A method for preparing fluoroethylene-ethylene copolymer

By using mixed organic solvents and ternary pentablock copolymer surfactants in the emulsion polymerization method of ethylene fluoride-ethylene copolymer and adding halogen salts, the problems of high copolymerization pressure and difficult composition are solved, and the product is improved The molecular weight and processing properties of the process can achieve a more efficient polymerization reaction.

CN118599047BActive Publication Date: 2024-11-15EAST CHINA UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411062778.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-15
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

In the prior art, when preparing ethylene fluoride-ethylene copolymers, the copolymerization reaction pressure is high and the composition of ethylene fluoride and ethylene is difficult to regulate, which affects the processing performance and industrial production efficiency of the product.

Method used

Using emulsion polymerization, mixed organic solvents such as N,N-dimethylformamide and high carbocycloalkanes were added, ternary pentablock copolymers were used as surfactants, and halogen salts were added to adjust the solvent in the aqueous phase and Distribution in micelles improves the solubility and diffusion rate of monomers and reduces the polymerization pressure.

Benefits of technology

It effectively reduces the polymerization reaction pressure, improves the molecular weight and composition regulation ability of ethylene fluoride-ethylene copolymer, and improves the processing performance and industrial production conditions of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_2
    Figure QLYQS_2
Patent Text Reader

Abstract

The invention discloses a method for preparing fluoroethylene-ethylene copolymer, and relates to the technical field of polymer preparation. Adopting emulsion polymerization, controlling the feeding ratio of fluoroethylene and ethylene monomers, using a ternary five-block copolymer as a surfactant, the middle of the surfactant is an ethylene oxide polymer segment with good hydrophilicity, the two ends are connected to the local lipophilic propylene oxide polymer segment, the outermost end is a tetrahydrofuran polymer segment with strong lipophilicity, and halogen salts and mixed organic solvents are added to the system at the same time, and the three act synergistically to effectively control the stability of micelles in the copolymer emulsion, accelerate the diffusion and dissolution of fluoroethylene and ethylene monomers from gas phase to water phase and from water to micelles, increase the concentration of monomers in micelles, enhance the swelling of polymer segments, and promote the chain growth reaction of fluoroethylene and ethylene. The method adopted by the present invention not only well regulates the polymer composition, but also effectively reduces the pressure of copolymerization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer preparation, and in particular to a method for preparing fluoroethylene-ethylene copolymer. Background Art

[0002] Polyvinyl fluoride (PVF) is widely used in chemical industry, electronics and electrical, aerospace, construction engineering, automobile industry, medical and other fields due to its excellent mechanical strength, chemical resistance, thermal stability, indoor functionality, outdoor durability, wear resistance and barrier properties. However, the application of polyvinyl fluoride products is largely limited by the processing method. The melting temperature (200~210℃) of polyvinyl fluoride is close to the decomposition temperature (210~220℃), and the processing window is narrow. It is not suitable for thermoplastic molding and can usually only be processed into films and coatings. By copolymerization modification, a small amount of fluorinated or non-fluorinated monomers, such as hexafluoropropylene, tetrafluoroethylene, trifluorochloroethylene, ethylene, etc., are introduced into the polymerization process of polyvinyl fluoride, which can not only improve the processing properties of polyvinyl fluoride polymers, but also improve the performance of polyvinyl fluoride polymers in specific applications. Among them, the introduction of a small amount of ethylene segments into the polyvinyl fluoride polymer chain can reduce the melting point of polyvinyl fluoride, making polyvinyl fluoride easy to process and form, and the obtained products also have improved properties in terms of flexibility and elasticity.

[0003] At present, there are literature reports on the modification of polyvinyl fluoride by introducing ethylene and vinyl fluoride copolymerization. U.S. Patents US2419008 and US2419009 disclose a method for preparing vinyl fluoride copolymers by emulsion polymerization, in which organic peroxide initiators are used in aqueous media to copolymerize vinyl fluoride and unsaturated monoolefins such as ethylene, propylene, butadiene, etc. under the preferred conditions of 10MPa~100MPa and 30℃~200℃. The prepared copolymers can be made into thin films, foils, sheets or strip products under high temperature and high pressure, and can also be used as coatings. Benzoyl peroxide initiator is used to initiate the copolymerization of vinyl fluoride and ethylene under the conditions of 80℃ and 30MPa, and the introduction ratio of vinyl fluoride to ethylene is 50:1. The generated white cake-like copolymer can be pressed into a transparent film at 200℃, and its hardness and toughness are similar to those of polyvinyl chloride, and its solubility in N,N-dimethylformamide solvent is better than that of vinyl fluoride homopolymer. Chinese patent CN108239214A discloses a method for continuous copolymerization of vinyl fluoride monomer and a second monomer using supercritical CO2 as a reaction medium and an azo and / or perfluoroperoxide initiator, wherein the second monomer is ethylene, propylene, isobutylene, vinyl chloride, vinyl butyric acid, vinyl acetate, etc., the mass ratio of the vinyl fluoride monomer to the second monomer is (40~500):1, the polymerization temperature and pressure range are 70℃~100℃, 15MPa~30MPa, respectively, and the prepared copolymer has improved melt processing performance and film adhesion performance.

[0004] The above-mentioned technologies introduce a small amount of ethylene and vinyl fluoride copolymerization to improve the processing properties of the polymer to a certain extent, but the pressure required for the polymerization reaction is very high, and the composition of vinyl fluoride and ethylene is not easy to control. In the actual industrial production process, the requirements for equipment, technology and safety are very high. The fundamental reason for these problems is related to the difference in the molecular structure of vinyl fluoride and ethylene. The vinyl fluoride molecule contains a highly electronegative F atom, while the ethylene molecule only contains C and H atoms, resulting in a great difference in the polarity of the two molecules and a great difference in solubility in water. The solubility parameter of ethylene is 12.437 (J / cm 3 ) 0.5 , while the solubility parameter of vinyl fluoride is 17.71 (J / cm 3 ) 0.5 Therefore, there is a big difference in the solubility of the two monomers in micelles during emulsion polymerization. The difference in structure between the two also leads to different diffusion behaviors. In the process of diffusion from the gas phase to water, vinyl fluoride can form hydrogen bonds with water molecules, so the diffusion rate is relatively fast, while ethylene has a weaker interaction with water molecules and a slower diffusion rate. When diffusing into micelles in water, vinyl fluoride is also more easily attracted to the polar region of the micelle due to its polarity, and the diffusion rate is faster, while ethylene has a weaker interaction with the micelle due to its non-polarity and a slower diffusion rate. This is manifested in the difficulty in controlling the ratio of ethylene to vinyl fluoride in micelles, which in turn affects the copolymerization ratio in the copolymer.

[0005] In view of the shortcomings of the prior art, the present invention proposes a new process for preparing a copolymer of vinyl fluoride and ethylene in combination with the dissolution and diffusion characteristics of the monomers and the characteristics of the emulsion polymerization method. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing vinyl fluoride-ethylene copolymer, solve the problem of high copolymerization reaction pressure when preparing vinyl fluoride and ethylene copolymer, and effectively regulate the composition of vinyl fluoride and ethylene monomer units in the polymer.

[0007] To achieve the above object, the present invention provides a method for preparing a fluoroethylene-ethylene copolymer, comprising the following steps:

[0008] S1. Add a surfactant and a mixed organic solvent to a reactor filled with pure water, add a halogen salt after stirring, stir and dissolve to obtain an emulsion containing an aqueous halogen salt solution, and introduce nitrogen to remove oxygen to obtain a uniform emulsion;

[0009] S2, heating the emulsion, then pumping vinyl fluoride monomer into the reactor, then pumping ethylene, and then pumping initiator solution, stirring and dissolving to obtain vinyl fluoride-ethylene copolymer emulsion;

[0010] S3, the reactor is cooled to room temperature, and then the pressure is released to normal pressure, nitrogen is introduced, and the reactor is stirred to remove residual vinyl fluoride and ethylene;

[0011] S4, filtering, washing and drying the solid-liquid mixture obtained in S3 to obtain a powdery resin product of fluoroethylene-ethylene copolymer.

