Ultra-low temperature lithium-ion battery electrolyte

The ultra-low temperature lithium-ion battery electrolyte improves battery performance in extreme cold environments by using specific components and solvents, ensuring stable capacity and expanded application.

CN118589038BActive Publication Date: 2024-12-06XINYUANXINAN TECH (BEIJING) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410844661.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-12-06
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

Lithium-ion batteries perform inadequately in extreme low-temperature environments, limiting their application in outdoor and high-cold areas.

Method used

An ultra-low temperature lithium-ion battery electrolyte is developed, comprising specific components and solvents, including film-forming additives and lithium salts, which enhance performance under ultra-low temperatures.

Benefits of technology

The electrolyte maintains excellent battery capacity and stability at ultra-low temperatures, expanding the battery's application scope in extreme climatic conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004915373170000021
    Figure BDA0004915373170000021
  • Figure BDA0004915373170000041
    Figure BDA0004915373170000041
  • Figure BDA0004915373170000051
    Figure BDA0004915373170000051
Patent Text Reader

Abstract

The invention discloses an ultra-low temperature lithium ion battery electrolyte, belonging to the technical field of lithium ion batteries. The electrolyte comprises lithium hexafluorophosphate, lithium difluorooxalate borate, film-forming additive A, film-forming additive B, magnesium trifluoromethanesulfonate, N,N-dimethyltrifluoroacetamide, non-aqueous organic solvent, and vinyl sulfite; 4-vinyl pyridine, anhydrous methanol, and chloropropane are used to prepare film-forming additive A; benzoic acid, 2,5-dimethoxybenzene-1,4-diformaldehyde, benzoic anhydride, and 2,4,6-trimethylpyridine are used to prepare film-forming additive B; the lithium ion battery electrolyte prepared by compounding the above components still has good performance even under ultra-low temperature conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion batteries, and in particular relates to an ultra-low temperature lithium ion battery electrolyte. Background Art

[0002] In today's era, lithium-ion batteries have undisputedly become the best energy choice for various portable consumer electronic devices. From the most common mobile phones, tablets and laptops, to sophisticated digital cameras, to convenient power tools and entertainment toys, lithium-ion batteries have won wide applications with their excellent durability, high specific energy and excellent high power output capabilities. This battery technology is not limited to consumer electronics. In recent years, lithium-ion batteries have gradually penetrated into the automotive industry, especially in the fields of hybrid vehicles and pure electric vehicles. As a key power component, it has injected strong impetus into the innovation of the automotive industry. At the same time, the application potential of lithium-ion batteries in the fields of unmanned aircraft, automated unmanned equipment, and increasingly intelligent products cannot be ignored. Although lithium-ion batteries have many advantages, their performance in special application environments is still insufficient. Especially in extreme low-temperature use scenarios such as outdoor and high-cold areas, the performance of lithium-ion batteries will be significantly affected and cannot achieve the expected results. In view of this problem, it is necessary for us to develop a lithium-ion battery that can still maintain excellent performance under ultra-low temperature conditions. Such batteries will be more adaptable to changing environmental demands and further broaden the application scope of lithium-ion batteries, thereby providing more stable and reliable energy guarantees for various devices, especially for those devices working in extreme climatic conditions. The advent of such batteries will be of great significance. Summary of the invention

[0003] The purpose of the present invention is to provide an ultra-low temperature lithium-ion battery electrolyte to improve the performance of the lithium-ion battery under ultra-low temperature conditions.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] An ultra-low temperature lithium-ion battery electrolyte comprises the following components in parts by weight:

[0006]

[0007] The preparation method of the film-forming additive A comprises the following steps:

[0008] Mix 4-vinylpyridine and anhydrous methanol, stir for 10-15 minutes, add chloropropane, reflux and stir at 40°C for 50-60 hours, transfer to anhydrous ether for precipitation, filter, wash and dry the solid phase to obtain film-forming additive A;

[0009] The preparation method of the film-forming additive B comprises the following steps:

[0010] In a nitrogen atmosphere, benzoic acid, 2,5-dimethoxybenzene-1,4-dicarboxaldehyde, benzoic anhydride, and 2,4,6-trimethylpyridine are mixed, transferred to a stirring kettle, stirred for 1-2 hours, vacuum-sealed, heated at 180° C. for 20-30 hours, cooled, washed, dried, crushed, and ground to obtain the film-forming additive B;

[0011] The film-forming additive C is magnesium trifluoromethanesulfonate.

