copper alloy to sintered NdFeB magnets, and performing specific processing and surface coating treatments, the problem of poor temperature stability of NdFeB magnets is solved, and the applicability and chemical stability of high-temperature applications are achieved. sexual enhancement.

CN118588437BActive Publication Date: 2024-10-18JIANGXI YG MAGNET CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411049460.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-18
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

Due to the low Curie temperature and high coercive force temperature coefficient, the existing sintered NdFeB magnets have poor temperature stability and cannot meet the needs of high-temperature applications.

Method used

By adding lanthanum copper alloy and samarium copper alloy, vacuum smelting, rapid solidification, hydrogen explosion, airflow grinding, mixing with nano-aluminum powder and compression molding, followed by vacuum sintering and two tempering heat treatments, and on the surface of the magnet The nickel-containing alloy powder is sputtered and subjected to high-temperature diffusion treatment to form NdFeB magnets with high thermal stability.

Benefits of technology

It significantly improves the thermal stability and coercivity of NdFeB magnets, expands its scope of application, meets the needs of high-temperature applications, and enhances chemical stability and corrosion resistance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a neodymium iron boron magnet with rare earth elements added thereto and a preparation process thereof, belonging to the technical field of rare earth permanent magnetic materials; the preparation process thereof comprises the following steps: adding lanthanum copper alloy and samarium copper alloy and smelting; smelting copper cobalt alloy and copper gallium alloy and pressing and forming; vacuum sintering and performing two tempering heat treatments; mixing and smelting copper neodymium alloy and nickel copper alloy and preparing nickel-containing alloy powder; magnetron sputtering nickel-containing alloy powder and performing high-temperature diffusion treatment. The present invention is to mix pure iron, ferroboron and praseodymium neodymium and smelt them, then mix them with lanthanum copper alloy, samarium copper alloy and cobalt iron alloy for rapid solidification and belt throwing, and then perform hydrogen explosion crushing and air flow grinding to prepare alloy fine powder, and then mix them with nano aluminum powder and alloy powder for pressing and forming, sintering and tempering to prepare magnetic blank, and then perform alloy coating sputtering and perform high-temperature diffusion treatment, so that the obtained neodymium iron boron magnet has not only excellent magnetic properties, but also high thermal stability, and can meet the requirements of high-temperature application fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rare earth permanent magnet materials, and in particular to a rare earth element-added neodymium iron boron magnet and a preparation process thereof. Background Art

[0002] Sintered NdFeB magnet is an intermetallic compound composed of rare earth element neodymium and iron and boron. It is usually made of praseodymium and neodymium as the main raw material through smelting, pressing and sintering processes. Compared with ordinary magnets, it has high remanence, high coercive force, high magnetic energy product and excellent machining properties. Therefore, it is called the king of magnets and has gradually become the most widely used permanent magnet material today.

[0003] However, the existing sintered NdFeB magnets have poor temperature stability due to their low Curie temperature and high coercive force temperature coefficient. The maximum operating temperature usually does not exceed 100°C. They will experience thermal demagnetization or even failure at high temperatures. It is difficult to exert the advantages of magnetic properties and cannot meet the requirements of high-temperature applications, resulting in a narrow range of applications for sintered NdFeB magnets.

[0004] In order to solve the deficiencies in the prior art, the present invention proposes a rare earth element-added NdFeB magnet with good thermal stability and a preparation process thereof to meet the needs of high temperature application fields. Summary of the invention

[0005] In view of the shortcomings of the prior art, the object of the present invention is to provide a neodymium iron boron magnet with added rare earth elements and a preparation process thereof.

[0006] S1: Add lanthanum copper alloy and samarium copper alloy and smelt

[0007] Pure iron, ferroboron and praseodymium-neodymium are vacuum smelted, then mixed with lanthanum-copper alloy and samarium-copper alloy for smelting and rapid solidification, and then subjected to hydrogen explosion treatment and helium gas flow milling to obtain alloy fine powder;

[0008] S2: Smelting copper-cobalt alloy and copper-gallium alloy and pressing them into shape

[0009] The copper-cobalt alloy and the copper-gallium alloy are mixed and smelted and spun into a rapid quenching strip, ball-milled into powder, fully mixed with the above alloy fine powder and nano-aluminum powder, and then oriented pressed and cold isostatically pressed to obtain a magnet compact;

[0010] S3: Vacuum sintering and double tempering heat treatment

[0011] The magnet green compact is subjected to vacuum sintering, cooled to room temperature in a furnace, and then subjected to two tempering heat treatments at different temperatures to obtain a magnet green compact;

[0012] S4: Mixing and melting copper-neodymium alloy and nickel-copper alloy to prepare nickel-containing alloy powder

[0013] The copper-neodymium alloy and the nickel-copper alloy are mixed and vacuum-melted, and after cooling, the mixture is placed in a ball mill and ball-milled into powder to obtain nickel-containing alloy powder;

[0014] S5: Magnetron sputtering of nickel-containing alloy powder and high temperature diffusion treatment

[0015] The nickel-containing alloy powder is sputtered onto the surface of the pretreated magnetic blank by using an ultra-high vacuum three-chamber magnetron sputtering system. After high-temperature diffusion treatment and tempering heat treatment, the powder is cooled to room temperature with the furnace to obtain a neodymium iron boron magnet.

