By using the bisphosphonic acid extractant P,P'-[(9-octadecenylimine)bis(methylene)]bis[p-phenylphosphinic acid] in the wet phosphoric acid solution, the wet problem was solved. It solves the problem of separation of iron and aluminum in phosphoric acid and achieves efficient and low-cost removal of iron and aluminum, which is significantly better than traditional phosphorus (phosphine) extraction agents.
Patent Information
- Application Number
- CN202411037122.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-07-31
AI Technical Summary
It is difficult to effectively separate iron and aluminum in a strongly acidic wet phosphoric acid system with existing technology. Traditional extraction agents show unsatisfactory extraction effects under high sulfuric acid and phosphoric acid concentrations, and there are problems with extraction agent loss and phosphoric acid loss.
Develop a bisphosphonic acid extractant P,P'-[(9-octadecenylimine)bis(methylene)]bis[p-phenylphosphinic acid], through specific preparation methods and process conditions, An extractant with good oil solubility and thermal stability was prepared for deep removal of iron and aluminum in wet phosphoric acid solution.
This extractant significantly improves the extraction efficiency of iron and aluminum without changing the wet phosphoric acid process, reduces the loss of the extractant, is not volatile, has high yield and low cost, and is suitable for large-scale industrial applications.
Smart Images

Figure CN118598907B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of extractants, and in particular relates to a diphosphonic acid extractant for extracting iron and aluminum, and a preparation method and application thereof. Background Art
[0002] Wet-process phosphoric acid is mainly divided into sulfuric acid method, hydrochloric acid method and nitric acid method according to the different acids used. Among them, the sulfuric acid method is the most basic and widely used method for producing wet-process phosphoric acid. Therefore, the so-called "wet-process phosphoric acid" actually refers to sulfuric acid wet-process phosphoric acid. The sulfuric acid method is divided into dihydrate method, semi-hydrate method and anhydrous method according to the different water content of the generated phosphogypsum. Regardless of the ore dissolution method used, impurities such as iron and aluminum in the phosphate ore will enter the acid solution and phosphogypsum, affecting the quality of phosphogypsum and the refining of phosphoric acid, and limiting the subsequent use of the two.
[0003] At present, the hydrometallurgical industry usually uses precipitation, adsorption and solvent extraction to remove impurities from the solution. The precipitation method is simple to operate, but it consumes a large amount of precipitant and cannot introduce other impurities while deeply removing impurities. The adsorption method often uses ion exchange resin, which has high impurity removal efficiency, but the load capacity is limited. It is only economically feasible when the impurity content is very low. The solvent extraction method has a large processing capacity, high efficiency, simple operation, and is easier to achieve large-scale industrialization. In the past few decades, people have conducted a lot of research on the technology of solvent extraction to remove iron. "A method for extracting and separating iron and phosphorus from iron phosphate slag to prepare iron phosphate" (CN 114804048 A) discloses a method for extracting and separating iron from iron phosphate slag acid leaching solution using P204. The invention requires strict control of the pH of the extraction system to about 1, and the concentration of sulfuric acid and phosphoric acid in the wet phosphoric acid acid leaching solution is high, so this method is not applicable. "A method for resource-based soil treatment of red mud" (CN 111690810 A) invented a method for extracting iron from red mud using a quaternary ammonium extractant, and the hydrogen ion concentration of the leaching system is 0.5~2 mol / L. However, the quaternary ammonium extractant is easy to emulsify and difficult to separate, and it also has a certain extraction effect on phosphoric acid in the acid solution, resulting in phosphorus loss. "A double phosphoric acid extractant for extracting and separating zirconium and hafnium and its preparation method" (CN 110746454 A) discloses a double phosphoric acid extractant, N,N-octylamine di(methylenebenzene hypophosphorous acid), which has a strong extraction ability for zirconium and hafnium. Under the same conditions, the extraction rate far exceeds that of common acidic organic phosphorus extractants. However, when the extractant is used to extract iron and aluminum from wet phosphoric acid solution, the extraction effect is not ideal, and the loss of the extractant is large. Alkaline organic amine extractants will extract phosphoric acid in the acid solution. Neutral extractants have poor coordination ability for iron and aluminum in strongly acidic sulfuric acid systems. Traditional acidic extractants are difficult to ionize in strongly acidic systems, and the extraction effect deteriorates as the acidity of the aqueous phase increases. The concentration of sulfuric acid and phosphoric acid in wet-process phosphoric acid acid is high, the composition is complex, and the removal of iron and aluminum is difficult. Currently, there are few reports on industrial technologies for simultaneously separating iron and aluminum from wet-process phosphoric acid acid. Therefore, it is necessary to develop a new extractant suitable for separating impurities iron and aluminum in strongly acidic wet-process phosphoric acid systems. Summary of the invention
[0004] Aiming at the problem that the acid liquid produced by wet-process phosphoric acid has complex components and high concentrations of sulfuric acid and phosphoric acid, and traditional extractants (such as P204, P507, TBP, cyclohexane acid, etc.) cannot effectively separate iron and aluminum, the present invention provides a diphosphonic acid extractant for extracting iron and aluminum, and a preparation method and application thereof. The extractant can effectively extract iron and aluminum in the acid liquid without changing the current wet-process phosphoric acid process.