[0012] As a preferred technical solution of the present invention, the non-aqueous organic solvent includes ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate.

[0013] As a preferred technical solution of the present invention, the volume ratio of ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 4-5:1-1.2:3.4-3.6:2.2-2.4.

[0014] As a preferred technical solution of the present invention, the mass ratio of 4-vinylpyridine, anhydrous methanol and chloropropane is 1-1.2:5-6:10-12.

[0015] As a preferred technical solution of the present invention, the dosage ratio of benzoic acid, 2,5-dimethoxybenzene-1,4-dicarbaldehyde, benzoic anhydride and 2,4,6-trimethylpyridine is 85-95 mg: 0.6-0.7 mmol: 150-160 mg: 60-70 μL.

[0016] As a preferred technical solution of the present invention, lithium hexafluorophosphate was purchased from Shanghai Lanrun Chemical Co., Ltd.; lithium difluorooxalatoborate was purchased from Hubei Bojie Biotechnology Co., Ltd.; N,N-dimethyltrifluoroacetamide was purchased from Tianjin Yichuangcheng Pharmaceutical Technology Co., Ltd.; ethylene sulfite was purchased from Nantong Runfeng Petrochemical Co., Ltd.; ethyl trifluoroacetate was purchased from Shanghai Bangcheng Chemical Co., Ltd.; propylene carbonate and dimethyl carbonate were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; ethyl methyl carbonate was purchased from Hubei Lidu New Materials Technology Co., Ltd.; 2,5-dimethoxybenzene-1,4-dicarboxaldehyde was purchased from Jilin Shengchuang Biotechnology Co., Ltd.; and 2,4,6-trimethylpyridine was purchased from Shanghai Tuoke Chemical Technology Co., Ltd.

[0017] Beneficial effects of the present invention:

[0018] The ultra-low temperature lithium ion battery electrolyte disclosed in the present invention is prepared by compounding two lithium salts, lithium hexafluorophosphate and lithium difluorooxalatoborate, which are dissolved in an organic solvent consisting of ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate. By compounding film-forming additives, the components work synergistically as a whole to improve the capacity achievement rate of the battery under ultra-low temperature conditions and the stability at low temperatures. DETAILED DESCRIPTION

[0019] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0020] Example 1

[0021] An ultra-low temperature lithium-ion battery electrolyte comprises the following components in parts by weight:

[0022]

[0023] The preparation method of the film-forming additive A comprises the following steps:

[0024] 4-vinylpyridine and anhydrous methanol were mixed, stirred for 10 minutes, chloropropane was added, refluxed and stirred at 40°C for 50 hours, transferred to anhydrous ether for precipitation, filtered, the solid phase was washed, and dried to obtain a film-forming additive A; the mass ratio of 4-vinylpyridine, anhydrous methanol, and chloropropane was 1:5:10;

[0025] The preparation method of the film-forming additive B comprises the following steps:

[0026] In a nitrogen atmosphere, benzoic acid, 2,5-dimethoxybenzene-1,4-dicarboxaldehyde, benzoic anhydride, and 2,4,6-trimethylpyridine were mixed, transferred to a stirring kettle, stirred for 1 hour, vacuum sealed, heated at 180° C. for 20 hours, cooled, washed, dried, crushed, and ground to obtain the film-forming additive B; the dosage ratio of benzoic acid, 2,5-dimethoxybenzene-1,4-dicarboxaldehyde, benzoic anhydride, and 2,4,6-trimethylpyridine was 85 mg: 0.6 mmol: 150 mg: 60 μL;

[0027] The film-forming additive C is magnesium trifluoromethanesulfonate;

[0028] The non-aqueous organic solvent includes ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate; the volume ratio of ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 4:1:3.4:2.2.