[0012] In S1, the mixed organic solvent is a mixture of one of N,N-dimethylformamide and N,N-dimethylacetamide and high-carbon cycloalkanes, wherein the volume ratio of the two is 0.5-2, and the sum of the concentrations of the two is 0.25wt%-7.5wt%; the surfactant is a tetrahydrofuran-propylene oxide-ethylene oxide-propylene oxide-tetrahydrofuran ternary pentablock copolymer.

[0013] Preferably, the high carbon cycloalkane is one of cyclooctane, cyclononane and cyclodecane;

[0014] The tetrahydrofuran-propylene oxide-ethylene oxide-propylene oxide-tetrahydrofuran ternary five-block copolymer is , the chemical formula structure is as follows, where: n 1=15~75, n 2=25~80, n 3 = 20 ~ 45, concentration is 0.1wt% ~ 5.0wt%, .

[0015] Preferably, in S1, the halide salt is one or more of ammonium fluoride, sodium fluoride, potassium fluoride, ammonium chloride, sodium chloride and potassium chloride.

[0016] Preferably, in S1, the concentration of the brine solution is 0.5wt%~10wt%, the stirring speed is 300rpm~1000rpm, and the space velocity of the nitrogen is 5h -1 ~500h -1 The introduction time is 15min~60min, the oxygen in the reactor is eliminated, and the oxygen content is controlled to be less than 5ppm.

[0017] Preferably, in S2, the emulsion is heated to 60°C to 90°C, the amount of vinyl fluoride pumped in is 3.5MPa to 15.0MPa, and the amount of ethylene pumped in is 0.5MPa to 5MPa.

[0018] Preferably, in S2, the initiator is a water-soluble initiator, the concentration of the water-soluble initiator is 10wt%, and the initiator concentration in the fluoroethylene-ethylene copolymer emulsion is 0.25wt%~1.5wt%.

[0019] Preferably, the water-soluble initiator is one of ammonium persulfate and potassium persulfate.

[0020] Preferably, in S3, the space velocity of nitrogen introduction is 5h -1 ~500h -1 The introduction time is 15min~30min, and the vinyl fluoride and ethylene in the reactor are removed to control the total content of vinyl fluoride and ethylene to be less than 15ppm.

[0021] In order to control the solubility of vinyl fluoride and ethylene in water and micelles, the present invention adds a mixed organic solvent, so that the water contains a certain amount of solvent that can dissolve ethylene-vinyl fluoride, and the micelles contain solvent that can dissolve vinyl fluoride-ethylene, so as to promote the diffusion and dissolution of vinyl fluoride-ethylene from the gas phase to the water phase, promote the diffusion and dissolution of vinyl fluoride-ethylene dissolved in the water phase into the micelles, increase the concentration of vinyl fluoride-ethylene in the micelles, increase the polymerization reaction speed, and reduce the pressure of the polymerization reaction. At the same time, the solvent in the micelles has good solubility for the generated copolymer, keeps the active polymer with good chain growth activity, increases the molecular weight of the vinyl fluoride-ethylene copolymer, and controls the composition of the copolymer.

[0022] The high-carbon cycloalkanes in the mixed organic solvent can effectively improve the stability of the micelles, increase the diffusion of vinyl fluoride-ethylene into the micelles, improve the dissolution of the newly formed copolymer in the micelles, enhance the swelling of the ethylene chain segments, and promote the chain growth reaction of vinyl fluoride and ethylene monomers.

[0023] The present invention adds a ternary five-block copolymer with the following structure to improve the stability of micelles.

[0024] ;

[0025] It is obtained by ring-opening polymerization of ethylene oxide (EO), propylene oxide (PO) and tetrahydrofuran (THF) with ethylene glycol as the initiator, wherein the middle part is an ethylene oxide (EO) polymer segment, and the two sides of the EO segment are connected to propylene oxide (PO) segments, and the propylene oxide (PO) segments on both sides are respectively connected to tetrahydrofuran (THF) segments. When the surfactant is added to water to form an emulsion and reaches the critical micelle concentration, the polymer chain folds into a U shape, and the middle EO segment extends to the water phase. After the epoxy folds, the propylene oxide (PO) and tetrahydrofuran (THF) polymer segments extend to the inside of the micelle, forming a stable dissolved state with the mixed solvent in the micelle, capturing the vinyl fluoride and ethylene monomers from outside the micelle, stabilizing the micelle while increasing the concentration of vinyl fluoride and ethylene in the micelle, and reducing the polymerization reaction pressure. When vinyl fluoride and ethylene copolymers are generated in micelles, the PO and THF segments and the mixed solvent can synergistically swell / dissolve the copolymers, allowing vinyl fluoride and ethylene molecules to diffuse freely in the polymer, effectively regulating the polymerization reaction rate and copolymer composition.

[0026] The invention adds halide salt to adjust the distribution of mixed organic solvent in water phase and micelle, and changes the dissolution behavior of mixed organic solvent in water through the association of halide salt and water, thereby changing the distribution of solvent in water phase and micelle phase.

[0027] Through the synergistic effect of the above aspects, not only the micelles are well stabilized, the distribution of the mixed solvent in the aqueous phase and the micelles is adjusted, the diffusion rate of fluoroethylene-ethylene from the gas phase into the aqueous phase and from the aqueous phase into the micelles is enhanced, the concentration of monomers in the micelles is increased, the swelling / dissolution of the generated copolymer in the micelles is increased, the activity of the growing chain is increased, the polymer composition is regulated, the polymerization reaction rate is increased, and the pressure of the polymerization reaction system is reduced.

[0028] Therefore, the present invention provides a method for preparing fluoroethylene-ethylene copolymer, compared with the prior art, the specific beneficial effects are as follows:

[0029] (1) In the process of preparing the copolymer of vinyl fluoride and ethylene by the emulsion polymerization method provided by the present invention, a mixed solvent of one of N,N-dimethylformamide (DMF) and N,N-dimethylacetamide (DMAC) and a mixture of one of high-carbon cycloalkanes, such as cyclooctane (COA), cyclononane (CNA), and cyclodecane (CDC) is added, so that the water contains a certain amount of solvent that can dissolve ethylene-vinyl fluoride, and the micelles contain solvent that can dissolve vinyl fluoride-ethylene. The solvent in the micelles can accelerate the dissolution of the monomers, increase the concentration of the monomers in the micelles, and thus increase the polymerization reaction rate and reduce the polymerization pressure. At the same time, the high-carbon cycloalkanes in the mixed solvent can enhance the swelling of the ethylene chain segments and promote the chain growth reaction of vinyl fluoride and ethylene monomers, while N,N-dimethylformamide and N,N-dimethylacetamide can enhance the swelling of the vinyl fluoride chain segments and synergistically promote the chain growth reaction of vinyl fluoride and ethylene.

[0030] (2) In the process of preparing fluoroethylene and ethylene copolymer by emulsion polymerization provided by the present invention, a ternary five-block copolymer is used as a surfactant. The middle of the surfactant is an ethylene oxide polymer segment with good hydrophilicity, which extends into the water and can further adjust the particle size and stability of the micelle. The two ends are connected to moderately lipophilic propylene oxide polymer segments. In the emulsion, the surfactant folds into a U-shape, and the propylene oxide polymer segment and the tetrahydrofuran polymer segment extend into the micelle, forming a stable dissolved state with the mixed solvent in the micelle, capturing the fluoroethylene and ethylene monomers from outside the micelle, dissolving and stabilizing the micelle and increasing the concentration of fluoroethylene and ethylene in the micelle, thereby reducing the polymerization reaction pressure. The fluoroethylene-ethylene copolymer generated by dissolving allows the monomer to diffuse freely in the polymer chain, increasing the polymer molecular weight and adjusting the polymer composition.