[0005] The present invention is achieved through the following technical solutions:
[0006] A bisphosphonic acid extractant for extracting iron and aluminum, wherein the structural formula of the bisphosphonic acid extractant for extracting iron and aluminum is:
[0007] .
[0008] The preparation method of the above-mentioned bisphosphonic acid extractant for extracting iron and aluminum comprises the following steps:
[0009] (1) Mix the solvent, oleylamine, phenylphosphinic acid and inorganic acid and heat until the solution becomes clear and transparent;
[0010] (2) adding formaldehyde solution or paraformaldehyde to the clear and transparent solution of step (1) to carry out a reaction;
[0011] (3) After the reaction in step (2) is completed, the aqueous phase is removed, and the colloid after the aqueous phase is removed is dissolved with dichloromethane. The colloid is washed, rotary evaporated, and dried to obtain a bisphosphonic acid extractant (P,P'-[(9-octadecene imine) di(methylene)] di[p-phenylphosphinic acid]) for extracting iron and aluminum.
[0012] Furthermore, the solvent in step (1) is one or more of water and alcohol; the inorganic acid is one of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid or acetic acid; and the purity of oleylamine is ≥90%.
[0013] Furthermore, the alcohol in step (1) is one of ethanol, propanol and isopropanol; and the inorganic acid is hydrochloric acid or sulfuric acid.
[0014] Furthermore, the molar ratio of oleylamine to phenylphosphinic acid is 1:1-1:4; the molar ratio of oleylamine to inorganic acid is 10:1-1:3; and the molar ratio of oleylamine to formaldehyde is 1:1-1:5.
[0015] Furthermore, the heating temperature in step (1) is 50-110° C.; the reaction temperature in step (2) is 50-110° C., and the reaction time is 1-10 h.
[0016] In the present invention, the diphosphonic acid extractant for extracting iron and aluminum is used in extracting iron and aluminum from wet-process phosphoric acid solution.
[0017] Furthermore, the Fe 3+ The concentration is 0.1~6.5 g / L, Al 3+ The concentration is 0.1~10 g / L, the concentration of sulfuric acid is 0.01~3 mol / L, and the concentration of phosphoric acid is 1~8 mol / L.
[0018] Furthermore, the method for extracting iron and aluminum from wet-process phosphoric acid solution comprises the following steps:
[0019] (1) The diluent-prepared bisphosphonic acid extractant for extracting iron and aluminum is used as the organic phase, and the concentration of the bisphosphonic acid extractant for extracting iron and aluminum is 0.01~0.5 mol / L;
[0020] (2) preheating the organic phase and the wet-process phosphoric acid solution in step (1), mixing and stirring them for extraction, and separating the mixed solution after extraction to obtain an organic phase loaded with iron and aluminum ions and a raffinate;
[0021] (3) The organic phase loaded with iron and aluminum ions is stripped with a stripping agent at a stripping temperature of 20-80 °C to obtain an aqueous solution containing iron and aluminum ions.
[0022] Furthermore, the diluent described in step (1) is one or more of aliphatic hydrocarbons, halogenated hydrocarbons, aromatic hydrocarbons, solvent oil and alcohol; the volume ratio of the wet-process phosphoric acid solution to the organic phase described in step (2) is 1:5~5:1, the extraction time is 1~120min, and the extraction temperature is 10~90°C; the stripping agent in step (3) is 0.1~1 mol / L ammonium oxalate, and the stripping time is 10~120min.