[0029] Example 2

[0030] An ultra-low temperature lithium-ion battery electrolyte comprises the following components in parts by weight:

[0031]

[0032] The preparation method of the film-forming additive A comprises the following steps:

[0033] 4-vinylpyridine and anhydrous methanol were mixed, stirred for 12 minutes, chloropropane was added, refluxed and stirred at 40°C for 52 hours, transferred to anhydrous ether for precipitation, filtered, the solid phase was washed, and dried to obtain a film-forming additive A; the mass ratio of 4-vinylpyridine, anhydrous methanol, and chloropropane was 1.05:5.3:10.5;

[0034] The preparation method of the film-forming additive B comprises the following steps:

[0035] In a nitrogen atmosphere, benzoic acid, 2,5-dimethoxybenzene-1,4-dicarboxaldehyde, benzoic anhydride, and 2,4,6-trimethylpyridine were mixed, transferred to a stirring kettle, stirred for 1.3 hours, vacuum sealed, heated at 180° C. for 23 hours, cooled, washed, dried, crushed, and ground to obtain the film-forming additive B; the dosage ratio of benzoic acid, 2,5-dimethoxybenzene-1,4-dicarboxaldehyde, benzoic anhydride, and 2,4,6-trimethylpyridine was 88 mg: 0.63 mmol: 153 mg: 63 μL;

[0036] The film-forming additive C is magnesium trifluoromethanesulfonate;

[0037] The non-aqueous organic solvent includes ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate; the volume ratio of ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 4.3:1.05:3.45:2.25.

[0038] Example 3

[0039] An ultra-low temperature lithium-ion battery electrolyte comprises the following components in parts by weight:

[0040]

[0041] The preparation method of the film-forming additive A comprises the following steps:

[0042] 4-vinylpyridine and anhydrous methanol were mixed, stirred for 13 minutes, chloropropane was added, refluxed and stirred at 40°C for 55 hours, transferred to anhydrous ether for precipitation, filtered, the solid phase was washed, and dried to obtain a film-forming additive A; the mass ratio of 4-vinylpyridine, anhydrous methanol, and chloropropane was 1.1:5.5:11;

[0043] The preparation method of the film-forming additive B comprises the following steps:

[0044] In a nitrogen atmosphere, benzoic acid, 2,5-dimethoxybenzene-1,4-dicarboxaldehyde, benzoic anhydride, and 2,4,6-trimethylpyridine were mixed, transferred to a stirring kettle, stirred for 1.5 hours, vacuum sealed, heated at 180° C. for 25 hours, cooled, washed, dried, crushed, and ground to obtain the film-forming additive B; the dosage ratio of benzoic acid, 2,5-dimethoxybenzene-1,4-dicarboxaldehyde, benzoic anhydride, and 2,4,6-trimethylpyridine was 90 mg: 0.65 mmol: 155 mg: 65 μL;

[0045] The film-forming additive C is magnesium trifluoromethanesulfonate;

[0046] The non-aqueous organic solvent includes ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate; the volume ratio of ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 4.5:1.1:3.5:2.3.