[0031] (3) In the process of preparing the copolymer of fluoroethylene and ethylene by the emulsion polymerization method provided by the present invention, a halide salt is added. On the one hand, the halide salt helps to promote the diffusion of the monomer dissolved in water into the micelles, thereby increasing the concentration of the monomer in the micelles. On the other hand, the association of the halide salt with water can change the dissolution behavior of the mixed solvent in water, thereby changing the distribution of the solvent in the aqueous phase and the micelle phase.

[0032] The technical solution of the present invention is further described in detail below through embodiments. DETAILED DESCRIPTION

[0033] The present invention provides a method for preparing a fluoroethylene-ethylene copolymer, which specifically comprises the following steps:

[0034] S1. Add a surfactant and a mixed organic solvent to a reactor filled with pure water, start stirring to obtain an emulsion. Add a halide salt and dissolve it to obtain an emulsion containing a halide salt aqueous solution, and at the same time, introduce nitrogen to remove the air in the reactor to obtain a uniform emulsion.

[0035] Among them, the surfactant is a tetrahydrofuran (THF)-propylene oxide (PO)-ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF) ternary five-block copolymer, and the typical structure is ,in, n 1=15~75, n 2=25~80, n 3=20~45, the chemical formula structure is as follows. The concentration is 0.1wt%~5.0wt%.

[0036] ;

[0037] Structure of ternary pentablock copolymer surfactant.

[0038] The ternary pentablock copolymer surfactant is firstly obtained by anionic ring-opening polymerization and then by cationic ring-opening polymerization. The synthesis method is as follows:

[0039] (1) Add ethylene glycol and KOH to a flask, heat to 120°C, react to generate potassium ethylene glycol, and dehydrate under vacuum at 80°C for 1 hour. Pour into a high-pressure reactor while hot, and introduce nitrogen while stirring slowly to replace oxygen for 30 minutes. Start stirring at a speed of 200-300 rpm, and add propylene oxide (EO) monomer. The molar ratio of EO to ethylene glycol is ( n 3-1). Polymerize for 2 h at a temperature range of 80-120°C to obtain a polymerization degree of n 3. Ethylene oxide (EO) polymer with double end group of −OK.

[0040] (2) Add propylene oxide (PO) monomer into the kettle, the molar ratio of PO to ethylene glycol is 2n 2. Polymerize at a temperature range of 90-130°C for 2h to obtain a propylene oxide (PO)-ethylene oxide (EO) polymer with −OK as a double end group. After the polymerization is completed, fill with nitrogen and cool to room temperature.

[0041] (3) Adding an acid catalyst, such as p-toluenesulfonic acid, trifluorosulfonic acid, trifluoromethanesulfonic acid, or heteropolyacid, into the kettle, wherein the molar ratio of the added acid catalyst to KOH is 2:1, so that the terminal group of the polymer obtained in step (2) becomes an oxonium ion, thereby initiating a ring-opening polymerization reaction of THF.

[0042] (4) Add tetrahydrofuran (THF) monomer into the kettle, the molar ratio of THF to ethylene glycol is 2 n 1. Set the stirring speed to 200-300 rpm, adjust the reaction temperature to 40-80°C, and polymerize for 2.5 hours. After the reaction is completed, fill with nitrogen, cool to room temperature, and discharge to obtain a crude product of tetrahydrofuran (THF)-propylene oxide (PO)-ethylene oxide (EO) ternary five-block copolymer, which is then treated with alkali neutralization, purification, drying, etc. to obtain a ternary five-block copolymer product.

[0043] The mixed organic solvent is a mixture of one of N,N-dimethylformamide (DMF) and N,N-dimethylacetamide (DMAC) and a high carbon cycloalkane, such as cyclooctane (COA), cyclononane (CNA), and cyclodecane (CDC), that is, DMF-COA, DMF-CNA, DMF-CDC, DMAC-COA, DMAC-CNA, and DMAC-CDC, and the volume ratio of the two in the mixed organic solvent is 0.5-2, and the sum of the concentrations of the two is 0.25wt%-7.5wt%.

[0044] The halide salt is at least one of ammonium fluoride, sodium fluoride, potassium fluoride, ammonium chloride, sodium chloride and potassium chloride, preferably ammonium fluoride or potassium fluoride. The concentration of the halide salt aqueous solution is 0.5wt% to 10wt%. The stirring speed is 300rpm to 1000rpm. The space velocity of the nitrogen is 5h -1 ~500h -1 The introduction time is 15min~60min, the oxygen in the reactor is eliminated, and the oxygen content is controlled below 5ppm.

[0045] S2, heating the emulsion in S1 to 60℃~90℃, then first introduce vinyl fluoride monomer into the reactor, then introduce ethylene, pump in the initiator solution through a high-pressure pump, stir and dissolve while initiating polymerization of vinyl fluoride and ethylene to obtain an emulsion of fluorinated vinyl-ethylene copolymer. During the reaction, as vinyl fluoride and ethylene are consumed, the pressure will gradually decrease, and the pressure in the reactor is kept stable by replenishing vinyl fluoride and ethylene. After a certain reaction time, pump in the remaining initiator, replenish vinyl fluoride and ethylene, continue polymerization, control the polymerization conversion rate, terminate the reaction, and obtain a vinyl fluoride-ethylene copolymer emulsion.

[0046] The total amount of fluoroethylene pumped in is 3.5MPa~15.0MPa, and the total amount of ethylene pumped in is 0.5MPa~5MPa. The initiator is a water-soluble initiator such as ammonium persulfate and potassium persulfate. 30%~60% of the total amount of initiator is pumped into the reactor for the first time, and the concentration of the initiator aqueous solution is 10wt%, so that the initiator concentration in the emulsion is 0.25wt%~1.5wt%.

[0047] The polymerization time after the first addition of the initiator is 1h~4h, and the polymerization time after the addition of the remaining initiator is 2h~5h. During the reaction, the consumption of vinyl fluoride and ethylene in polymerization causes a pressure drop. Vinyl fluoride and ethylene are added to the polymerization kettle through a booster pump to maintain the pressure of the reactor. The addition ratio between the two is controlled by a mass flow meter in the pipeline.

[0048] S3. Cool the reactor to room temperature with jacket cooling water, slowly release the pressure to normal pressure, introduce nitrogen, stir, and remove the residual vinyl fluoride and ethylene.

[0049] In the S3, the space velocity of nitrogen is 5h -1 ~500h -1 The introduction time is 15min~30min, and the total content of vinyl fluoride and ethylene in the reactor is controlled to be less than 15ppm.

[0050] S4, filtering, washing and drying the solid-liquid mixture obtained in S3 to obtain a powdery resin product of fluoroethylene-ethylene copolymer.

[0051] The present invention is further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Any other changes, modifications, substitutions, combinations, simplifications made without violating the spirit and principle of the present invention should all be equivalent replacement methods and are included in the protection scope of the present invention. In addition, it should be understood that after reading the content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application, and all belong to the scope of protection of the present invention.

[0052] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The term "embodiment" appearing in various places in the specification does not necessarily refer to the same embodiment, nor does it particularly limit its independence or association with other embodiments. In principle, in the present application, as long as there is no technical contradiction or conflict, the various technical features mentioned in the embodiments can be combined in any way to form a corresponding implementable technical solution.

[0053] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.

[0054] Unless otherwise specified in the present invention, the reagents, instruments, and equipment used are those commonly used by technicians in this field.

