Method and use of preparing monolithic ozone catalyst using sludge dry powder as raw material
By preparing an integrated ozone catalyst in dry sludge powder, the porous structure of the ZnAl-LDH composite material is used to improve the ozone decomposition efficiency, solve the explosion hazard of dry sludge powder and the problem of ozone tail gas treatment, and achieve resource utilization and efficient ozone. Remove.
Patent Information
- Application Number
- CN202411090314.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-08-09
AI Technical Summary
Municipal sludge dry powder has the risk of explosion, and its use as fertilizer or soil conditioner may affect the ecological balance of the soil. How to utilize resources and treat ozone exhaust has become a problem.
The monolithic ozone catalyst is prepared using dry sludge powder as the carrier, and the ZnAl-LDH composite material is prepared by co-precipitation method, kneading, pre-pressing, granulating, tableting and calcining to form a porous columnar catalyst to increase the specific surface area and activity of the catalyst.
It effectively solves the dust explosion problem of sludge dry powder, realizes resource utilization, significantly improves ozone decomposition efficiency and catalyst stability, and extends the maintenance time of ozone removal rate.
Smart Images

Figure CN118594524B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ozone treatment, and in particular to a method for preparing an integral ozone catalyst using sludge dry powder as a raw material and a use thereof. Background Art
[0002] Ozone catalytic decomposition technology is a process that uses catalysts to accelerate the decomposition of ozone into oxygen. Compared with non-catalytic decomposition, this technology can significantly improve the efficiency of ozone decomposition and reduce energy consumption. Because of its clean and pollution-free, high decomposition efficiency, simple operation, and low cost, it has become one of the most widely used technologies in ozone decomposition treatment, and has gained more and more favor in the tail gas treatment of sewage treatment plants.
[0003] Currently, ozone is used as a disinfectant in municipal sewage treatment to remove organic matter and pathogens in the water. However, the direct discharge of water or gas containing ozone into the environment is strictly controlled. Because ozone itself has potential hazards to the environment and human body, the treatment of ozone exhaust gas is crucial.
[0004] The dry powder after municipal sludge treatment is a solid powder that is easy to store, transport and use after a series of processes to reduce the moisture content of the sludge produced during sewage treatment. The powder usually contains conditioners and possible deodorant fungicide residues, with a mass ratio of 50-85% of water-containing sludge, 14-40% of conditioners, and 1-10% of deodorant fungicide. It is mainly composed of minerals such as silicon dioxide, calcium oxide, aluminum oxide, and iron oxide. These components come from inorganic particles suspended in sewage and chemicals added during the treatment process. Municipal sludge dry powder, as a product of sludge treatment, has a certain explosion hazard. In addition, the use of dried sludge as fertilizer or soil conditioner may change the physical and chemical properties of the soil, thereby affecting the ecological balance of the soil. Especially during the treatment and storage process, if the dust concentration in the air reaches a certain range, it may cause an explosion when encountering a fire source, so how to use it becomes a key problem. Summary of the invention
[0005] In order to solve the above technical problems, the embodiments of the present invention provide a method and use of preparing an integral ozone catalyst using sludge dry powder as a raw material, so as to realize resource utilization of municipal sludge dry powder and decomposition of ozone tail gas.
[0006] To achieve the above object, the embodiments of the present invention adopt the following technical solutions:
[0007] In one aspect, the present invention provides a method for preparing an integral ozone catalyst using sludge dry powder as a raw material, comprising the following steps:
[0008] A. Prepare Zn(NO3)2·6H2O and Al(NO3)3·6H2O into a first solution, and prepare NaOH and Na2CO3 into a second solution;
[0009] B. Under the condition of stirring in a constant temperature water bath, the second solution in step A is added dropwise to the first solution, and the pH is adjusted to 10-11, and the ZnAl-LDH composite material is obtained by ultrasonic oscillation, aging, centrifugation, washing and drying;
[0010] C. After drying, crushing and sieving the sludge, kneading, pre-pressing, granulating, drying and tableting with the ZnAl-LDH composite material obtained in step B, and finally calcining to obtain an integral ozone catalyst.
[0011] In some embodiments, in step A, the mass ratio of Zn(NO3)2·6H2O to Al(NO3)3·6H2O is (1-15):(1-15).
[0012] In some embodiments, in step A, the mass ratio of NaOH to Na2CO3 is (0.5-3): (0.5-3).
[0013] In some embodiments, in step B, the temperature of the constant temperature water bath is 60°C.