[0047] Example 4

[0048] An ultra-low temperature lithium-ion battery electrolyte comprises the following components in parts by weight:

[0049]

[0050] The preparation method of the film-forming additive A comprises the following steps:

[0051] 4-vinylpyridine and anhydrous methanol were mixed, stirred for 14 minutes, chloropropane was added, refluxed and stirred at 40°C for 58 hours, transferred to anhydrous ether for precipitation, filtered, the solid phase was washed, and dried to obtain a film-forming additive A; the mass ratio of 4-vinylpyridine, anhydrous methanol, and chloropropane was 1.15:5.8:11.5;

[0052] The preparation method of the film-forming additive B comprises the following steps:

[0053] In a nitrogen atmosphere, benzoic acid, 2,5-dimethoxybenzene-1,4-dicarboxaldehyde, benzoic anhydride, and 2,4,6-trimethylpyridine were mixed, transferred to a stirring kettle, stirred for 1-2 hours, vacuum sealed, heated at 180°C for 28 hours, cooled, washed, dried, crushed, and ground to obtain the film-forming additive B; the dosage ratio of benzoic acid, 2,5-dimethoxybenzene-1,4-dicarboxaldehyde, benzoic anhydride, and 2,4,6-trimethylpyridine was 92 mg: 0.68 mmol: 158 mg: 68 μL;

[0054] The film-forming additive C is magnesium trifluoromethanesulfonate;

[0055] The non-aqueous organic solvent includes ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate; the volume ratio of ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 4.8:1.15:3.55:2.35.

[0056] Example 5

[0057] An ultra-low temperature lithium-ion battery electrolyte comprises the following components in parts by weight:

[0058]

[0059] The preparation method of the film-forming additive A comprises the following steps:

[0060] 4-vinylpyridine and anhydrous methanol were mixed, stirred for 15 minutes, chloropropane was added, refluxed and stirred at 40°C for 60 hours, transferred to anhydrous ether for precipitation, filtered, the solid phase was washed, and dried to obtain a film-forming additive A; the mass ratio of 4-vinylpyridine, anhydrous methanol, and chloropropane was 1.2:6:12;

[0061] The preparation method of the film-forming additive B comprises the following steps:

[0062] In a nitrogen atmosphere, benzoic acid, 2,5-dimethoxybenzene-1,4-dicarboxaldehyde, benzoic anhydride, and 2,4,6-trimethylpyridine were mixed, transferred to a stirring kettle, stirred for 2 hours, vacuum sealed, heated at 180° C. for 30 hours, cooled, washed, dried, crushed, and ground to obtain the film-forming additive B; the dosage ratio of benzoic acid, 2,5-dimethoxybenzene-1,4-dicarboxaldehyde, benzoic anhydride, and 2,4,6-trimethylpyridine was 95 mg: 0.7 mmol: 160 mg: 70 μL;

[0063] The film-forming additive C is magnesium trifluoromethanesulfonate;

[0064] The non-aqueous organic solvent includes ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate; the volume ratio of ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 5:1.2:3.6:2.4.

[0065] Comparative Example 1

[0066] The difference from Example 3 is that an ultra-low temperature lithium ion battery electrolyte comprises the following components in parts by weight:

[0067]

[0068] Comparative Example 2

[0069] The difference from Example 3 is that an ultra-low temperature lithium ion battery electrolyte comprises the following components in parts by weight:

[0070]

[0071] Comparative Example 3

[0072] The difference from Example 3 is that an ultra-low temperature lithium ion battery electrolyte comprises the following components in parts by weight:

[0073]

[0074] Comparative Example 4

[0075] The difference from Example 3 is that an ultra-low temperature lithium ion battery electrolyte comprises the following components in parts by weight:

[0076]

[0077] Comparative Example 5

[0078] The difference from Example 3 is that an ultra-low temperature lithium ion battery electrolyte comprises the following components in parts by weight:

[0079]

[0080] Comparative Example 6

[0081] The difference from Example 3 is that an ultra-low temperature lithium ion battery electrolyte comprises the following components in parts by weight:

[0082]

[0083] Comparative Example 7

[0084] The difference from Example 3 is that an ultra-low temperature lithium ion battery electrolyte comprises the following components in parts by weight:

[0085]

[0086]

[0087] Comparative Example 8

[0088] The difference from Example 3 is that the volume ratio of ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate in the non-aqueous organic solvent is 0:5.6:3.5:2.3.