[0055] Example 1

[0056] This embodiment provides a method for preparing a fluoroethylene-ethylene copolymer, comprising the following steps:

[0057] S1. Add THF to a reactor filled with pure water. 20 -(PO) 25 -(EO) 25 -(PO) 25 -(THF) 20 The surfactant was added to a mixture of N,N-dimethylformamide and cyclooctane (DMF-COA solvent) at a volume ratio of 1.0 and a concentration of 1.0wt%. The stirring was started to emulsify the mixture and the stirring speed was set to 300rpm. Potassium fluoride was then added to dissolve the mixture to obtain an emulsion containing an aqueous potassium fluoride solution at a concentration of 2.0wt%. Nitrogen was introduced at a space velocity of 80h / min. -1 The introduction time was 30 minutes, the air in the reactor was excluded, the oxygen content of the system was controlled to be 3.8ppm, and a uniform emulsion was obtained.

[0058] S2, turn on the heating, raise the temperature of the emulsion to 60°C, introduce 5.0MPa of vinyl fluoride into the reactor, then introduce 2.0MPa of ethylene, pump in an initiator accounting for 50% of the total amount of initiator, that is, a 10wt% ammonium persulfate solution through a high-pressure pump, stir and dissolve while initiating the polymerization of vinyl fluoride and ethylene to obtain an emulsion of fluorine-containing ethylene-ethylene copolymer, after reacting for 2.0h, pump in the remaining initiator to make the initiator concentration in the emulsion 1.0wt%, and continue polymerization for 2.0h. During the process, when the pressure drops, vinyl fluoride and ethylene are added to the reactor respectively through a booster pump, and the ratio between the two is controlled by a mass flow meter to maintain the pressure in the polymerization kettle at 7.0MPa. Control the polymerization conversion rate, terminate the reaction, and obtain a vinyl fluoride-ethylene copolymer emulsion.

[0059] S3, cool the reactor to room temperature through jacket cooling water, slowly release the pressure to normal pressure, and introduce nitrogen at a space velocity of 400h -1 The introduction time is 18 minutes, stirring is continued, residual vinyl fluoride and ethylene are removed, and the total content of vinyl fluoride and ethylene in the system is controlled to be 5.0 ppm.

[0060] S4, filtering, washing and drying the obtained solid-liquid mixture to obtain a fluoroethylene-ethylene copolymer powdered resin product.

[0061] Example 2

[0062] This embodiment provides a method for preparing a fluoroethylene-ethylene copolymer, comprising the following steps:

[0063] S1. Add THF to a reactor filled with pure water. 25 -(PO) 30 -(EO) 30 -(PO) 30 -(THF) 25 The surfactant was added to a mixture with a concentration of 2.0 wt %. A mixed solvent of N,N-dimethylacetamide and cyclodecane (DMAC-CDC solvent) was added with a volume ratio of 1.5 and a concentration of 4.5 wt %. Stirring was started to emulsify the mixture. The stirring speed was set to 600 rpm. Sodium fluoride and sodium chloride were added in a mass ratio of 1:1 to dissolve the mixture. An emulsion containing a sodium fluoride-sodium chloride aqueous solution was obtained with a concentration of 3.0 wt %. Nitrogen was introduced at a space velocity of 300 h -1 The introduction time was 26 minutes, the air in the reactor was excluded, the oxygen content of the system was controlled to be 2.4ppm, and a uniform emulsion was obtained.

[0064] S2, turn on the heating, raise the temperature of the emulsion to 80°C, introduce 8.5MPa of vinyl fluoride into the reactor, then introduce 1.5MPa of ethylene, pump in an initiator accounting for 60% of the total amount of initiator, i.e., a 10wt% ammonium persulfate solution, through a high-pressure pump, stir and dissolve while initiating polymerization of vinyl fluoride and ethylene to obtain an emulsion of fluorine-containing ethylene-ethylene copolymer, after reacting for 2.5h, pump in the remaining initiator to make the initiator concentration in the emulsion 0.25wt%, and continue polymerization for 2.5h. During the process, when the pressure drops, vinyl fluoride and ethylene are added to the reactor respectively through a booster pump, and the ratio between the two is controlled by a mass flow meter to maintain the pressure in the polymerization kettle at 10.0MPa. Control the polymerization conversion rate, terminate the reaction, and obtain a vinyl fluoride-ethylene copolymer emulsion.

[0065] S3, cool the reactor to room temperature through jacket cooling water, slowly release the pressure to normal pressure, and introduce nitrogen at a space velocity of 500h -1 The introduction time is 16 minutes, stirring is continued, residual vinyl fluoride and ethylene are removed, and the total content of vinyl fluoride and ethylene in the system is controlled to be 4.5ppm.

[0066] S4, filtering, washing and drying the obtained solid-liquid mixture to obtain a fluoroethylene-ethylene copolymer powdered resin product.

[0067] Example 3

[0068] This embodiment provides a method for preparing a fluoroethylene-ethylene copolymer, comprising the following steps:

[0069] S1. Add THF to a reactor filled with pure water. 35 -(PO) 75 -(EO) 40 -(PO) 75 -(THF) 35 The surfactant was added to a mixture of N,N-dimethylacetamide and cyclononane (DMAC-CNA solvent) at a volume ratio of 1.2 and a concentration of 7.5wt%. Stirring was started to emulsify the mixture at a stirring speed of 800rpm. Ammonium fluoride was then added to dissolve the mixture to obtain an emulsion containing an aqueous solution of ammonium fluoride at a concentration of 6.0wt%. Nitrogen was introduced at a space velocity of 100h / min. -1 The introduction time was 50 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 3.1 ppm, and a uniform emulsion was obtained.

[0070] S2, turn on the heating, raise the temperature of the emulsion to 85°C, introduce 13.5MPa of vinyl fluoride into the reactor, then introduce 3.5MPa of ethylene, pump in an initiator accounting for 45% of the total amount of initiator, that is, a potassium persulfate solution with a concentration of 10wt%, through a high-pressure pump, stir and dissolve while initiating the polymerization of vinyl fluoride and ethylene to obtain an emulsion of fluorine-containing ethylene-ethylene copolymer, after reacting for 1.0h, pump in the remaining initiator to make the initiator concentration in the emulsion 1.5wt%, and continue polymerization for 4.5h. During the process, when the pressure drops, vinyl fluoride and ethylene are added to the reactor respectively through a booster pump, and the ratio between the two is controlled by a mass flow meter to maintain the pressure in the polymerization kettle at 17.0MPa. Control the polymerization conversion rate, terminate the reaction, and obtain a vinyl fluoride-ethylene copolymer emulsion.

[0071] S3, cool the reactor to room temperature through jacket cooling water, slowly release the pressure to normal pressure, and introduce nitrogen at a space velocity of 200h -1 The introduction time is 22 minutes, stirring is continued, residual vinyl fluoride and ethylene are removed, and the total content of vinyl fluoride and ethylene in the system is controlled to be 8.4ppm.

[0072] S4, filtering, washing and drying the obtained solid-liquid mixture to obtain a fluoroethylene-ethylene copolymer powdered resin product.

[0073] Example 4

[0074] This embodiment provides a method for preparing a fluoroethylene-ethylene copolymer, comprising the following steps:

[0075] S1. Add THF to a reactor filled with pure water. 20 -(PO) 60 -(EO) 25 -(PO) 60 -(THF) 20 The surfactant was added to a mixture of N,N-dimethylformamide and cyclononane (DMF-CNA solvent) with a volume ratio of 2.0 and a concentration of 0.5wt%. The mixture was stirred to emulsify the mixture and the stirring speed was set to 300rpm. Sodium chloride was then added to dissolve the mixture to obtain an emulsion containing an aqueous sodium chloride solution with a concentration of 8.5wt%. Nitrogen was introduced at a space velocity of 500h / min. -1 The introduction time was 15 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 2.5 ppm, and a uniform emulsion was obtained.