[0014] In some embodiments, in step C, the sludge drying temperature is 110° C. and the sludge sieving mesh number is 200 mesh.
[0015] In some embodiments, in step C, the amount of the ZnAl-LDH composite material added is 1-5% of the sludge mass.
[0016] In some embodiments, in step C, the kneading time is 40-100 min, and the water content is controlled at 10-15%.
[0017] In some embodiments, in step C, the heating rate during calcination is 5°C / min-15°C / min, until the temperature reaches 80°C-125°C, and the temperature is kept for 2h-6h.
[0018] In another aspect, the present invention provides a use of the integral ozone catalyst prepared by the above method in ozone decomposition.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The present invention uses municipal sludge dry powder as a carrier to prepare an integral ozone catalyst for ozone decomposition, uses a coprecipitation method to prepare a ZnAl-LDH composite material as an active component, adds water or a binder to the sludge dry powder, and passes through a kneading device to improve the adhesion and strength of the material and the dispersion between the catalysts after kneading; then the strength of the material is further improved through a pre-pressing step; the size of the material is made uniform through a granulating device so as to be better formed, and then the moisture is removed through oven drying, and appropriate parameters are adjusted through a tableting device to obtain a formed columnar ozone decomposition catalyst, and finally calcined in a nitrogen atmosphere in a tubular furnace to increase the specific surface area of the ozone decomposition catalyst, making it a porous material, which is helpful to improve the activity. Thus, the dust explosion and resource utilization problems of municipal sludge dry powder are effectively solved. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a curve diagram of ozone removal rate of the monolithic ozone catalyst prepared in Example 1 of the present invention and Comparative Example 1;
[0022] Figure 2 It is a curve diagram of ozone removal rate of the monolithic ozone catalyst prepared in Example 2 of the present invention and Comparative Example 2;
[0023] Figure 3 This is a physical picture of the integral ozone catalyst prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0024] The following will be combined with the accompanying drawings to clearly and completely describe the technical solutions in some embodiments of the present disclosure. Obviously, the described embodiments are only part of the embodiments of the present disclosure, rather than all the embodiments. Based on the embodiments provided by the present disclosure, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present disclosure.
[0025] In order to realize the recycling of sludge and the decomposition of ozone, the method of the present invention is further described through specific examples. The following example uses dry powder of municipal sludge as a carrier to prepare an integral ozone catalyst. The specific steps are as follows:
[0026] (1) Dissolve 1-15 g Zn(NO3)2·6H2O and 1-15 g Al(NO3)3·6H2O in 20-50 mL deionized water to prepare solution A.
[0027] (2) Dissolve 0.5-3 g NaOH and 0.5-3 g Na2CO3 in 20-50 mL deionized water to obtain solution B;
[0028] (3) While stirring in a 60°C constant temperature water bath, slowly add solution A to solution B at a concentration of 1 mol·L-1 The pH was adjusted with NaOH solution to maintain the pH at 10-11. After the addition was completed, the reaction was stirred at 60°C for 1 hour, ultrasonically vibrated for 30 minutes, and aged for 24 hours. The aging was divided into two stages: constant temperature water bath oscillation aging for 6 hours and room temperature static aging for 18 hours. Centrifugation, washing to neutrality, drying, and grinding were performed to obtain the ZnAl-LDH composite material;
[0029] (4) The dry powder after municipal sludge treatment is placed in an oven and dried at 110°C. After drying, it is crushed and passed through a 200-mesh sieve;
[0030] (5) Add 1% to 5% by weight of the catalytic active component ZnAl-LDH composite material to the dry powder after municipal sludge treatment and mix them evenly to achieve the purpose of dispersion;
[0031] (6) Weigh 1-5 kg of the sludge dry powder mixed with the ZnAl-LDH composite material and add it to the kneader. Control the kneading time to 40-100 minutes and adjust the water content to 10%-15%. According to the different properties of different materials, 1%-5% of the binder needs to be added to facilitate the overall construction.