[0023] Beneficial Effects
[0024] (1) The bisphosphonic acid extractant (P,P'-[(9-octadecene imine) di(methylene)] di[p-phenylphosphinic acid]) for extracting iron and aluminum in the present invention has a simple preparation method, high yield, and can be produced on a large scale; the octadecene group ensures that the extractant has good oil solubility and can greatly reduce the amount of extractant loss during high-temperature extraction.
[0025] (2) The present invention uses P,P'-[(9-octadecene imine)di(methylene)]di[p-phenylphosphinic acid] as an extractant, and exhibits a good extraction effect on iron and aluminum in a wet-process phosphoric acid acid system. It can achieve deep removal of iron and aluminum without changing the wet-process phosphoric acid process, and the extraction performance is significantly better than traditional phosphorus (phosphine) extractants such as P204, P507, and Cyanex272.
[0026] (3) The bisphosphonic acid extractant for extracting iron and aluminum of the present invention has good thermal stability in extracting iron and aluminum from wet-process phosphoric acid solution, is not easily volatile, and can be reused. All reagents used are low-priced and easily available, and the input amount is small, thus saving costs.
[0027] (4) The bisphosphonic acid extractant for extracting iron and aluminum of the present invention does not emulsify iron and aluminum in wet-process phosphoric acid solution, and the phase separation is fast, and the production efficiency is high. Compared with common phosphorus (phosphine) extractants, the extractant does not require saponification and is an environmentally friendly extractant. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The nuclear magnetic resonance spectrum of the bisphosphonic acid extractant for extracting iron and aluminum prepared in Example 4;
[0029] Figure 2 This is the infrared spectrum of the bisphosphonic acid extractant for extracting iron and aluminum prepared in Example 4. DETAILED DESCRIPTION
[0030] The present invention is described in detail below in conjunction with specific embodiments, but the protection scope of the present invention is not limited by the embodiments. All technologies implemented based on the above content of the present invention are included in the scope of protection intended by the present invention.
[0031] The structural formula of the bisphosphonic acid extractant (P,P'-[(9-octadecene imine) di(methylene)] di[p-phenylphosphinic acid]) for extracting iron and aluminum prepared by the present invention is:
[0032]
[0033] In the following examples and comparative examples, Fe 3+ The concentration is 1.7 g / L, Al 3+ The concentration is 7.6 g / L, the concentration of sulfuric acid is 1 mol / L, and the concentration of phosphoric acid is 6 mol / L;
[0034] The extraction rate (E) can directly show the extraction capacity of the extractant, and the stripping rate (S) can reflect the regeneration capacity of the extractant. The metal ion concentrations in the initial aqueous phase, raffinate and stripping raffinate were determined by ICP-OES, and the extraction rate E and stripping rate S were calculated by formulas (1) to (2) respectively:
[0035]
[0036] C0, C1 and C2 in the formula represent the metal ion concentrations in the initial aqueous phase, the raffinate and the strip raffinate, respectively. In the present invention, the metal ion concentration is determined by ICP-OES.
[0037] Example 1
[0038] (1) In a 1000 mL three-necked round-bottom flask equipped with a mechanical stirrer and a condensation reflux device, add 300 mL of water, 0.5 mol of oleylamine, 0.5 mol of phenylphosphinic acid and 0.1 mol of hydrochloric acid (HCl) in sequence, mix, and heat to 70°C. The mixture becomes clear and transparent.
[0039] (2) Add 1 mol of 37% formaldehyde solution to the clear and transparent solution of step (1), and react at 70°C for 4 hours;
[0040] (3) After the reaction in step (2) is completed, the upper aqueous phase is removed, and the colloid after the aqueous phase is removed is dissolved with dichloromethane, washed with dilute hydrochloric acid and water in turn, rotary evaporated, and vacuum dried to obtain a bisphosphonic acid extractant (P,P'-[(9-octadecene imine) di(methylene)] di[p-phenylphosphinic acid]) for extracting iron and aluminum.
[0041] Example 2
[0042] (1) In a 1000 mL three-necked round-bottom flask equipped with a mechanical stirrer and a condensation reflux device, add 300 mL of water, 0.5 mol of oleylamine, 1 mol of phenylphosphinic acid and 0.5 mol of hydrochloric acid (HCl) in sequence, mix, and heat to 90°C. The mixture becomes clear and transparent.