[0076] S2, turn on the heating, raise the temperature of the emulsion to 90°C, introduce 8.0MPa of vinyl fluoride into the reactor, then introduce 0.5MPa of ethylene, pump in an initiator accounting for 35% of the total amount of initiator, that is, a potassium persulfate solution with a concentration of 10wt%, through a high-pressure pump, stir and dissolve while initiating the polymerization of vinyl fluoride and ethylene to obtain an emulsion of fluorine-containing ethylene-ethylene copolymer, after reacting for 3.0h, pump in the remaining initiator to make the initiator concentration in the emulsion 0.8wt%, and continue polymerization for 5.0h. During the process, when the pressure drops, vinyl fluoride and ethylene are added to the reactor respectively through a booster pump, and the ratio between the two is controlled by a mass flow meter to maintain the pressure in the polymerization kettle at 8.5MPa. Control the polymerization conversion rate, terminate the reaction, and obtain a vinyl fluoride-ethylene copolymer emulsion.

[0077] S3, cool the reactor to room temperature through jacket cooling water, slowly release the pressure to normal pressure, and introduce nitrogen at a space velocity of 100h -1 The introduction time is 25 minutes, stirring is continued, residual vinyl fluoride and ethylene are removed, and the total content of vinyl fluoride and ethylene in the system is controlled to be 11.0 ppm.

[0078] S4, filtering, washing and drying the obtained solid-liquid mixture to obtain a fluoroethylene-ethylene copolymer powdered resin product.

[0079] Example 5

[0080] This embodiment provides a method for preparing a fluoroethylene-ethylene copolymer, comprising the following steps:

[0081] S1. Add THF to a reactor filled with pure water. 45 -(PO) 50 -(EO) 40 -(PO) 50 -(THF) 45 The surfactant was added to a solution with a concentration of 3.0wt%, and a mixed solvent of N,N-dimethylacetamide and cyclooctane (DMAC-COA solvent) was added with a volume ratio of 0.6 and a concentration of 6.0wt%. Stirring was started to emulsify the solution, and the stirring speed was set to 400rpm. Potassium fluoride and potassium chloride were added to the solution with a mass ratio of 1:1 to dissolve the solution, and an emulsion containing a potassium fluoride-potassium chloride aqueous solution with a concentration of 4.0wt% was obtained. Nitrogen was introduced at a space velocity of 400h -1 The introduction time was 20 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 2.2 ppm, and a uniform emulsion was obtained.

[0082] S2. Turn on the heating, raise the temperature of the emulsion to 70°C, introduce 12.0MPa of vinyl fluoride into the reactor, then introduce 4.0MPa of ethylene, pump in an initiator accounting for 30% of the total amount of initiator, i.e., a 10wt% ammonium persulfate solution, through a high-pressure pump, stir and dissolve while initiating polymerization of vinyl fluoride and ethylene to obtain an emulsion of fluorine-containing ethylene-ethylene copolymer, after reacting for 3.0h, pump in the remaining initiator to make the initiator concentration in the emulsion 0.6wt%, and continue polymerization for 4.0h. During the process, when the pressure drops, vinyl fluoride and ethylene are added to the reactor respectively through a booster pump, and the ratio between the two is controlled by a mass flow meter to maintain the pressure in the polymerization kettle at 16.0MPa. Control the polymerization conversion rate, terminate the reaction, and obtain a vinyl fluoride-ethylene copolymer emulsion.

[0083] S3, cool the reactor to room temperature through jacket cooling water, slowly release the pressure to normal pressure, and introduce nitrogen at a space velocity of 350h -1 The introduction time is 20 minutes, stirring is continued, residual vinyl fluoride and ethylene are removed, and the total content of vinyl fluoride and ethylene in the system is controlled to be 5.1ppm.

[0084] S4, filtering, washing and drying the obtained solid-liquid mixture to obtain a fluoroethylene-ethylene copolymer powdered resin product.

[0085] Example 6

[0086] This embodiment provides a method for preparing a fluoroethylene-ethylene copolymer, comprising the following steps:

[0087] S1. Add THF to a reactor filled with pure water. 40 -(PO) 70 -(EO) 20 -(PO) 70 -(THF) 40 A surfactant with a concentration of 5.0wt% was added, and a mixed solvent of N,N-dimethylformamide and cyclononane (DMF-CNA solvent) was added, with a volume ratio of 1.0 and a concentration of 0.25wt%. Stirring was started to emulsify it, and the stirring speed was set to 900rpm. Potassium chloride was then added thereto to dissolve, and an emulsion containing an aqueous potassium chloride solution with a concentration of 10.0wt% was obtained. Nitrogen was introduced at a space velocity of 350h -1 The introduction time was 35 minutes, the air in the reactor was excluded, the oxygen content of the system was controlled to be 1.5ppm, and a uniform emulsion was obtained.

[0088] S2, turn on the heating, raise the temperature of the emulsion to 65°C, introduce 3.5MPa of vinyl fluoride into the reactor, then introduce 3.0MPa of ethylene, pump in an initiator accounting for 50% of the total amount of initiator, that is, a potassium persulfate solution with a concentration of 10wt%, through a high-pressure pump, stir and dissolve while initiating the polymerization of vinyl fluoride and ethylene to obtain an emulsion of fluorine-containing ethylene-ethylene copolymer, after reacting for 4.0h, pump in the remaining initiator to make the initiator concentration in the emulsion 1.4wt%, and continue polymerization for 4.0h. During the process, when the pressure drops, vinyl fluoride and ethylene are added to the reactor respectively through a booster pump, and the ratio between the two is controlled by a mass flow meter to maintain the pressure in the polymerization kettle at 6.5MPa. Control the polymerization conversion rate, terminate the reaction, and obtain a vinyl fluoride-ethylene copolymer emulsion.

[0089] S3, cool the reactor to room temperature through jacket cooling water, slowly release the pressure to normal pressure, and introduce nitrogen at a space velocity of 250h -1 The introduction time is 19 minutes, stirring is continued, residual vinyl fluoride and ethylene are removed, and the total content of vinyl fluoride and ethylene in the system is controlled to be 8.0 ppm.

[0090] S4, filtering, washing and drying the obtained solid-liquid mixture to obtain a fluoroethylene-ethylene copolymer powdered resin product.

[0091] Example 7

[0092] This embodiment provides a method for preparing a fluoroethylene-ethylene copolymer, comprising the following steps:

[0093] S1. Add THF to a reactor filled with pure water. 45 -(PO) 45 -(EO) 20 -(PO) 45 -(THF) 45 The surfactant was added to a mixture of N,N-dimethylformamide and cyclodecane (DMF-CDC solvent) at a volume ratio of 0.5 and a concentration of 2.5wt%. The mixture was stirred at 700rpm to emulsify the mixture. Sodium fluoride was added to the mixture to dissolve the mixture. An emulsion containing an aqueous sodium fluoride solution was obtained at a concentration of 0.5wt%. Nitrogen was introduced at a space velocity of 5h -1 The introduction time was 55 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 4.8 ppm, and a uniform emulsion was obtained.

[0094] S2, turn on the heating, raise the temperature of the emulsion to 75°C, introduce 10.0MPa of vinyl fluoride into the reactor, then introduce 2.0MPa of ethylene, pump in an initiator accounting for 30% of the total amount of initiator, that is, a potassium persulfate solution with a concentration of 10wt%, through a high-pressure pump, stir and dissolve while initiating the polymerization of vinyl fluoride and ethylene to obtain an emulsion of fluorine-containing ethylene-ethylene copolymer, after reacting for 2.0h, pump in the remaining initiator to make the initiator concentration in the emulsion 0.4wt%, and continue polymerization for 3.5h. During the process, when the pressure drops, vinyl fluoride and ethylene are added to the reactor respectively through a booster pump, and the ratio between the two is controlled by a mass flow meter to maintain the pressure in the polymerization kettle at 12.0MPa. Control the polymerization conversion rate, terminate the reaction, and obtain a vinyl fluoride-ethylene copolymer emulsion.