[0032] (7) Pre-pressing the kneaded dry powder using a pre-pressing device, and controlling the speed of the pre-pressing machine to 60r / min-100r / min and the distance between the outer diameters of the bearings to 5mm-15mm so that the dry powder is rolled out in a flake shape;
[0033] (8) Granulating the pre-pressed flaky dry powder using a granulating device, wherein the diameter of the granulated object after granulation is 4 mm to 8 mm; then placing the granulated granules in an oven and drying them at a temperature of 60 to 120° C.;
[0034] (9) The dried granules are pressed into cylindrical tablets using a tabletting device. The production volume is controlled by adjusting the stepping speed of the tabletting gear to 60 r / min-100 r / min. The strength of the monolithic cylindrical ozone decomposition catalyst is controlled by controlling the gear ejector pin spacing to 2 mm-5 mm. Columnar products with a height of 2 mm-5 mm and a diameter of 3 mm-6 mm with different ejector pin widths are obtained.
[0035] (10) The columnar material is placed in a N2 atmosphere tubular furnace for calcination at a heating rate of 5°C / min-15°C / min until the temperature reaches 80°C-125°C, and the temperature is kept for 2-6 hours. Finally, the columnar material is naturally cooled to room temperature to obtain an integral ozone catalyst.
[0036] Example 1
[0037] (1) Dissolve 3.3 g Zn(NO3)2·6H2O and 4.2 g Al(NO3)3·6H2O in 20 mL deionized water to prepare solution A.
[0038] (2) Dissolve 1.8 g NaOH and 1.4 g Na2CO3 in 20 mL deionized water to obtain solution B.
[0039] (3) While stirring in a 60°C constant temperature water bath, slowly add solution A to solution B at a concentration of 1 mol·L -1 The pH value was adjusted by adding NaOH solution to maintain the pH value at 10-11. After the addition was completed, the reaction was stirred at 60°C for 1 hour, ultrasonically vibrated for 30 minutes, and aged for 24 hours. The aging was divided into two stages: constant temperature water bath oscillation aging for 6 hours and room temperature static aging for 18 hours. Centrifugation, washing to neutrality, drying, and grinding were performed to obtain ZnAl-LDH composite materials;
[0040] (4) The dry powder after municipal sludge treatment is placed in an oven and dried at 110°C. After drying, it is crushed and passed through a 200-mesh sieve;
[0041] (5) Add 3% by weight of the catalytic active component ZnAl-LDH composite material to the dry powder after municipal sludge treatment and mix them evenly to achieve the purpose of dispersion;
[0042] (6) Weigh 3 kg of the sludge dry powder mixed with the ZnAl-LDH composite material and add it into the kneader. The kneading time is controlled to 60 minutes and the water content is adjusted to 12%;
[0043] (7) pre-pressing the kneaded dry powder using a pre-pressing device, and controlling the speed of the pre-pressing machine to 60r / min and the distance between the outer diameters of the bearings to 5mm so that the dry powder is rolled out in a sheet shape;
[0044] (8) granulating the pre-pressed flaky dry powder using a granulating device, wherein the diameter of the granulated object after granulation is 4 mm; then placing the granulated granules in an oven and drying them at a temperature of 100° C.;
[0045] (9) The dried granules are pressed into cylindrical tablets using a tabletting device. The production volume is controlled by adjusting the stepping speed of the tabletting gear to 60 r / min. The strength of the monolithic cylindrical ozone decomposition catalyst is controlled by controlling the gear ejector pin spacing to 5 mm. Columnar products with a height of 5 mm and a diameter of 3 mm with different ejector pin widths are obtained.
[0046] (10) The columnar material is placed in a N2 atmosphere tubular furnace for calcination at a heating rate of 5°C / min until the temperature reaches 100°C, the temperature is kept for 4 hours, and finally cooled naturally to room temperature to obtain an integral ozone catalyst, such as Figure 3 Shown is a physical picture of the integral ozone catalyst obtained in Example 1.
[0047] After testing, the compressive strength of the monolithic ozone catalyst of Example 1 is 150N / cm 2 , bulk density is 0.8g / cm 2 The integral ozone catalyst of Example 1 is filled in the decomposition device, and the ozone generator is used as the gas source. The ozone concentration is 40 ppm, the gas flow rate is 2 L / min, the air humidity is 90%, and the temperature is room temperature 25°C.
[0048] Example 2
[0049] (1) Take 3.3 g Zn(NO3)2·6H2O and 4.2 g Al(NO3)3·6H2O and dissolve them in 20 mL deionized water to prepare solution A.
[0050] (2) Dissolve 1.8 g NaOH and 1.4 g Na2CO3 in 20 mL deionized water to obtain solution B.