[0043] (2) Add 2 mol of 37% formaldehyde solution to the clear and transparent solution of step (1), and react at 90°C for 5 hours;
[0044] (3) After the reaction in step (2) is completed, the upper aqueous phase is removed, and the colloid after the aqueous phase is removed is dissolved with dichloromethane, washed with dilute hydrochloric acid and water in turn, rotary evaporated, and vacuum dried to obtain a bisphosphonic acid extractant (P,P'-[(9-octadecene imine) di(methylene)] di[p-phenylphosphinic acid]) for extracting iron and aluminum.
[0045] Example 3
[0046] (1) In a 1000 mL three-necked round-bottom flask equipped with a mechanical stirrer and a condensation reflux device, add 300 mL of ethanol, 0.5 mol of oleylamine, 1 mol of phenylphosphinic acid and 0.3 mol of sulfuric acid (H2SO4) in sequence, mix, and heat to 80°C. The mixture becomes clear and transparent.
[0047] (2) Add 1 mol of 37% formaldehyde solution to the clear and transparent solution of step (1), and react at 80°C for 7 hours;
[0048] (3) After the reaction in step (2) is completed, the upper aqueous phase is removed, and the colloid after the aqueous phase is removed is dissolved with dichloromethane, washed with dilute hydrochloric acid and water in turn, rotary evaporated, and vacuum dried to obtain a bisphosphonic acid extractant (P,P'-[(9-octadecene imine) di(methylene)] di[p-phenylphosphinic acid]) for extracting iron and aluminum.
[0049] Example 4
[0050] (1) In a 1000 mL three-necked round-bottom flask equipped with a mechanical stirrer and a condensation reflux device, add 300 mL of ethanol, 0.5 mol of oleylamine, 1.2 mol of phenylphosphinic acid and 0.2 mol of sulfuric acid (H2SO4) in sequence, mix, and heat to 100°C. The mixture becomes clear and transparent.
[0051] (2) adding 1.5 mol of 37% formaldehyde solution to the clear and transparent solution of step (1), and reacting at 100°C for 6 hours;
[0052] (3) After the reaction in step (2) is completed, the upper aqueous phase is removed, and the colloid after the aqueous phase is removed is dissolved with dichloromethane, washed with dilute hydrochloric acid and water in turn, rotary evaporated, and vacuum dried to obtain a bisphosphonic acid extractant (P,P'-[(9-octadecene imine) di(methylene)] di[p-phenylphosphinic acid]) for extracting iron and aluminum.
[0053] Example 5
[0054] (1) In a 1000 mL three-necked round-bottom flask equipped with a mechanical stirrer and a condensation reflux device, add 300 mL of ethanol, 0.5 mol of oleylamine, 1.5 mol of phenylphosphinic acid and 0.5 mol of sulfuric acid (H2SO4) in sequence, mix, and heat to 110°C. The mixture becomes clear and transparent.
[0055] (2) Add 2 mol of 37% formaldehyde solution to the clear and transparent solution of step (1), and react at 110°C for 8 hours;
[0056] (3) After the reaction in step (2) is completed, the upper aqueous phase is removed, and the colloid after the aqueous phase is removed is dissolved with dichloromethane, washed with dilute hydrochloric acid and water in turn, rotary evaporated, and vacuum dried to obtain a bisphosphonic acid extractant (P,P'-[(9-octadecene imine) di(methylene)] di[p-phenylphosphinic acid]) for extracting iron and aluminum.
[0057] The raw materials and yields of the bisphosphonic acid extractants for extracting iron and aluminum prepared in Examples 1 to 5 are shown in Table 1 below:
[0058] Table 1
[0059]
[0060] The nuclear magnetic resonance hydrogen spectrum and infrared spectrum of the bisphosphonic acid extractant for extracting iron and aluminum prepared in Example 4 are as follows: Figure 1 and Figure 2 As shown. P,P'-[(9-octadecene imine)bis(methylene)]bis[p-phenylphosphinic acid]: 1 H NMR (400 MHz, DMSO) δ 7.71 (dd, J = 11.0, 7.6 Hz, 4H, -CH=), 7.51 (ddd, J = 11.8, 10.4, 5.5 Hz,6H, -CH=), 5.38 – 5.29 (m, 2H, -CH=CH-), 3.33 (d, J= 7.7 Hz, 4H, N-CH2-P),2.85 (s, 2H, -OH), 1.97 (s, 4H, -CH2-C=C), 1.34 – 1.00 (m, 24H, -CH2-), 0.84(t, J = 6.8 Hz, 3H, -CH3); IR(KBr, cm -1 ) C=C (film) / cm -1 1463; υ p-Ar (film) / cm -1 1439;υ p=o (film) / cm -1 1215; υ C-N (film) / cm -1 1136; υ p-o (film) / cm -1 947.