[0095] S3, cool the reactor to room temperature through jacket cooling water, slowly release the pressure to normal pressure, and introduce nitrogen at a space velocity of 450h -1 The introduction time is 15 minutes, stirring is continued, residual vinyl fluoride and ethylene are removed, and the total content of vinyl fluoride and ethylene in the system is controlled to be 5.2ppm.

[0096] S4, filtering, washing and drying the obtained solid-liquid mixture to obtain a fluoroethylene-ethylene copolymer powdered resin product.

[0097] Example 8

[0098] This embodiment provides a method for preparing a fluoroethylene-ethylene copolymer, comprising the following steps:

[0099] S1. Add THF to a reactor filled with pure water. 30 -(PO) 55 -(EO) 40 -(PO) 55 -(THF) 30 The surfactant was added to a mixture of N,N-dimethylformamide and cyclooctane (DMF-COA solvent) at a volume ratio of 0.8 and a concentration of 7.0wt%. Stirring was started to emulsify the mixture. The stirring speed was set to 450rpm. Ammonium chloride was added to the mixture to dissolve the mixture. An emulsion containing an aqueous solution of ammonium chloride was obtained. The concentration was 1.5wt%. Nitrogen was introduced at a space velocity of 200h / min. -1 The introduction time was 40 minutes, the air in the reactor was excluded, the oxygen content of the system was controlled to be 2.2ppm, and a uniform emulsion was obtained.

[0100] S2, turn on the heating, raise the temperature of the emulsion to 90°C, introduce 15.0MPa of vinyl fluoride into the reactor, then introduce 5.0MPa of ethylene, pump in an initiator accounting for 40% of the total amount of initiator, i.e., a 10wt% ammonium persulfate solution, through a high-pressure pump, stir and dissolve while initiating polymerization of vinyl fluoride and ethylene to obtain an emulsion of fluorine-containing ethylene-ethylene copolymer, after reacting for 3.5h, pump in the remaining initiator to make the initiator concentration in the emulsion 0.7wt%, and continue polymerization for 3.0h. During the process, when the pressure drops, vinyl fluoride and ethylene are added to the reactor respectively through a booster pump, and the ratio between the two is controlled by a mass flow meter to maintain the pressure in the polymerization kettle at 20.0MPa. Control the polymerization conversion rate, terminate the reaction, and obtain a vinyl fluoride-ethylene copolymer emulsion.

[0101] S3, cool the reactor to room temperature through jacket cooling water, slowly release the pressure to normal pressure, and introduce nitrogen at a space velocity of 5h -1 The introduction time is 30 minutes, stirring is continued, residual vinyl fluoride and ethylene are removed, and the total content of vinyl fluoride and ethylene in the system is controlled to be 14.6ppm.

[0102] S4, filtering, washing and drying the obtained solid-liquid mixture to obtain a fluoroethylene-ethylene copolymer powdered resin product.

[0103] Example 9

[0104] This embodiment provides a method for preparing a fluoroethylene-ethylene copolymer, comprising the following steps:

[0105] S1. Add THF to a reactor filled with pure water. 35 -(PO) 80 -(EO) 35 -(PO) 80 -(THF) 35 The surfactant was added to a mixture of N,N-dimethylacetamide and cyclodecane (DMAC-CDC solvent) at a volume ratio of 0.75 and a concentration of 5.0wt%. Stirring was started to emulsify the mixture. The stirring speed was set to 500rpm. Ammonium fluoride and ammonium chloride were added at a mass ratio of 1:1 to dissolve the mixture. An emulsion containing an ammonium fluoride-ammonium chloride aqueous solution was obtained with a concentration of 7.0wt%. Nitrogen was introduced at a space velocity of 250h -1 The introduction time was 45 minutes, the air in the reactor was excluded, the oxygen content of the system was controlled to be 1.8ppm, and a uniform emulsion was obtained.

[0106] S2, turn on the heating, raise the temperature of the emulsion to 75°C, introduce 9.0MPa of vinyl fluoride into the reactor, then introduce 2.5MPa of ethylene, pump in an initiator accounting for 60% of the total amount of initiator, that is, a 10wt% ammonium persulfate solution through a high-pressure pump, stir and dissolve while initiating the polymerization of vinyl fluoride and ethylene to obtain an emulsion of fluorine-containing ethylene-ethylene copolymer, after reacting for 1.5h, pump in the remaining initiator to make the initiator concentration in the emulsion 0.5wt%, and continue polymerization for 5.0h. During the process, when the pressure drops, vinyl fluoride and ethylene are added to the reactor respectively through a booster pump, and the ratio between the two is controlled by a mass flow meter to maintain the pressure in the polymerization kettle at 11.5MPa. Control the polymerization conversion rate, terminate the reaction, and obtain a vinyl fluoride-ethylene copolymer emulsion.

[0107] S3, cool the reactor to room temperature through jacket cooling water, slowly release the pressure to normal pressure, and introduce nitrogen at a space velocity of 50h -1 The introduction time is 28 minutes, stirring is continued, residual vinyl fluoride and ethylene are removed, and the total content of vinyl fluoride and ethylene in the system is controlled to be 13.2ppm.

[0108] Example 10

[0109] This embodiment provides a method for preparing a fluoroethylene-ethylene copolymer, comprising the following steps:

[0110] S1. Add THF to a reactor filled with pure water. 25 -(PO) 35 -(EO) 45 -(PO) 35 -(THF) 25 The surfactant was added to a mixture of N,N-dimethylacetamide and cyclooctane (DMAC-COA solvent) at a volume ratio of 0.5 and a concentration of 4.0wt%. Stirring was started to emulsify the mixture. The stirring speed was set to 1000rpm. Ammonium fluoride was added thereto to dissolve the mixture. An emulsion containing an aqueous solution of ammonium fluoride was obtained. The concentration was 5.5wt%. Nitrogen was introduced at a space velocity of 50h. -1 The introduction time was 60 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 4.1 ppm, and a uniform emulsion was obtained.

[0111] S2, turn on the heating, raise the temperature of the emulsion to 85°C, introduce 7.5MPa of vinyl fluoride into the reactor, then introduce 2.5MPa of ethylene, pump in an initiator accounting for 55% of the total amount of initiator, that is, a potassium persulfate solution with a concentration of 10wt%, through a high-pressure pump, stir and dissolve while initiating the polymerization of vinyl fluoride and ethylene to obtain an emulsion of fluorine-containing ethylene-ethylene copolymer, after reacting for 3.0h, pump in the remaining initiator to make the initiator concentration in the emulsion 1.2wt%, and continue polymerization for 2.5h. During the process, when the pressure drops, vinyl fluoride and ethylene are added to the reactor respectively through a booster pump, and the ratio between the two is controlled by a mass flow meter to maintain the pressure in the polymerization kettle at 10.0MPa. Control the polymerization conversion rate, terminate the reaction, and obtain a vinyl fluoride-ethylene copolymer emulsion.

[0112] S3, cool the reactor to room temperature through jacket cooling water, slowly release the pressure to normal pressure, and introduce nitrogen at a space velocity of 300h -1 The introduction time is 25 minutes, stirring is continued, residual vinyl fluoride and ethylene are removed, and the total content of vinyl fluoride and ethylene in the system is controlled to be 4.8ppm.

[0113] S4, filtering, washing and drying the obtained solid-liquid mixture to obtain a fluoroethylene-ethylene copolymer powdered resin product.

[0114] The reaction pressure during the reaction of Examples 1-10, the number average molecular weight of the obtained vinyl fluoride-ethylene copolymer, and the vinyl fluoride content in the copolymer were measured. The specific results are shown in Table 1.

[0115] From the data in Table 1, it can be seen that the number average molecular weight of the fluoroethylene-ethylene copolymer powdered resin product prepared in Examples 1-10 is between 250,000 and 350,000, and the content of fluoroethylene in the copolymer is mainly concentrated in the range of 67% to 95%.

