Low expansion antibacterial microcrystalline glassware and preparation method thereof

By adopting low expansion technology and modified chitosan antibacterial coatings in microcrystalline glassware, the problem of unstable antibacterial properties of traditional microcrystalline glassware is solved, and its heat resistance and resistance are improved Impact and antibacterial properties significantly enhance their application value.

CN118598521BActive Publication Date: 2024-11-05CNBM RESEARCH INSTITUTE FOR ADVANCED GLASS MATERIALS GROUP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411087933.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-05
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

Traditional microcrystalline glassware is prone to high cost, unstable antibacterial properties, reduced transmittance and coating peeling after antibacterial treatment, which limits its application areas.

Method used

By preparing low-expanded microcrystalline glassware, the water-based antibacterial coating prepared with strict control of melting and crystallization temperatures and combined with modified chitosan can enhance the antibacterial properties and flexibility of the glassware to prevent the coating from falling off.

Benefits of technology

The heat and impact resistance of glassware has been improved, and the long-term stability and flexibility of antibacterial properties have been enhanced, which has significantly improved its application value in the technical field of glassware.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention discloses a method for preparing low-expansion antibacterial microcrystalline glassware, belonging to the technical field of glassware. The prepared glassware makes the crystal more complete by strictly controlling the temperature of nucleation and crystallization, and the microcrystallization heat treatment can greatly improve the heat resistance and impact resistance of the glassware; the prepared antibacterial coating is a water-based coating, which is environmentally friendly and has high flexibility and strong impact resistance through the selection of monomers; homemade modified chitosan is added to the antibacterial coating, and the modified chitosan has good compatibility with the acrylate matrix, and the various groups in the modified chitosan molecules play a synergistic role, which can significantly enhance the antibacterial property of the glassware and the flexibility of the antibacterial coating, and the performance is stable and not easy to fall off; therefore, the glassware prepared by the present invention belongs to microcrystalline glassware, with complete crystals, good heat resistance and impact resistance, and stable and efficient antibacterial performance, and has important application value in the field of glassware technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of glassware, and in particular, relates to a low-expansion antibacterial microcrystalline glassware and a preparation method thereof. Background Art

[0002] Glass-ceramics is an inorganic non-metallic material with high mechanical strength, good chemical stability and excellent wear resistance. It can be widely used as a functional material and decorative material in different technical fields such as construction, chemical industry, electronics, machinery, etc. However, glass-ceramics have certain limitations in some aspects. Traditional glass-ceramics are easily scratched and worn, which reduces their beauty and service life. People usually apply coatings on glass-ceramics to protect them.

[0003] With the further strengthening of awareness of improving the quality of life and cherishing physical health, the market demand for antibacterial products has skyrocketed, and preparing antibacterial functions on various glassware has become a popular trend.

[0004] Chinese patent CN104192398A antibacterial glassware and its processing method adopt the process scheme of surface silver ion diffusion, adsorption, adhesion → thermal diffusion → aging to prepare an antibacterial layer in high borosilicate glassware, and exert a lasting antibacterial effect by slowly releasing silver ions. However, although silver has excellent antibacterial properties, its cost is relatively high. After the glass is treated with Ag+ antibacterial treatment, Ag+ aggregation will occur on the surface, resulting in yellow block spots on the glass, which seriously affects the optical properties such as transmittance. Not only that, some conventional organic antibacterial agents have poor compatibility with the coating matrix, and will precipitate or even fall off during use, making it difficult to maintain the antibacterial properties of the glassware for a long time, limiting its field of use. Therefore, it is urgent to invent an antibacterial microcrystalline glassware that can solve the above problems to meet the higher demands in the field of glassware technology. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a low-expansion antibacterial microcrystalline glass vessel and a preparation method thereof.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing a low-expansion antibacterial microcrystalline glass vessel comprises the following steps:

[0008] A1. SiO2, Al2O3, Li2O, Na2O, K2O, ZnO, TiO2 and ZrO2 are melted, clarified and homogenized, cooled and pressed into glassware, and cooled and annealed to obtain basic glassware;

[0009] A2. The basic glassware obtained in step A1 is nucleated, re-crystallized, and cooled in the furnace to obtain a low-expansion microcrystalline glassware, and then the antibacterial coating is evenly applied on the inner and outer surfaces of the glassware to obtain a low-expansion antibacterial microcrystalline glassware.