[0061] Example 6
[0062] (1) A 0.3 mol / L bisphosphonic acid extractant for extracting iron and aluminum was prepared with a diluent and 20% n-octanol (phase regulator) as the organic phase. The diluents used were 1, 2, 4-trimethylbenzene, S-150 solvent oil, and S-260 solvent oil;
[0063] (2) 25 mL of the organic phase in step (1) and 25 mL of wet-process phosphoric acid solution (aqueous phase) were mixed and stirred for extraction. The extraction temperature was 10 min at 25 °C. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate. The Fe content in the raffinate was determined. 3+ 、Al 3+ The concentration (Fe 3+ The concentrations were all less than 0.043 g / L, Al 3+ The concentrations were all less than 5.85 g / L). The extraction rate (E) was calculated according to formula (1). The effect of the diluent on the extraction rate is shown in Table 2.
[0064] Table 2
[0065]
[0066] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C and a stripping time of 30 min to obtain an aqueous solution containing iron and aluminum ions, wherein Fe 3+ The concentrations were all greater than 1.65 g / L, Al 3+The concentrations are all greater than 1.75 g / L. The stripping rate (S) is calculated according to formula (2). The stripping rate of aluminum is greater than 99.9%, and the stripping rate of iron is greater than 99%.
[0067] Example 7
[0068] (1) A 0.3 mol / L bisphosphonic acid extractant for extracting iron and aluminum was prepared with S-260 solvent oil diluent and 20% n-octanol (phase regulator) as the organic phase;
[0069] (2) 25 mL of the organic phase in step (1) and 25 mL of wet phosphoric acid solution (aqueous phase) were mixed and stirred for extraction. The extraction temperature was 15 min at 45 °C. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate. The Fe content in the raffinate was determined. 3+ 、Al 3+ The concentration (Fe 3+ The concentration is 0.044 g / L, Al 3+ The concentration is 5.88 g / L), and the extraction rate (E) is calculated according to formula (1). The extraction results are shown in Table 3;
[0070] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C and a stripping time of 30 min to obtain an aqueous solution containing iron and aluminum ions, wherein Fe 3+ The concentration is 1.64 g / L, Al 3+ The concentration is 1.72 g / L. The stripping rate (S) is calculated according to formula (2). The stripping rate of aluminum is greater than 99.9%, and the stripping rate of iron is greater than 99%.
[0071] Example 8
[0072] (1) A 0.3 mol / L bisphosphonic acid extractant for extracting iron and aluminum was prepared with S-260 solvent oil diluent and 20% n-octanol (phase regulator) as the organic phase;
[0073] (2) 25 mL of the organic phase in step (1) and 25 mL of wet-process phosphoric acid solution (aqueous phase) were mixed and stirred for extraction. The extraction temperature was 15 min at 55 °C. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate. The Fe content in the raffinate was determined. 3+ 、Al 3+ The concentration (Fe 3+ The concentration is 0.056 g / L, Al 3+ The concentration is 6.16 g / L), and the extraction rate (E) is calculated according to formula (1). The extraction results are shown in Table 3;
[0074] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C and a stripping time of 30 min to obtain an aqueous solution containing iron and aluminum ions, wherein Fe 3+ The concentration is 1.63 g / L, Al 3+ The concentration is 1.44 g / L. The stripping rate (S) is calculated according to formula (2). The stripping rate of aluminum is greater than 99.9%, and the stripping rate of iron is greater than 99%.
[0075] Example 9
[0076] (1) A 0.3 mol / L bisphosphonic acid extractant for extracting iron and aluminum was prepared with S-260 solvent oil diluent and 20% n-octanol (phase regulator) as the organic phase;
[0077] (2) 30 mL of the organic phase in step (1) and 10 mL of wet-process phosphoric acid solution (aqueous phase) were mixed and stirred for extraction. The extraction temperature was 15 min at 65 °C. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate. The Fe content in the raffinate was determined. 3+ 、Al 3+ The concentration (Fe 3+ The concentration is 3.4×10 -3 g / L,Al 3+ The concentration is 3.59 g / L), and the extraction rate (E) is calculated according to formula (1). The extraction results are shown in Table 3;
[0078] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C and a stripping time of 30 min to obtain an aqueous solution containing iron and aluminum ions, wherein Fe 3+ The concentration is 1.68 g / L, Al 3+ The concentration is 4.01 g / L. The stripping rate (S) is calculated according to formula (2). The stripping rate of aluminum is greater than 99.9%, and the stripping rate of iron is greater than 99%.