[0116] Comparative Example 1

[0117] This comparative example provides a method for preparing a fluoroethylene-ethylene copolymer, comprising the following steps:

[0118] S1. Add the surfactant sodium dodecyl sulfate to a reactor filled with pure water at a concentration of 5.0wt%, add a mixed solvent of N,N-dimethylacetamide and cyclooctane (DMAC-COA solvent) at a volume ratio of 0.5 and a concentration of 4.0wt%, start stirring to emulsify it, set the stirring speed to 1000rpm, then add ammonium fluoride to dissolve it to obtain an emulsion containing an ammonium fluoride aqueous solution at a concentration of 5.5wt%, and introduce nitrogen at a space velocity of 50h -1 The introduction time was 60 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 4.1 ppm, and a uniform emulsion was obtained.

[0119] S2, turn on the heating, raise the temperature of the emulsion to 85°C, introduce 7.5MPa of vinyl fluoride into the reactor, then introduce 2.5MPa of ethylene, pump in an initiator accounting for 55% of the total amount of initiator, that is, a potassium persulfate solution with a concentration of 10wt%, through a high-pressure pump, stir and dissolve while initiating the polymerization of vinyl fluoride and ethylene to obtain an emulsion of fluorine-containing ethylene-ethylene copolymer, after reacting for 3.0h, pump in the remaining initiator to make the initiator concentration in the emulsion 1.2wt%, and continue polymerization for 2.5h. During the process, when the pressure drops, vinyl fluoride and ethylene are added to the reactor respectively through a booster pump, and the ratio between the two is controlled by a mass flow meter to maintain the pressure in the polymerization kettle at 10.0MPa. Control the polymerization conversion rate, terminate the reaction, and obtain a vinyl fluoride-ethylene copolymer emulsion.

[0120] S3, cool the reactor to room temperature through jacket cooling water, slowly release the pressure to normal pressure, and introduce nitrogen at a space velocity of 300h -1 The introduction time is 25 minutes, stirring is continued, residual vinyl fluoride and ethylene are removed, and the total content of vinyl fluoride and ethylene in the system is controlled to be 4.8ppm.

[0121] S4, filtering, washing and drying the obtained solid-liquid mixture to obtain a fluoroethylene-ethylene copolymer powdered resin product.

[0122] The reaction pressure during the reaction of this comparative example, as well as the number average molecular weight of the obtained vinyl fluoride-ethylene copolymer and the vinyl fluoride content in the copolymer were measured. The specific results are shown in Table 1.

[0123] From the data in Table 1, it can be seen that the number average molecular weight of the vinyl fluoride-ethylene copolymer prepared by using the surfactant sodium dodecyl sulfate instead of the surfactant tetrahydrofuran (THF)-propylene oxide (PO)-ethylene oxide (EO) ternary pentablock copolymer is 41,000, and the content of vinyl fluoride in the copolymer is 45%. The polymerization effect is not as good as that of the surfactant tetrahydrofuran (THF)-propylene oxide (PO)-ethylene oxide (EO) ternary pentablock copolymer.

[0124] Comparative Example 2

[0125] This comparative example provides a method for preparing a fluoroethylene-ethylene copolymer, comprising the following steps:

[0126] S1. Add THF to a reactor filled with pure water. 35 -(PO) 75 -(EO) 40 -(PO) 75 -(THF) 35The surfactant was added to a mixture of N,N-dimethylformamide and acetone (DMF-Ace solvent) at a volume ratio of 0.5 and a concentration of 0.6wt%. Stirring was started to emulsify the mixture. The stirring speed was set to 800rpm. Ammonium fluoride was added thereto to dissolve the mixture. An emulsion containing an aqueous solution of ammonium fluoride was obtained. The concentration was 6.0wt%. Nitrogen was introduced at a space velocity of 100h / min. -1 The introduction time was 50 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 3.1 ppm, and a uniform emulsion was obtained.

[0127] S2, turn on the heating, raise the temperature of the emulsion to 85°C, introduce 13.5MPa of vinyl fluoride into the reactor, then introduce 3.5MPa of ethylene, pump in an initiator accounting for 45% of the total amount of initiator, that is, a potassium persulfate solution with a concentration of 10wt%, through a high-pressure pump, stir and dissolve while initiating the polymerization of vinyl fluoride and ethylene to obtain an emulsion of fluorine-containing ethylene-ethylene copolymer, after reacting for 1.0h, pump in the remaining initiator to make the initiator concentration in the emulsion 1.5wt%, and continue polymerization for 4.5h. During the process, when the pressure drops, vinyl fluoride and ethylene are added to the reactor respectively through a booster pump, and the ratio between the two is controlled by a mass flow meter to maintain the pressure in the polymerization kettle at 17.0MPa. Control the polymerization conversion rate, terminate the reaction, and obtain a vinyl fluoride-ethylene copolymer emulsion.

[0128] S3, cool the reactor to room temperature through jacket cooling water, slowly release the pressure to normal pressure, and introduce nitrogen at a space velocity of 200h -1 The introduction time is 22 minutes, stirring is continued, residual vinyl fluoride and ethylene are removed, and the total content of vinyl fluoride and ethylene in the system is controlled to be 8.4ppm.

[0129] S4, filtering, washing and drying the obtained solid-liquid mixture to obtain a fluoroethylene-ethylene copolymer powdered resin product.

[0130] The reaction pressure during the reaction of this comparative example, as well as the number average molecular weight of the obtained vinyl fluoride-ethylene copolymer and the vinyl fluoride content in the copolymer were measured. The specific results are shown in Table 1.

[0131] From the data in Table 1, it can be seen that the number average molecular weight of the fluoroethylene-ethylene copolymer prepared using a mixed solvent of N,N-dimethylformamide and acetone is 48,000, and the content of fluoroethylene in the copolymer is 47%. The polymerization effect is not as good as that using a mixed solvent of N,N-dimethylformamide or N,N-dimethylacetamide with cyclooctane, cyclononane or cyclodecane.

[0132] Comparative Example 3

[0133] This comparative example provides a method for preparing a fluoroethylene-ethylene copolymer, comprising the following steps:

[0134] S1. Add THF to a reactor filled with pure water. 45 -(PO) 50 -(EO) 40 -(PO) 50 -(THF) 45 The surfactant was added at a concentration of 3.0wt%, and a mixed solvent of N,N-dimethylacetamide and cyclooctane (DMAC-COA solvent) was added at a volume ratio of 0.6 and a concentration of 6.0wt%. Stirring was started to emulsify the mixture, and the stirring speed was set to 400rpm. Nitrogen was introduced at a space velocity of 400h -1 The introduction time was 20 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 2.2 ppm, and a uniform emulsion was obtained.

[0135] S2. Turn on the heating, raise the temperature of the emulsion to 70°C, introduce 12.0MPa of vinyl fluoride into the reactor, then introduce 4.0MPa of ethylene, pump in an initiator accounting for 30% of the total amount of initiator, i.e., a 10wt% ammonium persulfate solution, through a high-pressure pump, stir and dissolve while initiating polymerization of vinyl fluoride and ethylene to obtain an emulsion of fluorine-containing ethylene-ethylene copolymer, after reacting for 3.0h, pump in the remaining initiator to make the initiator concentration in the emulsion 0.6wt%, and continue polymerization for 4.0h. During the process, when the pressure drops, vinyl fluoride and ethylene are added to the reactor respectively through a booster pump, and the ratio between the two is controlled by a mass flow meter to maintain the pressure in the polymerization kettle at 16.0MPa. Control the polymerization conversion rate, terminate the reaction, and obtain a vinyl fluoride-ethylene copolymer emulsion.

[0136] S3, cool the reactor to room temperature through jacket cooling water, slowly release the pressure to normal pressure, and introduce nitrogen at a space velocity of 350h -1 The introduction time is 20 minutes, stirring is continued, residual vinyl fluoride and ethylene are removed, and the total content of vinyl fluoride and ethylene in the system is controlled to be 5.1ppm.