[0010] Further, the glassware includes the following raw materials in percentage by mass: SiO2: 65%-72%, Al2O3: 15%-20%, Li2O: 2.5%-4%, Na2O: 0%-1%, K2O: 0-1%, ZnO: 1%-2.5%, TiO2: 2%-6%, and ZrO2: 0-3%.

[0011] Furthermore, in step A1, the melting temperature is 1550-1650°C.

[0012] Furthermore, the pressing temperature in step A1 is 1350-1400°C.

[0013] Furthermore, in step A2, the nucleation temperature is 750-850° C., and the nucleation time is 1-4 h.

[0014] Furthermore, in step A2, the crystallization temperature is 850-1000° C., and the crystallization time is 4-10 h.

[0015] Furthermore, in step A2, the furnace cooling temperature is below 200°C.

[0016] During the nucleation treatment, the temperature is strictly controlled between 750℃-850℃. Within this temperature range, the crystal nuclei of the basic glassware are relatively complete; during the crystallization treatment, the crystal nuclei grow into complete crystals with better performance; the microcrystallization heat treatment can precipitate a large amount of low-expansion crystalline phases in the basic glass, thereby achieving a low-expansion effect and greatly improving the heat resistance and impact resistance of the glassware.

[0017] Furthermore, the antibacterial coating is prepared by the following steps:

[0018] Butyl acrylate, ethyl acrylate, acrylic acid, sodium dodecyl sulfate (emulsifier), silicone defoamer and water are added into a reactor for emulsification to obtain an emulsion, and then modified chitosan and initiator are added and kept at 70-90°C for 2 hours to initiate a polymerization reaction. After the reaction is completed, an antibacterial coating is obtained.

[0019] Furthermore, the raw materials are calculated in parts by weight as follows: 35-45 parts of butyl acrylate, 40-50 parts of ethyl acrylate, 6-10 parts of acrylic acid, 3-5 parts of sodium dodecyl sulfate, 2-4 parts of silicone defoamer, 80-100 parts of water, 5-15 parts of modified chitosan, and 0.1-0.3 parts of initiator.

[0020] Furthermore, the defoaming agent is a silicone defoaming agent.

[0021] Furthermore, the initiator is a water-soluble initiator.

[0022] The prepared antibacterial coating is a water-based coating, which is not only highly weather-resistant but also environmentally friendly; the raw materials selected are butyl acrylate and ethyl acrylate, both of which are soft monomers, and the prepared water-based coating has high flexibility and strong impact resistance.

[0023] Furthermore, the modified chitosan is prepared by the following steps:

[0024] S1. Add 4-aminopyridine, stearic acid, dicyclohexylcarbodiimide (DCC, dehydrating agent) and pyridine to a three-necked flask equipped with a stirring device, stir and mix well, place in a 45°C water bath, and heat in a water bath for 8 hours. After the reaction is completed, filter, remove the solvent by vacuum distillation, and then purify by column chromatography (the eluent is a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two is 5:1), and remove the eluent by rotary evaporation to obtain intermediate 1; the ratio of 4-aminopyridine, stearic acid, dicyclohexylcarbodiimide and pyridine is 9.4g:28.4g:20.6g:120mL;

[0025] Under the action of a dehydrating agent, 4-aminopyridine and stearic acid undergo an amidation reaction to obtain intermediate 1. The specific reaction process is as follows:

[0026]

[0027] S2. Add intermediate 1 and ether to a three-necked flask equipped with a stirring reflux device, stir and mix evenly, then drop epibromopropane, control the reaction temperature to 68°C, reflux reaction for 8h, and after the reaction is completed, remove part of the solvent by distillation under reduced pressure, and then purify by column chromatography (the eluent is a mixed solvent of petroleum ether / ethyl acetate, the volume ratio of the two is 5:1), remove the eluent by rotary evaporation to obtain intermediate 2; the ratio of the amount of intermediate 1, ether, and epibromopropane is 41.3g:150mL:13.5g;

[0028] Intermediate 1 undergoes quaternization reaction with epibromopropane to obtain intermediate 2; the specific reaction process is as follows:

[0029]

[0030] S3. Mix chitosan, deionized water and isopropanol in a three-necked flask equipped with a stirring device, stir in a water bath at 80°C for 2 h, add sodium hydroxide solution (mass fraction 35%) dropwise, and add intermediate 2, continue stirring and reacting for 48 h, adjust the pH to 7, filter, wash with ethanol and water in turn, and vacuum dry to obtain pre-modified chitosan; the ratio of chitosan, deionized water, isopropanol, and intermediate 2 is 2 g:10 mL:20 mL:8 g;