[0016] Furthermore, step S1 specifically includes the following steps:

[0017] S1.1: Place pure iron, ferroboron and praseodymium-neodymium in a vacuum melting and quenching furnace and perform vacuum melting for 1-2 hours to obtain an alloy ingot;

[0018] S1.2: adding the alloy ingot, lanthanum copper alloy, samarium copper alloy and cobalt iron alloy into a vacuum quick-setting furnace, smelting for 1-2 hours, and quick-setting and cooling to room temperature to obtain a 0.2-0.4 mm alloy quick-setting strip, wherein the operation speed of the quick-setting and cooling device is 1.5-2 m / s;

[0019] S1.3: adding the alloy quick-solidification belt into a hydrogen crushing furnace and performing hydrogen explosion crushing to obtain alloy coarse powder with a particle size of 0.1-0.3 mm;

[0020] S1.4: The above alloy coarse powder is placed in a jet mill, and subjected to a jet milling process in a helium environment to obtain alloy fine powder with a particle size of 0.8-1.2 μm.

[0021] Furthermore, step S2 specifically includes the following steps:

[0022] S2.1: Add the copper-cobalt alloy and the copper-gallium alloy into a vacuum arc furnace, and repeatedly melt them 4-5 times, each time for 40-50 minutes, to obtain an alloy ingot;

[0023] S2.2: The alloy ingot is placed in a vacuum quenching belt spinning device, and spun at a speed of 6-8 m / s into a quenching belt with a width of 10-12 mm and a thickness of 0.2-0.3 mm, and then placed in a ball mill for ball milling to obtain an alloy powder with a particle size of 4-5 μm;

[0024] S2.3: Add the alloy fine powder obtained in step S1.4, the alloy powder and nano aluminum powder into a mixer at a mass ratio of 450-500:3-5:1, and mix for 4-5 hours to obtain mixed magnetic powder;

[0025] S2.4: Under the protection of nitrogen, the mixed magnetic powder is added into a pressing mold, and then placed into a molding press, and then pressed and molded under the condition of magnetic field orientation to obtain a magnet green body;

[0026] S2.5: Place the magnet green body in a static press and perform cold isostatic pressing at a pressure of 220-230 MPa to obtain a magnet compact.

[0027] Furthermore, step S3 specifically includes the following steps:

[0028] S3.1: placing the magnet compact obtained in step S2.5 in a vacuum sintering furnace, sintering at a temperature of 1000-1200°C for 4-5h, and cooling to room temperature to obtain a sintered compact;

[0029] S3.2: placing the sintered green body in a tempering furnace, heating it to 800-900°C at a rate of 10-20°C / min, and then keeping it at that temperature for 2-3h to perform a tempering heat treatment to obtain a primary heat-treated green body;

[0030] S3.3: Adjust the heating rate of the tempering furnace to 5-10°C / min, heat the above-mentioned primary heat-treated green body to 450-500°C, then keep it warm for 2-3h, and perform secondary tempering heat treatment to obtain a magnetic green body.

[0031] Furthermore, step S4 specifically includes the following steps:

[0032] S4.1: placing the copper-neodymium alloy and the nickel-copper alloy in a vacuum arc furnace, vacuum melting for 1-2 hours, and cooling the furnace to room temperature to obtain a nickel-containing ingot;

[0033] S4.2: Place the above nickel-containing ingot in a ball mill and ball mill for 2-3 hours to obtain a nickel-containing alloy powder with a particle size of 1.5-2 μm.

[0034] Furthermore, step S5 specifically includes the following steps:

[0035] S5.1: polishing the surface of the magnetic body obtained in step S3.3 with sandpaper, washing with deionized water, ultrasonically treating in ethanol for 15-20 minutes, and then vacuum drying to obtain a surface pretreated body;

[0036] S5.2: Set the vacuum degree of the ultra-high vacuum three-chamber magnetron sputtering system to (8-10)×10 -5 Pa, argon gas flow rate of 40-50sccm, coating working pressure of 1-1.3Pa and sputtering power of 100-120W;

[0037] S5.3: placing the surface pretreated body in an ultra-high vacuum three-chamber magnetron sputtering system, and sputtering the nickel-containing alloy powder obtained in step S4.2 on the upper and lower surfaces of the surface pretreated body to form an alloy coating with a thickness of 2.8-3 μm, thereby obtaining a coated body;

[0038] S5.4: Wrap the coated body with molybdenum foil, place it in a vacuum tube furnace, heat it to 800-900°C at a rate of 5-10°C / min, and then keep it at that temperature for 5-6h to perform high temperature diffusion treatment to obtain a precursor magnet;

[0039] S5.5: When the precursor magnet is cooled to 70-80°C, the temperature is raised to 450-550°C and kept at this temperature for 2-3 hours for tempering heat treatment. After the precursor magnet is cooled to room temperature in the furnace, a NdFeB magnet is obtained.

[0040] Furthermore, the alloy quick-setting belt comprises: 15-16wt% Nd, 5-6wt% B, 5-6wt% Pr, 8-12wt% Cu, 0.05-0.1wt% La, 0.05-0.1wt% Sm, and the balance is Fe and unavoidable impurities.

[0041] Further, the alloy ingot includes 15-20wt% Co and 8-12wt% Ga, with the balance being Cu.

[0042] Furthermore, the nickel-containing alloy powder includes 40-50 wt % Nd and 35-45 wt % Ni, with the balance being Cu.

[0043] A neodymium iron boron magnet with added rare earth elements is prepared by any of the above-mentioned processes for preparing a neodymium iron boron magnet with added rare earth elements.