[0079] Example 10
[0080] (1) A 0.3 mol / L bisphosphonic acid extractant for extracting iron and aluminum was prepared with S-260 solvent oil diluent and 20% n-octanol (phase regulator) as the organic phase;
[0081] (2) 10 mL of the organic phase in step (1) and 30 mL of wet-process phosphoric acid solution (aqueous phase) were mixed and stirred for extraction. The extraction temperature was 15 min at 75 °C. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate. The Fe content in the raffinate was determined. 3+ 、Al 3+ The concentration (Fe 3+The concentration is 0.81 g / L, Al 3+ The concentration is 7.38 g / L), and the extraction rate (E) is calculated according to formula (1). The extraction results are shown in Table 3;
[0082] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C and a stripping time of 30 min to obtain an aqueous solution containing iron and aluminum ions, wherein Fe 3+ The concentration is 0.89 g / L, Al 3+ The concentration is 0.22 g / L. The stripping rate (S) is calculated according to formula (2). The stripping rate of aluminum is greater than 99.9%, and the stripping rate of iron is greater than 99%.
[0083] Examples 7-10: Effect of bisphosphonic acid extractant on Fe in wet-process phosphoric acid solution 3+ 、Al 3+ The extraction rates are shown in Table 3 below:
[0084] Table 3
[0085]
[0086] Embodiment 11
[0087] (1) A 0.3 mol / L bisphosphonic acid extractant for extracting iron and aluminum was prepared with S-260 solvent oil diluent and 20% n-octanol (phase regulator) as the organic phase;
[0088] (2) 25 mL of the organic phase in step (1) and 25 mL of wet phosphoric acid solution (aqueous phase) were mixed for extraction. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate (aqueous phase). The extraction time was 5 min, the extraction temperature was 25 °C, and the Fe content in the raffinate was determined. 3+ 、Al 3+ The concentration (Fe 3+ The concentration is 0.23 g / L, Al 3+ The concentration is 6.64 g / L), and the extraction rate (E) is calculated according to formula (1). The extraction results are shown in Table 4;
[0089] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C and a stripping time of 30 min to obtain an aqueous solution containing iron and aluminum ions, wherein Fe 3+ The concentration is 1.45 g / L, Al 3+ The concentration is 0.96 g / L. The stripping rate (S) is calculated according to formula (2). The stripping rate of aluminum is greater than 99.9%, and the stripping rate of iron is greater than 99%.
[0090] Example 12
[0091] (1) A 0.3 mol / L bisphosphonic acid extractant for extracting iron and aluminum was prepared with S-260 solvent oil diluent and 20% n-octanol (phase regulator) as the organic phase;
[0092] (2) 25 mL of the organic phase in step (1) and 25 mL of wet phosphoric acid solution (aqueous phase) were mixed for extraction. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate (aqueous phase). The extraction time was 15 min, the extraction temperature was 25 °C, and the Fe content in the raffinate was determined. 3+ 、Al 3+ The concentration (Fe 3+ The concentration is 5.1×10 -3 g / L,Al 3+ The concentration is 5.60 g / L), and the extraction rate (E) is calculated according to formula (1). The extraction results are shown in Table 4;
[0093] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C and a stripping time of 30 min to obtain an aqueous solution containing iron and aluminum ions, wherein Fe 3+ The concentration is 1.68 g / L, Al 3+ The concentration is 2.00 g / L. The stripping rate (S) is calculated according to formula (2). The stripping rate of aluminum is greater than 99.9%, and the stripping rate of iron is greater than 99%.