[0137] S4, filtering, washing and drying the obtained solid-liquid mixture to obtain a fluoroethylene-ethylene copolymer powdered resin product.

[0138] The reaction pressure during the reaction of this comparative example, as well as the number average molecular weight of the obtained vinyl fluoride-ethylene copolymer and the vinyl fluoride content in the copolymer were measured. The specific results are shown in Table 1.

[0139] From the data in Table 1, it can be seen that the number average molecular weight of the fluoroethylene-ethylene copolymer prepared without adding halide salt is 39,000, the content of fluoroethylene in the copolymer is 40%, and the polymerization effect is not as good as that of adding halide salt.

[0140] Comparative Example 4

[0141] This comparative example provides a method for preparing a fluoroethylene-ethylene copolymer, comprising the following steps:

[0142] S1. Add the surfactant sodium dodecyl sulfate to a reactor filled with pure water at a concentration of 4.5wt%, start stirring to emulsify it, set the stirring speed to 300rpm, and introduce nitrogen at a space velocity of 500h / min. -1 The introduction time was 15 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 4.0 ppm, and a uniform emulsion was obtained.

[0143] S2, turn on the heating, raise the temperature of the emulsion to 90°C, introduce 8.0MPa of vinyl fluoride into the reactor, then introduce 0.5MPa of ethylene, pump in an initiator accounting for 35% of the total amount of initiator, i.e., a 10wt% ammonium persulfate solution, through a high-pressure pump, stir and dissolve while initiating polymerization of vinyl fluoride and ethylene to obtain an emulsion of fluorine-containing ethylene-ethylene copolymer, after reacting for 3.0h, pump in the remaining initiator to make the initiator concentration in the emulsion 0.8wt%, and continue polymerization for 5.0h. During the process, when the pressure drops, vinyl fluoride and ethylene are added to the reactor respectively through a booster pump, and the ratio between the two is controlled by a mass flow meter to maintain the pressure in the polymerization kettle at 8.5MPa. Control the polymerization conversion rate, terminate the reaction, and obtain a vinyl fluoride-ethylene copolymer emulsion.

[0144] S3, cool the reactor to room temperature through jacket cooling water, slowly release the pressure to normal pressure, and introduce nitrogen at a space velocity of 100h -1 The introduction time is 25 minutes, stirring is continued, residual vinyl fluoride and ethylene are removed, and the total content of vinyl fluoride and ethylene in the system is controlled to be 11.0 ppm.

[0145] S4, filtering, washing and drying the obtained solid-liquid mixture to obtain a fluoroethylene-ethylene copolymer powdered resin product.

[0146] The reaction pressure during the reaction of this comparative example, as well as the number average molecular weight of the obtained vinyl fluoride-ethylene copolymer and the vinyl fluoride content in the copolymer were measured. The specific results are shown in Table 1.

[0147] From the data in Table 1, it can be seen that the number average molecular weight of the fluoroethylene-ethylene copolymer prepared by using the surfactant sodium dodecyl sulfate without using the surfactant tetrahydrofuran (THF)-propylene oxide (PO)-ethylene oxide (EO) ternary five-block copolymer and without adding a mixed solvent and a halogen salt is 28,000, and the content of fluoroethylene in the copolymer is 30%. The polymerization effect is not as good as that of the surfactant tetrahydrofuran (THF)-propylene oxide (PO)-ethylene oxide (EO) ternary five-block copolymer and adding a mixed solvent and a halogen salt.

[0148] Table 1

[0149] ;

[0150] In summary, the present invention uses a mixture of one of N,N-dimethylformamide (DMF) and N,N-dimethylacetamide (DMAC) and a high-carbon cycloalkane, such as cyclooctane (COA), cyclononane (CNA), and cyclodecane (CDC) as a mixed organic solvent, a ternary pentablock copolymer as a surfactant, and a halogen salt is added. Through the synergistic effect of the above aspects, the micelles are well stabilized, the distribution of the mixed solvent in the water phase and the micelles is adjusted, the diffusion rate of fluoroethylene-ethylene from the gas phase into the water phase and from the water phase into the micelles is enhanced, the concentration of the monomers in the micelles is increased, the swelling / dissolution of the generated copolymer in the micelles is increased, the activity of the growing chain is increased, the polymer composition is regulated, the polymerization reaction rate is increased, and the pressure of the polymerization reaction system is reduced.

[0151] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a fluoroethylene-ethylene copolymer, characterized in that: The following steps are involved: S1. Add a surfactant and a mixed organic solvent to a reactor filled with pure water, add a halogen salt after stirring, stir and dissolve to obtain an emulsion containing a halogen salt aqueous solution, and introduce nitrogen to remove oxygen to obtain a uniform emulsion; S2, heating the emulsion, then pumping vinyl fluoride monomer into the reactor, then pumping ethylene, and then pumping initiator solution, stirring and dissolving to obtain vinyl fluoride-ethylene copolymer emulsion; S3, the reactor is cooled to room temperature, and then the pressure is released to normal pressure, nitrogen is introduced, and the reactor is stirred to remove residual vinyl fluoride and ethylene; S4, filtering, washing and drying the solid-liquid mixture obtained in S3 to obtain a powdered resin product of fluoroethylene-ethylene copolymer; In S1, the mixed organic solvent is a mixture of one of N,N-dimethylformamide and N,N-dimethylacetamide and high-carbon cycloalkanes, wherein the volume ratio of the two is 0.5-2, and the sum of the concentrations of the two is 0.25wt%-7.5wt%; the surfactant is a tetrahydrofuran-propylene oxide-ethylene oxide-propylene oxide-tetrahydrofuran ternary five-block copolymer; the halide salt is one or more of ammonium fluoride, sodium fluoride, potassium fluoride, ammonium chloride, sodium chloride, and potassium chloride; Wherein, the high carbon cycloalkane is one of cyclooctane, cyclononane and cyclodecane.

2. A method for preparing a fluoroethylene-ethylene copolymer according to claim 1, characterized in that: The tetrahydrofuran-propylene oxide-ethylene oxide-propylene oxide-tetrahydrofuran ternary five-block copolymer is , the chemical formula structure is as follows, where: n 1=15~75, n 2=25~80, n 3 = 20 ~ 45, concentration is 0.1wt% ~ 5.0wt%, 。 3. The method for preparing a fluoroethylene-ethylene copolymer according to claim 1, characterized in that: In S1, the concentration of the brine solution is 0.5 wt% to 10 wt%, the stirring speed is 300 rpm to 1000 rpm, and the space velocity of the nitrogen is 5 h −1 ~500h −1 The introduction time is 15min~60min, the oxygen in the reactor is eliminated, and the oxygen content is controlled to be less than 5ppm.

4. The method for preparing a fluoroethylene-ethylene copolymer according to claim 1, characterized in that: In S2, the emulsion is heated to 60°C to 90°C, the amount of vinyl fluoride pumped in is 3.5MPa to 15.0MPa, and the amount of ethylene pumped in is 0.5MPa to 5MPa.

5. The method for preparing a fluoroethylene-ethylene copolymer according to claim 1, characterized in that: In S2, the initiator is a water-soluble initiator, the concentration of the water-soluble initiator is 10wt%, and the concentration of the initiator in the fluoroethylene-ethylene copolymer emulsion is 0.25wt%~1.5wt%.

6. A method for preparing a fluoroethylene-ethylene copolymer according to claim 5, characterized in that: The water-soluble initiator is one of ammonium persulfate and potassium persulfate.

7. The method for preparing a fluoroethylene-ethylene copolymer according to claim 1, characterized in that: In S3, the space velocity of nitrogen introduction is 5h −1 ~500h −1 The introduction time is 15min~30min, and the vinyl fluoride and ethylene in the reactor are removed to control the total content of vinyl fluoride and ethylene to be less than 15ppm.