[0044] Compared with the prior art, the present invention has the following beneficial effects:

[0045] (1) The present invention prepares a magnetic blank by mixing pure iron, ferroboron and praseodymium-neodymium and smelting the mixture, and then rapidly solidifying and spinning the mixture with lanthanum-copper alloy, samarium-copper alloy and cobalt-iron alloy, and then subjecting the mixture to hydrogen explosion crushing and air flow grinding to prepare alloy fine powder, and then mixing the mixture with nano-aluminum powder and alloy powder, pressing and molding the mixture, vacuum sintering the mixture and subjecting the mixture to two tempering heat treatments, and then sputtering alloy coating on the upper and lower surfaces thereof, respectively, and subjecting the mixture to high temperature diffusion treatment and tempering heat treatment. The obtained NdFeB magnet has not only excellent magnetic properties, but also high thermal stability and can meet the requirements of high temperature application fields.

[0046] (2) The present invention melts pure iron, ferroboron and praseodymium-neodymium into a melt, and then mixes it with lanthanum-copper alloy, samarium-copper alloy and cobalt-iron alloy through a vacuum rapid solidification belt spinning process, so as to incorporate copper, lanthanum and samarium elements into the neodymium iron boron magnet. After the three elements of copper, lanthanum and samarium are incorporated, the irreversible magnetic flux loss of the neodymium iron boron magnet after being kept at 180°C for 2 hours is significantly reduced, thereby achieving the effect of improving the thermal stability of the neodymium iron boron magnet.

[0047] (3) The present invention prepares an NdFeB magnet by mixing copper-cobalt alloy and copper-gallium alloy for smelting, quenching, belt spinning and ball milling to prepare an alloy powder, and then adding the alloy powder together with nano-aluminum powder into the alloy fine powder. The coercive force and temperature stability of the NdFeB magnet can be effectively improved to meet the needs of high-temperature applications and expand the application range of sintered NdFeB.

[0048] (4) The present invention mixes and melts a copper-neodymium alloy and a nickel-copper alloy into a neodymium-nickel-copper ternary alloy, and then magnetron sputters the ternary alloy onto the surface of a magnetic blank. After high-temperature diffusion treatment and tempering heat treatment, the magnetic properties of the prepared neodymium-iron-boron magnet can be further improved, and its chemical stability can be increased, and the driving force of electrochemical corrosion can be reduced, thereby achieving the effect of improving the corrosion resistance of the magnet. DETAILED DESCRIPTION

[0049] The following is a detailed description of a rare earth element added NdFeB magnet and its preparation process provided by the present invention in conjunction with specific embodiments. At the same time, it is explained here that in order to make the embodiments more detailed, the following embodiments are the best and preferred embodiments, and those skilled in the art may also adopt other alternatives to implement some known technologies; and some of them are only for more specific description of the embodiments, and are not intended to specifically limit the present invention.

[0050] Example 1

[0051] A preparation process of a rare earth element-added NdFeB magnet comprises the following steps:

[0052] S1: Add lanthanum copper alloy and samarium copper alloy and smelt

[0053] Put pure iron, ferroboron and praseodymium-neodymium in a vacuum melting furnace, vacuum melt for 1 hour to obtain an alloy ingot, then add the alloy ingot and lanthanum copper alloy, samarium copper alloy and cobalt iron alloy into a vacuum quick-setting furnace, melt for 1 hour, and quickly cool to room temperature to obtain a 0.2 mm alloy quick-setting belt, wherein the operation speed of the quick-setting cooling device is 1.5 m / s, and the alloy quick-setting belt includes 15wt% Nd, 5wt% B, 5wt% Pr, 8wt% Cu, 0.05wt% La, 0.05wt% Sm, and the balance is Fe and unavoidable impurities. Subsequently, the alloy quick-setting belt is added to a hydrogen crushing furnace for hydrogen explosion treatment to obtain an alloy coarse powder with a particle size of 0.1 mm. Finally, the alloy coarse powder is placed in a jet mill, and a jet milling process is performed in a helium environment to obtain an alloy fine powder with a particle size of 0.8 μm.

[0054] S2: Smelting copper-cobalt alloy and copper-gallium alloy and pressing them into shape

[0055] The copper-cobalt alloy and the copper-gallium alloy are added to a vacuum arc furnace, and smelted repeatedly for 4 times, each time for 40 minutes, to obtain an alloy ingot, wherein the alloy ingot includes 15wt% Co and 8wt% Ga, and the remainder is Cu, and then the alloy ingot is placed in a vacuum quenching belt throwing device, and thrown into a quenching belt with a width of 10mm and a thickness of 0.2mm at a rate of 6m / s, and then placed in a ball mill for ball milling to obtain an alloy powder with a particle size of 4μm, and then the above alloy fine powder, alloy powder and nano aluminum powder are added to a mixer at a mass ratio of 450:3:1, mixed for 4h, to obtain mixed magnetic powder, and then, under the protection of nitrogen, the mixed magnetic powder is added to a pressing mold, and placed in a molding press, and then pressed and molded under the condition of adding a magnetic field orientation to obtain a magnet green body, and finally, the magnet green body is placed in a static press, and cold isostatically pressed at a pressure of 220MPa to obtain a magnet compact;

[0056] S3: Vacuum sintering and double tempering heat treatment

[0057] The magnet green compact is placed in a vacuum sintering furnace, vacuum sintered at 1000°C for 4 hours, cooled to room temperature with the furnace, and a sintered green body is obtained. The sintered green body is then placed in a tempering furnace, heated to 800°C at a rate of 10°C / min, and then kept warm for 2 hours to perform a tempering heat treatment to obtain a primary heat-treated green body. Subsequently, the heating rate of the tempering furnace is adjusted to 5°C / min, and the primary heat-treated green body is heated to 450°C, and then kept warm for 2 hours to perform a secondary tempering heat treatment to obtain a magnet green body.