[0031] The amino group on the chitosan molecule reacts with the epoxy group on the intermediate 2 molecule, and the intermediate 2 is connected with the chitosan to obtain the pre-modified chitosan;

[0032] S4. In a three-necked flask equipped with a stirring device, pre-modified chitosan, N,N-dimethylformamide and isopropanol were mixed, stirred in a 65°C water bath for 1 hour, sodium hydroxide solution (mass fraction 35%) was added to adjust the pH to 9, and allyl chloride was added dropwise. After keeping warm for 1 hour, the reaction was completed, filtered, washed with ethanol and water in turn, and dried to obtain modified chitosan; the ratio of pre-modified chitosan, N,N-dimethylformamide, isopropanol, and allyl chloride was 1g:30mL:10mL:6g;

[0033] The pre-modified chitosan reacts with allyl chloride to introduce a carbon-carbon double bond into the pre-modified chitosan to obtain modified chitosan;

[0034] Chitosan is the only positively charged polymer substance among natural polysaccharides. It has good stability, biofunctionality and antibacterial properties. By modifying chitosan through connecting organic molecular chains, the interfacial effect of chitosan is greatly improved, and the compatibility of chitosan with acrylate matrix is ​​significantly enhanced, so that the antibacterial property of chitosan is fully exerted, and the antibacterial property of the matrix is ​​greatly enhanced. In addition, the modified chitosan molecule also contains pyridinium quaternary ammonium salt, long carbon chain and carbon-carbon double bond structure. Pyridinium quaternary ammonium salt is a new type of quaternary ammonium salt with positive charge. It is more concentrated and has stronger bactericidal ability, avoiding the problem of bacterial resistance caused by the long-term use of quaternary ammonium antimicrobial agents, and further enhancing the antibacterial properties of the matrix; the introduced long carbon chain structure can not only penetrate between the macromolecular chains of the matrix to improve the toughness of the matrix, but also the long carbon chain has strong hydrophobicity, which can promote the interaction between chitosan and bacterial cell walls, further enhancing the antibacterial properties of the matrix; finally, the carbon-carbon double bond can be cross-linked with the matrix, enhancing the interaction between the modified chitosan and the matrix, making the antibacterial properties of the modified chitosan even better;

[0035] It should be noted that chitosan grafted onto organic molecular chains can significantly improve the migration and exudation resistance of the organic molecular chains, thus ensuring the long-term stability of the performance of the modified chitosan.

[0036] Beneficial effects of the present invention:

[0037] 1. The glassware prepared by the present invention makes the crystal more complete by strictly controlling the temperature of nucleation and crystallization. The microcrystallization heat treatment can precipitate a large amount of low expansion crystal phase in the base glass, greatly improving the heat resistance and impact resistance of the glassware;

[0038] 2. The antibacterial coating is a water-based coating, which is environmentally friendly and has high flexibility and strong impact resistance through the selection of monomers;

[0039] 3. Adding homemade modified chitosan to the antibacterial coating, the modified chitosan has good compatibility with the acrylate matrix, and the various groups in the modified chitosan molecules play a synergistic role, which can significantly enhance the antibacterial properties of glassware and the flexibility of the antibacterial coating, and the performance is stable and not easy to fall off;

[0040] Therefore, the glassware prepared by the present invention is a microcrystalline glassware, which has complete crystals, good heat resistance and impact resistance, and stable and efficient antibacterial performance, and has important application value in the field of glassware technology. DETAILED DESCRIPTION

[0041] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] Example 1

[0043] Preparation of modified chitosan:

[0044] S1. Add 9.4 g 4-aminopyridine, 28.4 g stearic acid, 20.6 g dicyclohexylcarbodiimide and 120 mL pyridine to a three-necked flask equipped with a stirring device, stir and mix well, place in a 45°C water bath, and heat in a water bath for 8 h. After the reaction is completed, filter, remove the solvent by vacuum distillation, and purify by column chromatography (the eluent is a mixed solvent of petroleum ether / ethyl acetate, the volume ratio of the two is 5:1), and remove the eluent by rotary evaporation to obtain intermediate 1;