[0094] Example 13
[0095] (1) A 0.1 mol / L bisphosphonic acid extractant for extracting iron and aluminum was prepared with S-260 solvent oil diluent and 20% n-octanol (phase regulator) as the organic phase;
[0096] (2) 25 mL of the organic phase in step (1) and 25 mL of wet phosphoric acid solution (aqueous phase) were mixed for extraction. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate (aqueous phase). The extraction time was 10 min, the extraction temperature was 25 °C, and the Fe content in the raffinate was determined. 3+ 、Al 3+ The concentration (Fe 3+ The concentration is 0.73 g / L, Al 3+ The concentration is 7.23 g / L), and the extraction rate (E) is calculated according to formula (1). The extraction results are shown in Table 4;
[0097] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C and a stripping time of 30 min to obtain an aqueous solution containing iron and aluminum ions, wherein Fe 3+ The concentration is 0.96 g / L, Al 3+The concentration is 0.37 g / L. The stripping rate (S) is calculated according to formula (2). The stripping rate of aluminum is greater than 99.9%, and the stripping rate of iron is greater than 99%.
[0098] Embodiment 14
[0099] (1) A 0.2 mol / L bisphosphonic acid extractant for extracting iron and aluminum was prepared with S-260 solvent oil diluent and 20% n-octanol (phase regulator) as the organic phase;
[0100] (2) 25 mL of the organic phase in step (1) and 25 mL of wet phosphoric acid solution (aqueous phase) were mixed for extraction. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate (aqueous phase). The extraction time was 10 min, the extraction temperature was 25 °C, and the Fe content in the raffinate was determined. 3+ 、Al 3+ The concentration (Fe 3+ The concentration is 0.37 g / L, Al 3+ The concentration is 7.08 g / L), and the extraction rate (E) is calculated according to formula (1). The extraction results are shown in Table 4;
[0101] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C and a stripping time of 30 min to obtain an aqueous solution containing iron and aluminum ions, wherein Fe 3+ The concentration is 1.31 g / L, Al 3+ The concentration is 0.52 g / L. The stripping rate (S) is calculated according to formula (2). The stripping rate of aluminum is greater than 99.9%, and the stripping rate of iron is greater than 99%.
[0102] Table 4
[0103]
[0104] Embodiment 15
[0105] (1) A 0.3 mol / L bisphosphonic acid extractant for extracting iron and aluminum was prepared with S-260 solvent oil diluent and 20% n-octanol (phase regulator) as the organic phase;
[0106] (2) 25 mL of the organic phase in step (1) and 25 mL of wet phosphoric acid solution were mixed for extraction. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate (aqueous phase). The aqueous phase after separation was mixed with 25 mL of fresh organic phase, and seven-stage cross-current extraction was repeated. The extraction time for each extraction was 15 min and the extraction temperature was 25 °C. The Fe content in the raffinate was determined. 3+ 、Al 3+ The concentration of , the extraction rate (E) was calculated according to formula (1), and the extraction results are shown in Table 5;
[0107] Table 5
[0108]
[0109] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C for 30 min to obtain an aqueous solution containing iron and aluminum ions. The stripping rate (S) was calculated according to formula (2). The stripping rate of aluminum was greater than 99.9%, and the stripping rate of iron was greater than 99%.
[0110] Example 16
[0111] (1) A 0.3 mol / L bisphosphonic acid extractant for extracting iron and aluminum was prepared with S-260 solvent oil diluent and 20% n-octanol (phase regulator) as the organic phase;
[0112] (2) 25 mL of the organic phase in step (1) and 25 mL of wet phosphoric acid solution were mixed and subjected to secondary countercurrent extraction for deep iron removal. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate (aqueous phase). The aqueous phase after separation was mixed with 25 mL of fresh organic phase and subjected to tertiary countercurrent aluminum removal. The extraction time for each extraction was 15 min and the extraction temperature was 25 °C. The Fe content in the raffinate was determined. 3+ 、Al 3+ The concentration of , the extraction rate (E) was calculated according to formula (1), and the extraction results are shown in Table 6;
[0113] Table 6
[0114]
[0115] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C for 30 min to obtain an aqueous solution containing iron and aluminum ions. The stripping rate (S) was calculated according to formula (2). The stripping rate of aluminum was greater than 99.9%, and the stripping rate of iron was greater than 99%.