[0058] S4: Mixing and melting copper-neodymium alloy and nickel-copper alloy to prepare nickel-containing alloy powder

[0059] The copper-neodymium alloy and the nickel-copper alloy are placed in a vacuum arc furnace for vacuum melting for 1 hour, and then cooled to room temperature with the furnace to obtain a nickel-containing ingot, and then the nickel-containing ingot is placed in a ball mill for ball milling for 2 hours to obtain a nickel-containing alloy powder with a particle size of 1.5 μm, wherein the nickel-containing alloy powder includes 40wt% Nd and 35wt% Ni, and the balance is Cu;

[0060] S5: Magnetron sputtering of nickel-containing alloy powder and high temperature diffusion treatment

[0061] The surface of the magnetic body was polished with sandpaper, washed with deionized water, and then ultrasonically treated in ethanol for 15 min. Then, it was vacuum dried to obtain a surface pretreated body. Subsequently, the vacuum degree of the ultra-high vacuum three-chamber magnetron sputtering system was set to 8×10 -5 The surface pretreated blank is placed in an ultra-high vacuum three-chamber magnetron sputtering system, and the nickel-containing alloy powder is sputtered on the upper and lower surfaces of the surface pretreated blank respectively to form an alloy coating with a thickness of 2.8 μm to obtain a coated blank, which is then wrapped with molybdenum foil and placed in a vacuum tube furnace. The temperature is increased to 800°C at a rate of 5°C / min, and then kept warm for 5 hours for high-temperature diffusion treatment to obtain a precursor magnet. When the precursor magnet is cooled to 70°C, the temperature is increased to 450°C and kept warm for 2 hours for tempering heat treatment. After cooling to room temperature with the furnace, a neodymium iron boron magnet is obtained.

[0062] Performance Test:

[0063] 1. The magnetic properties of the prepared NdFeB magnets at room temperature were tested using a NIM-500C high temperature permanent magnet measuring instrument. The results are shown in Table 1 below.

[0064] 2. The irreversible magnetic flux loss of the prepared NdFeB magnet was tested in a Helmholtz coil by the Czochralski method at 180°C for 2 hours. The results are shown in Table 1 below.

[0065] 3. A high temperature and high pressure accelerated corrosion test was carried out using a PCT-30-2 high pressure accelerated life test machine. The experimental parameters were set at 120°C, 0.2MPa and 100% relative humidity. The corrosion weight loss of the NdFeB magnet was tested for 96 hours. The results are shown in Table 1 below.

[0066] Table 1 Summary of performance test results of Example 1

[0067] Test items Coercive force (kA / m) Irreversible flux loss (%) <![CDATA[Corrosion weight loss (mg / cm 2 )]]> Example 1 1647 38.86 0.24

[0068] Example 2

[0069] A preparation process of a rare earth element-added NdFeB magnet comprises the following steps:

[0070] S1: Add lanthanum copper alloy and samarium copper alloy and smelt

[0071] Put pure iron, ferroboron and praseodymium-neodymium in a vacuum melting furnace, vacuum melt for 1.5 hours to obtain an alloy ingot, then add the alloy ingot and lanthanum copper alloy, samarium copper alloy and cobalt iron alloy into a vacuum quick-setting furnace, melt for 1.5 hours, and quickly cool to room temperature to obtain a 0.3 mm alloy quick-setting belt, wherein the operation speed of the quick-setting cooling device is 1.75 m / s, and the alloy quick-setting belt includes 15.5wt% Nd, 5.5wt% B, 5.5wt% Pr, 10wt% Cu, 0.075wt% La, 0.075wt% Sm, and the balance is Fe and unavoidable impurities. Subsequently, the alloy quick-setting belt is added to a hydrogen crushing furnace for hydrogen explosion treatment to obtain an alloy coarse powder with a particle size of 0.2 mm. Finally, the alloy coarse powder is placed in a jet mill, and a jet milling process is performed in a helium environment to obtain an alloy fine powder with a particle size of 1 μm.

[0072] S2: Smelting copper-cobalt alloy and copper-gallium alloy and pressing them into shape

[0073] The copper-cobalt alloy and the copper-gallium alloy are added to a vacuum arc furnace, and smelted repeatedly for 4 times, each time for 45 minutes, to obtain an alloy ingot, wherein the alloy ingot includes 17.5wt% Co and 10wt% Ga, and the balance is Cu, and then the alloy ingot is placed in a vacuum quenching belt throwing device, and thrown into a quenching belt with a width of 11mm and a thickness of 0.25mm at a rate of 7m / s, and then placed in a ball mill for ball milling to obtain an alloy powder with a particle size of 4.5μm, and then the above alloy fine powder, alloy powder and nano aluminum powder are added to a mixer at a mass ratio of 475:4:1, mixed for 4.5h to obtain mixed magnetic powder, and then, under the protection of nitrogen, the mixed magnetic powder is added to a pressing mold and placed in a molding press, and then pressed and molded under the condition of adding a magnetic field orientation to obtain a magnet green body, and finally, the magnet green body is placed in a static press, and cold isostatically pressed at a pressure of 225MPa to obtain a magnet compact;