[0045] S2, in a three-necked flask equipped with a stirring reflux device, 41.3g of intermediate 1 and 150mL of ether were added and stirred and mixed evenly, and then 13.5g of epibromopropane was added dropwise, and the reaction temperature was controlled to 68°C, and the reaction was refluxed for 8h. After the reaction was completed, part of the solvent was removed by distillation under reduced pressure, and then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two was 5:1), and the eluent was removed by rotary evaporation to obtain intermediate 2;

[0046] S3. In a three-necked flask equipped with a stirring device, 2 g of chitosan, 10 mL of deionized water and 20 mL of isopropanol were mixed, stirred in a water bath at 80°C for 2 h, sodium hydroxide solution (mass fraction 35%) was added dropwise, and 8 g of intermediate 2 was added, and the reaction was continued with stirring for 48 h. The pH was adjusted to 7, filtered, washed with ethanol and water in turn, and vacuum dried to obtain pre-modified chitosan;

[0047] S4. In a three-necked flask equipped with a stirring device, mix 1 g of pre-modified chitosan, 30 mL of N,N-dimethylformamide and 10 mL of isopropanol. After stirring in a 65°C water bath for 1 h, add sodium hydroxide solution (35% by mass) to adjust the pH to 9, and then add 6 g of allyl chloride dropwise. After keeping warm for 1 h, the reaction is complete. Filter, wash with ethanol and water in turn, and dry to obtain modified chitosan.

[0048] Example 2

[0049] Preparation of modified chitosan:

[0050] S1. Add 18.8 g 4-aminopyridine, 56.8 g stearic acid, 41.2 g dicyclohexylcarbodiimide and 240 mL pyridine to a three-necked flask equipped with a stirring device, stir and mix well, place in a 45°C water bath, and heat in a water bath for 8 h. After the reaction is completed, filter, remove the solvent by vacuum distillation, and purify by column chromatography (the eluent is a mixed solvent of petroleum ether / ethyl acetate, the volume ratio of the two is 5:1), and remove the eluent by rotary evaporation to obtain intermediate 1;

[0051] S2, in a three-necked flask equipped with a stirring reflux device, add 82.6g of intermediate 1 and 300mL of ether, stir and mix evenly, then add 27.0g of epibromopropane dropwise, control the reaction temperature to 68°C, reflux reaction for 8h, the reaction is completed, remove part of the solvent by vacuum distillation, and then purify by column chromatography (the eluent is a mixed solvent of petroleum ether / ethyl acetate, the volume ratio of the two is 5:1), and remove the eluent by rotary evaporation to obtain intermediate 2;

[0052] S3. In a three-necked flask equipped with a stirring device, 4 g of chitosan, 20 mL of deionized water and 40 mL of isopropanol were mixed, stirred in a water bath at 80°C for 2 h, sodium hydroxide solution (mass fraction 35%) was added dropwise, and 16 g of intermediate 2 was added, and the reaction was continued with stirring for 48 h. The pH was adjusted to 7, filtered, washed with ethanol and water in turn, and vacuum dried to obtain pre-modified chitosan;

[0053] S4. In a three-necked flask equipped with a stirring device, mix 2 g of pre-modified chitosan, 60 mL of N,N-dimethylformamide and 20 mL of isopropanol. After stirring in a 65°C water bath for 1 h, add sodium hydroxide solution (35% by mass) to adjust the pH to 9, and then add 12 g of allyl chloride dropwise. After keeping warm for 1 h, the reaction is complete. Filter, wash with ethanol and water in turn, and dry to obtain modified chitosan.

[0054] Example 3

[0055] Preparation of antimicrobial coating:

[0056] 35 g of butyl acrylate, 40 g of ethyl acrylate, 6 g of acrylic acid, 3 g of sodium dodecyl sulfate, 2 g of silicone defoamer (produced by Shandong Juneng Chemical Co., Ltd.) and 80 g of water were added to a reactor and emulsified to obtain an emulsion. Then, 5 g of the modified chitosan obtained in Example 1 and 0.1 g of azodiisopropylimidazoline were added and the mixture was kept at 70° C. for 2 h to initiate a polymerization reaction. The reaction was completed to obtain an antibacterial coating.

[0057] Example 4

[0058] Preparation of antimicrobial coating:

[0059] 40 g of butyl acrylate, 45 g of ethyl acrylate, 8 g of acrylic acid, 4 g of sodium dodecyl sulfate, 3 g of silicone defoamer (produced by Shandong Juneng Chemical Co., Ltd.) and 90 g of water were added to a reactor and emulsified to obtain an emulsion. Then, 10 g of the modified chitosan obtained in Example 2 and 0.2 g of azodiisopropylimidazoline were added, and the mixture was kept warm at 80° C. for 2 h to initiate a polymerization reaction. The reaction was completed to obtain an antibacterial coating.