[0089] Comparative Example 9

[0090] The difference from Example 3 is that the volume ratio of ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate in the non-aqueous organic solvent is 4.5:0:4.6:2.3.

[0091] Comparative Example 10

[0092] The difference from Example 3 is that the volume ratio of ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate in the non-aqueous organic solvent is 4.5:4.6:0:2.3.

[0093] Comparative Example 11

[0094] The difference from Example 3 is that the volume ratio of ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate in the non-aqueous organic solvent is 4.5:3.4:3.5:0.

[0095] Performance Testing

[0096] The lithium-ion battery electrolyte prepared in the above Examples 1-5 and Comparative Examples 1-11 was injected into a fully dried graphite / lithium cobalt oxide soft-package battery. After one-sealed static, pre-charged and formed, and two-sealed capacity division, the battery was fully charged at 1C and then discharged at a constant current of 1A at room temperature (20°C) and (-55°C). The battery capacity achievement rate under the ultra-low temperature condition (-55°C) relative to that under the room temperature (20°C) condition was calculated. The experimental data obtained are shown in Table 1.

[0097] Table 1

[0098] Battery capacity achievement rate / % Example 1 84.16 Example 2 84.78 Example 3 85.36 Example 4 84.03 Example 5 83.88 Comparative Example 1 80.76 Comparative Example 2 73.39 Comparative Example 3 69.71 Comparative Example 4 67.34 Comparative Example 5 69.36 Comparative Example 6 79.14 Comparative Example 7 78.33 Comparative Example 8 81.45 Comparative Example 9 80.84 Comparative Example 10 81.24 Comparative Example 11 80.76

[0099] It can be seen from Table 1 that the electrolytes prepared in Examples 1-5 of the present application are used in lithium-ion batteries and still have a relatively stable capacity achievement rate of the lithium battery in an ultra-low temperature environment.

[0100] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. An ultra-low temperature lithium-ion battery electrolyte, characterized in that: It includes the following components by weight: Lithium hexafluorophosphate 10-12 parts by mass 3-5 parts by mass of lithium difluorooxalate borate Film-forming additive A 0.8-1.2 parts by mass Film-forming additive B 2-3 parts by mass Film-forming additive C 0.8-1.2 parts by mass N,N-dimethyltrifluoroacetamide 1.4-1.8 parts by mass 65-75 parts by mass of non-aqueous organic solvent Ethylene sulfite 1-1.5 parts by mass; The preparation method of the film-forming additive A comprises the following steps: Mix 4-vinylpyridine and anhydrous methanol, stir for 10-15 minutes, add chloropropane, reflux and stir at 40°C for 50-60 hours, transfer to anhydrous ether for precipitation, filter, wash and dry the solid phase to obtain film-forming additive A; The preparation method of the film-forming additive B comprises the following steps: In a nitrogen atmosphere, benzoic acid, 2,5-dimethoxybenzene-1,4-dicarboxaldehyde, benzoic anhydride, and 2,4,6-trimethylpyridine are mixed, transferred to a stirring kettle, stirred for 1-2 hours, vacuum-sealed, heated at 180° C. for 20-30 hours, cooled, washed, dried, crushed, and ground to obtain the film-forming additive B; The film-forming additive C is magnesium trifluoromethanesulfonate; The non-aqueous organic solvent includes ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate; The volume ratio of ethyl trifluoroacetate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 4-5:1-1.2:3.4-3.6:2.2-2.4; The mass ratio of 4-vinylpyridine, anhydrous methanol and chloropropane is 1-1.2:5-6:10-12; The dosage ratio of the benzoic acid, 2,5-dimethoxybenzene-1,4-dicarbaldehyde, benzoic anhydride, and 2,4,6-trimethylpyridine is 85-95 mg: 0.6-0.7 mmol: 150-160 mg: 60-70 μL; The operating temperature of the ultra-low temperature lithium-ion battery electrolyte is -55°C.