[0074] S3: Vacuum sintering and double tempering heat treatment

[0075] The magnet green compact is placed in a vacuum sintering furnace, vacuum sintered at 1100°C for 4.5h, cooled to room temperature with the furnace to obtain a sintered green body, and then placed in a tempering furnace, heated to 850°C at a rate of 15°C / min, and then kept warm for 2.5h, and subjected to a first tempering heat treatment to obtain a first heat-treated green body, and then the heating rate of the tempering furnace is adjusted to 7.5°C / min, the first heat-treated green body is heated to 475°C, and then kept warm for 2.5h, and subjected to a second tempering heat treatment to obtain a magnet green body;

[0076] S4: Mixing and melting copper-neodymium alloy and nickel-copper alloy to prepare nickel-containing alloy powder

[0077] The copper-neodymium alloy and the nickel-copper alloy are placed in a vacuum arc furnace for vacuum melting for 1.5 hours, and after cooling to room temperature with the furnace, a nickel-containing ingot is obtained, and then the nickel-containing ingot is placed in a ball mill for ball milling for 2.5 hours to obtain a nickel-containing alloy powder with a particle size of 1.75 μm, wherein the nickel-containing alloy powder includes 45wt% Nd and 40wt% Ni, and the balance is Cu;

[0078] S5: Magnetron sputtering of nickel-containing alloy powder and high temperature diffusion treatment

[0079] The surface of the magnetic body was polished with sandpaper, washed with deionized water, and then ultrasonically treated in ethanol for 17.5 min. Then, it was vacuum dried to obtain a surface pretreated body. Subsequently, the vacuum degree of the ultra-high vacuum three-chamber magnetron sputtering system was set to 9×10 -5 The surface pretreated blank is placed in an ultra-high vacuum three-chamber magnetron sputtering system, and the nickel-containing alloy powder is sputtered on the upper and lower surfaces of the surface pretreated blank respectively to form an alloy coating with a thickness of 2.9 μm to obtain a coated blank, which is then wrapped with molybdenum foil and placed in a vacuum tube furnace. The temperature is increased to 850°C at a rate of 7.5°C / min, and then kept warm for 5.5 hours for high-temperature diffusion treatment to obtain a precursor magnet. When the precursor magnet is cooled to 75°C, the temperature is increased to 500°C and kept warm for 2.5 hours for tempering heat treatment. After cooling to room temperature with the furnace, a neodymium iron boron magnet is obtained.

[0080] Performance Testing:

[0081] 1. The magnetic properties of the prepared NdFeB magnets at room temperature were tested using a NIM-500C high temperature permanent magnet measuring instrument. The results are shown in Table 2 below.

[0082] 2. The irreversible magnetic flux loss of the prepared NdFeB magnet was tested in a Helmholtz coil by the Czochralski method at 180°C for 2 hours. The results are shown in Table 2 below.

[0083] 3. A high temperature and high pressure accelerated corrosion test was carried out using a PCT-30-2 high pressure accelerated life test machine. The experimental parameters were set to 120°C, 0.2MPa and 100% relative humidity. The corrosion weight loss of the NdFeB magnet was tested for 96 hours. The results are shown in Table 2 below.

[0084] Table 2 Summary of performance test results of Example 2

[0085] Test items Coercive force (kA / m) Irreversible flux loss (%) <![CDATA[Corrosion weight loss (mg / cm 2 ).]]> Example 2 1648 38.79 0.24

[0086] Example 3

[0087] A preparation process of a rare earth element-added NdFeB magnet comprises the following steps:

[0088] S1: Add lanthanum copper alloy and samarium copper alloy and smelt

[0089] Put pure iron, ferroboron and praseodymium-neodymium in a vacuum melting furnace, vacuum melt for 2 hours to obtain an alloy ingot, then add the alloy ingot and lanthanum copper alloy, samarium copper alloy and cobalt iron alloy into a vacuum quick-setting furnace, melt for 2 hours, and quickly cool to room temperature to obtain a 0.4 mm alloy quick-setting belt, wherein the operation speed of the quick-setting cooling device is 2 m / s, and the alloy quick-setting belt includes 16wt% Nd, 6wt% B, 6wt% Pr, 12wt% Cu, 0.1wt% La, 0.1wt% Sm, and the balance is Fe and unavoidable impurities. Subsequently, the alloy quick-setting belt is added to a hydrogen crushing furnace for hydrogen explosion treatment to obtain an alloy coarse powder with a particle size of 0.3 mm. Finally, the alloy coarse powder is placed in a jet mill, and a jet milling process is performed in a helium environment to obtain an alloy fine powder with a particle size of 1.2 μm.