[0060] Example 5

[0061] Preparation of antimicrobial coating:

[0062] 45 g of butyl acrylate, 50 g of ethyl acrylate, 10 g of acrylic acid, 5 g of sodium dodecyl sulfate, 4 g of silicone defoamer (produced by Shandong Juneng Chemical Co., Ltd.) and 100 g of water were added to a reactor and emulsified to obtain an emulsion. Then, 15 g of the modified chitosan obtained in Example 2 and 0.3 g of azodiisopropylimidazoline were added, and the mixture was kept warm at 90° C. for 2 h to initiate a polymerization reaction. The reaction was completed to obtain an antibacterial coating.

[0063] Example 6

[0064] A1. 65g SiO2, 18g Al2O3, 4g Li2O, 1g Na2O, 1g K2O, 2g ZnO, 6g TiO2 and 3g ZrO2 are melted at 1550°C, clarified and homogenized, cooled to 1350°C, pressed into glassware and cooled and annealed to obtain basic glassware;

[0065] A2. The basic glassware obtained in step A1 is nucleated at 750°C for 1 hour, then crystallized at 850°C for 4 hours, and cooled to below 200°C in the furnace to obtain low-expansion microcrystalline glassware. The antibacterial coating prepared in Example 3 is then evenly applied to the inner and outer surfaces of the glassware to obtain low-expansion antibacterial microcrystalline glassware.

[0066] Example 7

[0067] A1. 72g SiO2, 15g Al2O3, 2.5g Li2O, 1g Na2O, 1g K2O, 2.5g ZnO, 5g TiO2 and 1g ZrO2 are melted at 1600°C, clarified and homogenized, cooled to 1375°C, pressed into glassware and cooled and annealed to obtain basic glassware;

[0068] A2. The basic glassware obtained in step A1 is nucleated at 800°C for 2 hours, then crystallized at 925°C for 7 hours, and cooled to below 200°C in the furnace to obtain low-expansion microcrystalline glassware. The antibacterial coating prepared in Example 4 is then evenly applied to the inner and outer surfaces of the glassware to obtain low-expansion antibacterial microcrystalline glassware.

[0069] Example 8

[0070] A1. 72g SiO2, 20g Al2O3, 4g Li2O, 1g ZnO and 3g TiO2 are melted at 1650°C, clarified and homogenized, cooled to 1400°C, pressed into glassware and cooled and annealed to obtain basic glassware;

[0071] A2. The basic glassware obtained in step A1 is nucleated at 850°C for 4 hours, then crystallized at 1000°C for 10 hours, and cooled to below 200°C in the furnace to obtain low-expansion microcrystalline glassware. The antibacterial coating prepared in Example 5 is then evenly applied to the inner and outer surfaces of the glassware to obtain low-expansion antibacterial microcrystalline glassware.

[0072] Comparative Example 1

[0073] Use commercially available acrylate antimicrobial coatings.

[0074] Comparative Example 2

[0075] The antibacterial coating in Example 8 was replaced with a commercially available acrylate antibacterial coating, and the remaining steps were the same as those in Example 8.

[0076] The following performance tests were performed on Examples 3-5 and Comparative Example 1:

[0077] The flexibility is measured using the national standard GB / T 1731-1993 "Determination of paint film flexibility";

[0078] The measured results are shown in Table 1:

[0079] Table 1

[0080]

[0081] The following performance tests were performed on Examples 6-8 and Comparative Example 2:

[0082] The method in standard JC / T1054-2007 is used to inoculate the surface with a suspension containing E. coli bacteria. After 24 hours of inoculation, the number of bacteria obtained on the surface of the antibacterial product and the untreated product is subtracted from the number of bacteria obtained on the surface of the untreated product (B) by the number of bacteria obtained on the surface of the antibacterial product (A) and divided by the number of bacteria obtained on the surface of the untreated product to obtain the antibacterial rate.

[0083] After the samples were placed at room temperature for 180 days, the antibacterial rate was determined using the same standard;

[0084] The measured results are shown in Table 2:

[0085] Table 2

[0086]

[0087] It can be seen from the above table that the glassware prepared in the embodiment of the present invention has stable and efficient antibacterial performance, and the antibacterial coating has excellent flexibility, and has important application value in the field of glassware technology.