[0116] Comparative Example 1
[0117] (1) Using S-260 solvent oil as a diluent, D2EHPA, P538, PC-88A, cyclohexane acid, CA-12, Cyanex 272, TOPO and TBP solutions with a concentration of 0.5 mol / L were prepared as the organic phase; the organic phase and wet-process phosphoric acid solution were mixed in a volume ratio of 5:1 for extraction. The extraction time was 30 min and the extraction temperature was 25 °C. After the extraction, the mixed solution was separated to obtain the organic phase loaded with iron and aluminum ions and the raffinate; the Fe content in the raffinate was determined. 3+ 、Al 3+The concentration of , the extraction rate (E) was calculated according to formula (1), and the extraction results are shown in Table 7;
[0118] (2) A 0.5 mol / L bisphosphonic acid extractant (P,P'-[(9-octadecene imine) di(methylene)] di[p-phenylphosphinic acid]) for extracting iron and aluminum was prepared with S-260 solvent oil diluent and 20% n-octanol (phase regulator) as the organic phase. The organic phase and wet phosphoric acid solution (aqueous phase) were mixed in a volume ratio of 5:1 for extraction. The extraction time was 15 min and the extraction temperature was 25 °C. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate. The Fe content in the raffinate was determined. 3+ 、Al 3+ The extraction rate (E) was calculated according to formula (1) and the extraction results are shown in Table 7.
[0119] Table 7
[0120]
Claims
1. A bisphosphonic acid extractant for extracting iron and aluminum, characterized in that: The structural formula of the bisphosphonic acid extractant for extracting iron and aluminum is: 。 2. A method for preparing the diphosphonic acid extractant for extracting iron and aluminum according to claim 1, characterized in that: The following steps are involved: (1) Mix the solvent, oleylamine, phenylphosphinic acid and inorganic acid and heat until the solution becomes clear and transparent; (2) adding formaldehyde solution or paraformaldehyde to the clear and transparent solution of step (1) to carry out a reaction; (3) After the reaction in step (2) is completed, the aqueous phase is removed, and the colloid after the aqueous phase is removed is dissolved with dichloromethane. The colloid is washed, rotary evaporated, and dried to obtain a bisphosphonic acid extractant for extracting iron and aluminum.
3. The method for preparing the bisphosphonic acid extractant for extracting iron and aluminum according to claim 2, characterized in that: The solvent in step (1) is one or more of water and alcohol; the inorganic acid is one of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid or acetic acid; the purity of oleylamine is ≥90%; The molar ratio of oleylamine to phenylphosphinic acid is 1:1 to 1:4; the molar ratio of oleylamine to inorganic acid is 10:1 to 1:3; the molar ratio of oleylamine to formaldehyde is 1:1 to 1:5; The heating temperature in step (1) is 50 to 110° C.; the reaction temperature in step (2) is 50 to 110° C., and the reaction time is 1 to 10 h.
4. The method for preparing the bisphosphonic acid extractant for extracting iron and aluminum according to claim 3, characterized in that: The alcohol described in step (1) is one of ethanol, propanol and isopropanol; and the inorganic acid is hydrochloric acid or sulfuric acid.
5. Use of the bisphosphonic acid extractant for extracting iron and aluminum according to claim 1 in extracting iron and aluminum from wet-process phosphoric acid solution.
6. The use according to claim 5, characterized in that The Fe in the wet phosphoric acid solution 3+ The concentration is 0.1 ~6.5 g / L, Al 3+ The concentration is 0.1 ~ 10 g / L, the concentration of sulfuric acid is 0.01 ~ 3 mol / L, and the concentration of phosphoric acid is 1 ~ 8 mol / L.
7. The use according to claim 5, characterized in that The method for extracting iron and aluminum from wet-process phosphoric acid solution comprises the following steps: (1) The diluent-prepared bisphosphonic acid extractant for extracting iron and aluminum is used as the organic phase, and the concentration of the bisphosphonic acid extractant for extracting iron and aluminum is 0.01 ~ 0.5 mol / L; (2) preheating the organic phase and the wet-process phosphoric acid solution in step (1), mixing and stirring them for extraction, and separating the mixed solution after extraction to obtain an organic phase loaded with iron and aluminum ions and a raffinate; (3) The organic phase loaded with iron and aluminum ions is stripped with a stripping agent at a stripping temperature of 20 to 80 °C to obtain an aqueous solution containing iron and aluminum ions.
8. The use according to claim 7, characterized in that The diluent described in step (1) is one or more of aliphatic hydrocarbons, halogenated hydrocarbons, aromatic hydrocarbons, solvent oil and alcohol; the volume ratio of the wet-process phosphoric acid solution to the organic phase described in step (2) is 1:5 to 5:1, the extraction time is 1 to 120 min, and the extraction temperature is 10 to 90 ° C; the stripping agent in step (3) is 0.1 to 1 mol / L ammonium oxalate, and the stripping time is 10 to 120 min.