[0090] S2: Smelting copper-cobalt alloy and copper-gallium alloy and pressing them into shape

[0091] The copper-cobalt alloy and the copper-gallium alloy are added to a vacuum arc furnace, and smelted repeatedly for 5 times, each time for 50 minutes, to obtain an alloy ingot, wherein the alloy ingot includes 20wt% Co and 12wt% Ga, and the remainder is Cu, and then the alloy ingot is placed in a vacuum rapid quenching belt throwing device, and thrown into a rapid quenching belt with a width of 12mm and a thickness of 0.3mm at a rate of 8m / s, and then placed in a ball mill for ball milling to obtain an alloy powder with a particle size of 5μm, and then the above alloy fine powder, alloy powder and nano aluminum powder are added to a mixer at a mass ratio of 500:5:1, mixed for 5h, to obtain mixed magnetic powder, and then, under the protection of nitrogen, the mixed magnetic powder is added to a pressing mold, and placed in a molding press, and then pressed and molded under the condition of adding a magnetic field orientation to obtain a magnet green body, and finally, the magnet green body is placed in a static press, and cold isostatically pressed at a pressure of 230MPa to obtain a magnet compact;

[0092] S3: Vacuum sintering and double tempering heat treatment

[0093] The magnet green compact is placed in a vacuum sintering furnace, vacuum sintered at 1200°C for 5 hours, cooled to room temperature with the furnace, and a sintered green body is obtained. The sintered green body is then placed in a tempering furnace, heated to 900°C at a rate of 20°C / min, and then kept warm for 3 hours to perform a tempering heat treatment to obtain a primary heat-treated green body. Subsequently, the heating rate of the tempering furnace is adjusted to 10°C / min, and the primary heat-treated green body is heated to 500°C, and then kept warm for 3 hours to perform a secondary tempering heat treatment to obtain a magnet green body.

[0094] S4: Mixing and melting copper-neodymium alloy and nickel-copper alloy to prepare nickel-containing alloy powder

[0095] The copper-neodymium alloy and the nickel-copper alloy are placed in a vacuum arc furnace for vacuum melting for 2 hours, and then cooled to room temperature with the furnace to obtain a nickel-containing ingot, and then the nickel-containing ingot is placed in a ball mill for ball milling for 3 hours to obtain a nickel-containing alloy powder with a particle size of 2 μm, wherein the nickel-containing alloy powder includes 50wt% Nd and 45wt% Ni, and the balance is Cu;

[0096] S5: Magnetron sputtering of nickel-containing alloy powder and high temperature diffusion treatment

[0097] The surface of the magnetic body was polished with sandpaper, washed with deionized water, and then ultrasonically treated in ethanol for 20 min. Then, it was vacuum dried to obtain a surface pretreated body. Subsequently, the vacuum degree of the ultra-high vacuum three-chamber magnetron sputtering system was set to 10×10 -5 The surface pretreated blank is placed in an ultra-high vacuum three-chamber magnetron sputtering system, and the nickel-containing alloy powder is sputtered on the upper and lower surfaces of the surface pretreated blank respectively to form an alloy coating with a thickness of 3 μm to obtain a coated blank, which is then wrapped with molybdenum foil and placed in a vacuum tube furnace. The temperature is increased to 900°C at a rate of 10°C / min, and then kept warm for 6 hours for high-temperature diffusion treatment to obtain a precursor magnet. When the precursor magnet is cooled to 80°C, the temperature is increased to 550°C and kept warm for 3 hours for tempering heat treatment. After cooling to room temperature with the furnace, a NdFeB magnet is obtained.

[0098] Performance Test:

[0099] 1. The magnetic properties of the prepared NdFeB magnets at room temperature were tested using a NIM-500C high temperature permanent magnet measuring instrument. The results are shown in Table 3 below.

[0100] 2. The irreversible magnetic flux loss of the prepared NdFeB magnet was tested in a Helmholtz coil by the Czochralski method at 180°C for 2 hours. The results are shown in Table 3 below.

[0101] 3. A high temperature and high pressure accelerated corrosion test was carried out using a PCT-30-2 high pressure accelerated life test machine. The experimental parameters were set to 120°C, 0.2MPa and 100% relative humidity. The corrosion weight loss of the NdFeB magnet was tested for 96 hours. The results are shown in Table 2 below.

[0102] Table 3 Summary of performance test results of Example 3

[0103] Test items Coercive force (kA / m) Irreversible flux loss (%) <![CDATA[Corrosion weight loss (mg / cm 2 )]]> Example 3 1647 38.92 0.24

[0104] Comparative Example 1

[0105] The difference between this comparative example 1 and Example 1 is that, first, the lanthanum copper alloy, samarium copper alloy and cobalt iron alloy in step S1 are removed; secondly, the step of preparing alloy ingots and alloy powder in step S2 is removed, and the alloy powder and nano aluminum powder are replaced with an equal amount of alloy fine powder; finally, step S4 and step S5 are removed. That is, the magnetic blank obtained after sintering and two tempering heat treatments is directly subjected to performance testing, and the testing method is referred to Example 1, and the test results are shown in Table 4 below.

[0106] Table 4 Summary of performance test results of comparative example 1

[0107] Test items Coercive force (kA / m) Irreversible flux loss (%) <![CDATA[Corrosion weight loss (mg / cm 2 ).]]> Comparative Example 1 1176 69.34 1.58

[0108] From the performance test comparison between Comparative Example 1 and Example 1, it can be seen that the NdFeB magnet obtained by smelting pure iron, ferroboron and praseodymium-neodymium mixed, then mixing with lanthanum-copper alloy, samarium-copper alloy and cobalt-iron alloy for rapid solidification and belt spinning, hydrogen explosion crushing and air flow grinding to make alloy fine powder, then mixing with nano-aluminum powder and alloy powder and pressing and molding, vacuum sintering and tempering heat treatment twice to make a magnetic blank, and then sputtering alloy coating on the upper and lower surfaces respectively and performing high-temperature diffusion treatment and tempering heat treatment. Not only does it have excellent magnetic properties, but it also has high thermal stability and can meet the requirements of high-temperature application fields.