[0051] (3) While stirring in a 60°C constant temperature water bath, slowly add solution A to solution B at a concentration of 1 mol·L -1 The pH value was adjusted by adding NaOH solution to maintain the pH value at 10-11. After the addition was completed, the reaction was stirred at 60°C for 1 hour, ultrasonically vibrated for 30 minutes, and aged for 24 hours. The aging was divided into two stages: constant temperature water bath oscillation aging for 6 hours and room temperature static aging for 18 hours. Centrifugation, washing to neutrality, drying, and grinding were performed to obtain ZnAl-LDH composite materials;
[0052] (4) The dry powder after municipal sludge treatment is placed in an oven and dried at 110°C. After drying, it is crushed and passed through a 200-mesh sieve;
[0053] (5) After adding 4% by weight of the catalytic active component ZnAl-LDH composite material to the dry powder after municipal sludge treatment, the mixture was evenly mixed to achieve the purpose of dispersion;
[0054] (6) Weigh 2 kg of the sludge dry powder mixed with the ZnAl-LDH composite material and add it into the kneader. The kneading time is controlled to 80 minutes and the water content is adjusted to 15%;
[0055] (7) pre-pressing the kneaded dry powder using a pre-pressing device, and controlling the speed of the pre-pressing machine to 80 r / min and the distance between the outer diameters of the bearings to 4 mm so that the dry powder is rolled out in a sheet form;
[0056] (8) Granulating the pre-pressed flaky dry powder using a granulating device, wherein the diameter of the granulated object after granulation is 6 mm; then placing the granulated granules in an oven and drying them at 60° C.;
[0057] (9) The dried granules are pressed into cylindrical tablets using a tabletting device. The production volume is controlled by adjusting the stepping speed of the tabletting gear to 80 r / min. The strength of the monolithic cylindrical ozone decomposition catalyst is controlled by controlling the gear ejector pin spacing to 4 mm. Columnar products with a height of 4 mm and a diameter of 5 mm with different ejector pin widths are obtained.
[0058] (10) The columnar material was placed in a N2 atmosphere tubular furnace for calcination at a heating rate of 10°C / min until the temperature reached 102°C and the temperature was kept at this temperature for 5 hours. Finally, the columnar material was naturally cooled to room temperature to obtain an integral ozone catalyst.
[0059] After testing, the compressive strength of the integral ozone catalyst of Example 2 is 160N / cm 2 , bulk density is 0.9g / cm 2 The integral ozone catalyst of Example 2 is filled in the decomposition device, and the ozone generator is used as the gas source. The ozone concentration is 40 ppm, the gas flow rate is 2 L / min, the air humidity is 90%, and the temperature is room temperature 25°C.
[0060] Comparative Example 1
[0061] (1) Take 3.3 g Zn(NO3)2·6H2O and 4.2 g Al(NO3)3·6H2O and dissolve them in 20 mL deionized water to prepare solution A.
[0062] (2) Dissolve 1.8 g NaOH and 1.4 g Na2CO3 in 20 mL deionized water to obtain solution B.
[0063] (3) While stirring in a 60°C constant temperature water bath, slowly add solution A to solution B at a concentration of 1 mol·L -1 The pH was adjusted with NaOH solution to maintain the pH at 10-11. After the addition was completed, the reaction was stirred at 60°C for 1 hour, ultrasonically vibrated for 30 minutes, and aged for 24 hours. The aging was divided into two stages: constant temperature water bath oscillation aging for 6 hours and room temperature static aging for 18 hours. Centrifugation, washing to neutrality, drying, and grinding to obtain ZnAl-LDH composite material;
[0064] (4) The dry powder after municipal sludge treatment is placed in an oven and dried at 110°C. After drying, it is crushed and passed through a 200-mesh sieve;
[0065] (5) Add 3% by weight of the catalytic active component ZnAl-LDH composite material to the dry powder after municipal sludge treatment and mix them evenly to achieve the purpose of dispersion;
[0066] (6) Weigh 3 kg of the sludge dry powder mixed with the ZnAl-LDH composite material and add it into the kneader. The kneading time is controlled to 60 minutes and the water content is adjusted to 12%;
[0067] (7) pre-pressing the kneaded dry powder using a pre-pressing device, and controlling the speed of the pre-pressing machine to 60r / min and the distance between the outer diameters of the bearings to 5mm so that the dry powder is rolled out in a sheet shape;
[0068] (8) The pre-pressed flaky dry powder is granulated using a granulation device, and the diameter of the granulated object after granulation is 4 mm; the granulated granules are then placed in an oven and dried at 100° C. to obtain an integral ozone catalyst.