[0088] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0089] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a low-expansion antibacterial glass-ceramic vessel, characterized in that: The following steps are involved: A1. SiO2, Al2O3, Li2O, Na2O, K2O, ZnO, TiO2 and ZrO2 are melted, clarified and homogenized, cooled and pressed into glassware, and cooled and annealed to obtain basic glassware; A2, nucleating the basic glassware obtained in step A1, re-crystallizing, and cooling with the furnace to obtain a low-expansion microcrystalline glassware, and then evenly applying the antibacterial coating on the inner and outer surfaces of the glassware to obtain a low-expansion antibacterial microcrystalline glassware; Wherein, the antibacterial coating is prepared by the following steps: Butyl acrylate, ethyl acrylate, acrylic acid, sodium lauryl sulfate, a defoamer and water are added into a reaction kettle for emulsification to obtain an emulsion, and then modified chitosan and an initiator are added to initiate a polymerization reaction, and the reaction is completed to obtain an antibacterial coating; Wherein, the modified chitosan is prepared by the following steps: S1, 4-aminopyridine, stearic acid, dicyclohexylcarbodiimide and pyridine were mixed, heated at 45°C for 8 hours, the reaction was completed, filtered, distilled under reduced pressure, purified by column chromatography, and rotary evaporated to obtain intermediate 1; S2, after mixing the intermediate 1 and ether evenly, epibromopropane was added dropwise, and the mixture was refluxed at 68°C for 8 hours. After the reaction was completed, the mixture was distilled under reduced pressure, purified by column chromatography, and rotary evaporated to obtain the intermediate 2; S3, chitosan, deionized water and isopropanol were mixed, stirred in a water bath at 80°C for 2h, sodium hydroxide solution was added dropwise, and intermediate 2 was added, stirring and reacting was continued for 48h, pH was adjusted to 7, filtered, washed, and vacuum dried to obtain pre-modified chitosan; S4. Mix the pre-modified chitosan, N,N-dimethylformamide and isopropanol, stir in a 65°C water bath for 1 hour, add sodium hydroxide solution to adjust the pH to 9, then add allyl chloride dropwise, keep warm for 1 hour, the reaction is complete, filter, wash with water, and dry to obtain modified chitosan.

2. The method for preparing a low expansion antibacterial glass-ceramic vessel according to claim 1, characterized in that: In step S1, the ratio of 4-aminopyridine, stearic acid, dicyclohexylcarbodiimide and pyridine is 9.4 g: 28.4 g: 20.6 g: 120 mL.

3. The method for preparing a low expansion antibacterial glass-ceramic vessel according to claim 1, characterized in that: In step S2, the ratio of the amount of intermediate 1, ether and epibromopropane used is 41.3 g:150 mL:13.5 g.

4. The method for preparing a low expansion antibacterial glass-ceramic vessel according to claim 1, characterized in that: In step S3, the ratio of chitosan, deionized water, isopropanol and intermediate 2 is 2 g:10 mL:20 mL:8 g.

5. The method for preparing a low expansion antibacterial glass-ceramic vessel according to claim 1, characterized in that: In step S4, the ratio of the amount of pre-modified chitosan, N,N-dimethylformamide, isopropanol and allyl chloride is 1 g:30 mL:10 mL:6 g.

6. The method for preparing a low expansion antibacterial microcrystalline glass vessel according to claim 1, characterized in that: The glassware includes the following raw materials in percentage by mass: SiO2: 65%-72%, Al2O3: 15%-20%, Li2O: 2.5%-4%, Na2O: 0%-1%, K2O: 0-1%, ZnO: 1%-2.5%, TiO2: 2%-6%, and ZrO2: 0-3%.

7. The method for preparing a low expansion antibacterial micro-ceramic glass vessel according to claim 1, characterized in that: The raw materials are calculated in parts by weight as follows: 35-45 parts of butyl acrylate, 40-50 parts of ethyl acrylate, 6-10 parts of acrylic acid, 3-5 parts of sodium dodecyl sulfate, 2-4 parts of defoaming agent, 80-100 parts of water, 5-15 parts of modified chitosan, and 0.1-0.3 parts of initiator.

8. A low expansion antibacterial glass-ceramic vessel, characterized in that: Prepared according to the method according to any one of claims 1 to 7.