[0109] Comparative Example 2

[0110] The difference between this comparative example and Example 1 is that only the lanthanum iron alloy, samarium copper alloy and cobalt iron alloy in step S1 are removed, and then the performance test of the prepared NdFeB magnet is carried out according to the performance test method in Example 1, and the results are shown in Table 5 below.

[0111] Table 5 Summary of performance test results of comparative example 2

[0112] Test items Coercive force (kA / m) Irreversible flux loss (%) <![CDATA[Corrosion weight loss (mg / cm 2 )]]> Comparative Example 2 1529 53.47 0.27

[0113] From the performance test comparison between Comparative Example 2 and Example 1, it can be seen that after pure iron, ferroboron and praseodymium-neodymium are smelted into a melt, they are mixed with lanthanum-copper alloy, samarium-copper alloy and cobalt-iron alloy through a vacuum rapid solidification belt spinning process, so as to incorporate copper, lanthanum and samarium elements into the NdFeB magnet. After the three elements of copper, lanthanum and samarium are incorporated, the irreversible flux loss of the NdFeB magnet after being kept at 180°C for 2h is significantly reduced, thereby achieving the effect of improving the thermal stability of the NdFeB magnet.

[0114] Comparative Example 3

[0115] The difference between this comparative example and Example 1 is that the step of preparing alloy ingots and alloy powder in step S2 is removed, and the alloy powder and nano-aluminum powder are replaced with an equal amount of alloy fine powder, and then the performance test method in Example 1 is referred to to perform a performance test on the prepared NdFeB magnet, and the results are shown in Table 6 below.

[0116] Table 6 Summary of performance test results of comparative example 3

[0117] Test items Coercive force (kA / m) Irreversible flux loss (%) <![CDATA[Corrosion weight loss (mg / cm 2 ).]]> Comparative Example 3 1382 56.16 0.26

[0118] From the performance test comparison between Comparative Example 3 and Example 1, it can be seen that by mixed melting of copper-cobalt alloy and copper-gallium alloy, rapid quenching and ball milling to make alloy powder, and then adding it together with nano-aluminum powder into alloy fine powder to make NdFeB magnet, the coercive force and temperature stability of NdFeB magnet can be effectively improved to meet the needs of high-temperature applications and expand the scope of application of sintered NdFeB.

[0119] Comparative Example 4

[0120] The difference between this comparative example and Example 1 is that step S4 and step S5 are removed, and then the performance test of the prepared NdFeB magnet is carried out with reference to the performance test method in Example 1, and the results are shown in Table 7 below.

[0121] Table 7 Summary of performance test results of comparative example 4

[0122] Test items Coercive force (kA / m) Irreversible flux loss (%) <![CDATA[Corrosion weight loss (mg / cm 2 )]]> Comparative Example 4 1584 39.26 1.55

[0123] From the performance test comparison between Comparative Example 4 and Example 1, it can be seen that by mixing and smelting the copper-neodymium alloy and the nickel-copper alloy into a neodymium-nickel-copper ternary alloy, and then magnetron sputtering the ternary alloy on the surface of the magnetic blank, after high-temperature diffusion treatment and tempering heat treatment, not only can the magnetic properties of the prepared neodymium iron boron magnet be further improved, but also its chemical stability can be increased and the motive force of electrochemical corrosion can be reduced, thereby achieving the effect of improving the corrosion resistance of the magnet.