[0069] After testing, the stability efficiency of Example 1 is 60% higher than that of Comparative Example 1. Figure 1 It can be seen that the ozone removal rate of the integral ozone catalyst of Example 1 reached 100% through the ozone analyzer and was maintained for 6 days, while that of Comparative Example 1 could only be maintained for 1 day. Comparative Example 1 maintained an ozone removal rate of 100% for 1 day, and then the removal rate dropped to 40% as time went on.
[0070] Comparative Example 2
[0071] (1) Place the dry powder after municipal sludge treatment in an oven and dry it at 110°C. After drying, crush it and pass it through a 200-mesh sieve.
[0072] (2) Weigh 2 kg of dry powder from the municipal sludge after screening and add it into the kneading machine. Control the kneading time to 80 minutes and adjust the water content to 15%;
[0073] (3) Pre-pressing the kneaded dry powder using a pre-pressing device, and controlling the speed of the pre-pressing machine (80 r / min) and the distance between the outer diameters of the bearings (4 mm) so that the dry powder is rolled out in a flake shape;
[0074] (4) The pre-pressed flaky dry powder is granulated using a granulating device, and the diameter of the granulated object after granulation is 6 mm; the granulated granules are then placed in an oven and dried at 60°C.
[0075] (5) The dried granules were pressed into cylindrical tablets using a tabletting device. The production volume was controlled by adjusting the stepping speed of the tabletting gear to 80 r / min, and the strength of the monolithic cylindrical ozone decomposition catalyst was controlled by controlling the gear ejector pin spacing to 4 mm. Columnar products with a height of 4 mm and a diameter of 5 mm with different ejector pin widths were obtained.
[0076] (6) The columnar material is placed in a N2 atmosphere tubular furnace for calcination at a heating rate of 10°C / min until the temperature reaches 102°C and the temperature is kept at this temperature for 5 hours. Finally, the columnar material is naturally cooled to room temperature to obtain an integral ozone catalyst.
[0077] After testing, the stable efficiency of Example 2 is improved by 50% compared with that of Comparative Example 2. Figure 2 It can be seen that the ozone removal rate of the integral ozone catalyst of Example 2 reached 100% through the ozone analyzer and lasted for 6 days, while that of Comparative Example 2 could only last for 1 day. Then, as time went on, the removal rate remained at 50% after 6 days.
[0078] In the description of this specification, specific features, structures, materials or characteristics may be combined in an appropriate manner in any one or more embodiments or examples.
[0079] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing an integral ozone catalyst using sludge dry powder as raw material, characterized in that: The following steps are involved: A. Prepare Zn(NO3)2·6H2O and Al(NO3)3·6H2O into a first solution, and prepare NaOH and Na2CO3 into a second solution; B. Under the condition of stirring in a constant temperature water bath, the second solution in step A is added dropwise to the first solution, and the pH is adjusted to 10-11, and the ZnAl-LDH composite material is obtained by ultrasonic oscillation, aging, centrifugation, washing and drying; C. After drying, crushing and sieving the sludge, kneading, pre-pressing, granulating, drying and tableting with the ZnAl-LDH composite material obtained in step B, and finally calcining to obtain an integral ozone catalyst; in step C, the heating rate during calcination is 5°C / min-15°C / min, until the temperature is raised to 80°C-125°C, and the temperature is kept for 2h-6h, and the calcination is carried out in a nitrogen atmosphere; In step C, the amount of the ZnAl-LDH composite material added is 1-5% of the sludge mass.
2. The preparation method according to claim 1, characterized in that: In step A, the mass ratio of Zn(NO3)2·6H2O to Al(NO3)3·6H2O is (1-15):(1-15).
3. The method according to claim 1, characterized in that In step A, the mass ratio of the NaOH to the Na2CO3 is (0.5-3): (0.5-3), and the mass ratio of the Zn(NO3)2·6H2O to the NaOH is (1-15): (0.5-3).
4. The method according to claim 1, characterized in that: In step B, the temperature of the constant temperature water bath is 60°C.
5. The method according to claim 1, characterized in that In step C, the sludge is dried at a temperature of 110° C. and sieved through a mesh of 200 meshes.
6. The method according to claim 1, characterized in that In step C, the kneading time is 40-100 minutes, and the water content is controlled at 10-15%.
7. Use of the integral ozone catalyst prepared by the method according to any one of claims 1 to 6 in ozone decomposition.