[0124] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A process for preparing a neodymium iron boron magnet with rare earth elements added, characterized in that: The steps include: S1: Add lanthanum copper alloy and samarium copper alloy and smelt Pure iron, ferroboron and praseodymium-neodymium are vacuum smelted, then mixed with lanthanum-copper alloy and samarium-copper alloy for smelting and rapid solidification, and then subjected to hydrogen explosion treatment and helium gas flow milling to obtain alloy fine powder; S2: Smelting copper-cobalt alloy and copper-gallium alloy and pressing them into shape The copper-cobalt alloy and the copper-gallium alloy are mixed and smelted and spun into a rapid quenching strip, ball-milled into powder, fully mixed with the above alloy fine powder and nano-aluminum powder, and then oriented pressed and cold isostatically pressed to obtain a magnet compact; S3: Vacuum sintering and double tempering heat treatment The magnet green compact is subjected to vacuum sintering, cooled to room temperature in a furnace, and then subjected to two tempering heat treatments at different temperatures to obtain a magnet green compact; S4: Mixing and melting copper-neodymium alloy and nickel-copper alloy to prepare nickel-containing alloy powder The copper-neodymium alloy and the nickel-copper alloy are mixed and vacuum-melted, and after cooling, the mixture is placed in a ball mill and ball-milled into powder to obtain nickel-containing alloy powder; S5: Magnetron sputtering of nickel-containing alloy powder and high temperature diffusion treatment The nickel-containing alloy powder is sputtered onto the surface of the magnetic blank obtained in step S3 by using an ultra-high vacuum three-chamber magnetron sputtering system, and after high-temperature diffusion treatment and tempering heat treatment, the powder is cooled to room temperature with the furnace to obtain a neodymium iron boron magnet; Step S1 specifically includes the following steps: S1.1: Place pure iron, ferroboron and praseodymium-neodymium in a vacuum melting and quenching furnace and perform vacuum melting for 1-2 hours to obtain an alloy ingot; S1.2: adding the alloy ingot, lanthanum copper alloy, samarium copper alloy and cobalt iron alloy into a vacuum quick-setting furnace, smelting for 1-2 hours, and quick-setting and cooling to room temperature to obtain a 0.2-0.4 mm alloy quick-setting strip, wherein the operation speed of the quick-setting and cooling device is 1.5-2 m / s; S1.3: adding the alloy quick-solidification belt into a hydrogen crushing furnace and performing hydrogen explosion crushing to obtain alloy coarse powder with a particle size of 0.1-0.3 mm; S1.4: placing the alloy coarse powder in a jet mill, and performing a jet milling process in a helium environment to obtain alloy fine powder with a particle size of 0.8-1.2 μm; Step S2 specifically includes the following steps: S2.1: Add the copper-cobalt alloy and the copper-gallium alloy into a vacuum arc furnace, and repeatedly melt them 4-5 times, each time for 40-50 minutes, to obtain an alloy ingot; S2.2: The alloy ingot is placed in a vacuum quenching belt spinning device, and spun at a speed of 6-8 m / s into a quenching belt with a width of 10-12 mm and a thickness of 0.2-0.3 mm, and then placed in a ball mill for ball milling to obtain an alloy powder with a particle size of 4-5 μm; S2.3: Add the alloy fine powder obtained in step S1.4, the alloy powder and nano aluminum powder into a mixer at a mass ratio of 450-500:3-5:1, and mix for 4-5 hours to obtain mixed magnetic powder; S2.4: Under the protection of nitrogen, the mixed magnetic powder is added into a pressing mold, and then placed into a molding press, and then pressed and molded under the condition of magnetic field orientation to obtain a magnet green body; S2.5: placing the magnet green body in a static press, and performing cold isostatic pressing at a pressure of 220-230 MPa to obtain a magnet green body; Step S4 specifically includes the following steps: S4.1: placing the copper-neodymium alloy and the nickel-copper alloy in a vacuum arc furnace, vacuum melting for 1-2 hours, and cooling the furnace to room temperature to obtain a nickel-containing ingot; S4.2: placing the nickel-containing ingot in a ball mill and milling for 2-3 hours to obtain a nickel-containing alloy powder with a particle size of 1.5-2 μm; The alloy quick-setting belt comprises: 15-16wt% Nd, 5-6wt% B, 5-6wt% Pr, 8-12wt% Cu, 0.05-0.1wt% La, 0.05-0.1wt% Sm, and the balance is Fe and unavoidable impurities; The alloy ingot includes 15-20wt% Co and 8-12wt% Ga, and the balance is Cu; The nickel-containing alloy powder includes 40-50 wt % Nd and 35-45 wt % Ni, with the balance being Cu.

2. The process for preparing a rare earth element-added NdFeB magnet according to claim 1, characterized in that: Step S3 specifically includes the following steps: S3.1: placing the magnet compact obtained in step S2.5 in a vacuum sintering furnace, sintering at a temperature of 1000-1200°C for 4-5h, and cooling to room temperature to obtain a sintered compact; S3.2: placing the sintered green body in a tempering furnace, heating it to 800-900°C at a rate of 10-20°C / min, and then keeping it at that temperature for 2-3h to perform a tempering heat treatment to obtain a primary heat-treated green body; S3.3: Adjust the heating rate of the tempering furnace to 5-10°C / min, heat the above-mentioned primary heat-treated green body to 450-500°C, then keep it warm for 2-3h, and perform secondary tempering heat treatment to obtain a magnetic green body.

3. The process for preparing a rare earth element-added NdFeB magnet according to claim 2, characterized in that: Step S5 specifically includes the following steps: S5.1: polishing the surface of the magnetic body obtained in step S3.3 with sandpaper, washing with deionized water, ultrasonically treating in ethanol for 15-20 minutes, and then vacuum drying to obtain a surface pretreated body; S5.2: Set the vacuum degree of the ultra-high vacuum three-chamber magnetron sputtering system to (8-10)×10 -5 Pa, argon gas flow rate of 40-50sccm, coating working pressure of 1-1.3Pa and sputtering power of 100-120W; S5.3: placing the surface pretreated body in an ultra-high vacuum three-chamber magnetron sputtering system, and sputtering the nickel-containing alloy powder obtained in step S4.2 on the upper and lower surfaces of the surface pretreated body to form an alloy coating with a thickness of 2.8-3 μm, thereby obtaining a coated body; S5.4: Wrap the coated body with molybdenum foil, place it in a vacuum tube furnace, heat it to 800-900°C at a rate of 5-10°C / min, and then keep it at that temperature for 5-6h to perform high temperature diffusion treatment to obtain a precursor magnet; S5.5: When the precursor magnet is cooled to 70-80°C, the temperature is raised to 450-550°C and kept at this temperature for 2-3 hours for tempering heat treatment. After the precursor magnet is cooled to room temperature in the furnace, a NdFeB magnet is obtained.

4. A neodymium iron boron magnet with added rare earth elements, characterized in that: It is prepared by the preparation process of a rare earth element-added neodymium iron boron magnet as described in any one of claims 1 to 3.

Citation Information

Patent Citations

  • Preparation method for neodymium-iron-boron magnet capable of improving utilization rate of rare earth elements

    CN112750614A

  • Low (zero) heavy rare earth and high coercivity sintered neodymium-iron-boron magnet and preparation method thereof

    CN113782289A

  • Neodymium-iron-boron magnetic material and preparation method thereof

    CN115472372A

  • Neodymium Iron Boron Magnet and Preparation Method Thereof

    US20170178778A1