A composite perfluorosulfonic acid proton exchange membrane and preparation method thereof
By using the hot pressing forming technology of long-branched and short-branched resins in perfluorosulfonic acid proton exchange membrane, the contradiction between the proton conduction ability and vanadium ion barrier properties is solved, and a high-efficiency energy exchange membrane is achieved The preparation of the whole vanadium redox flow battery has improved the performance of all vanadium redox flow battery.
Patent Information
- Application Number
- CN202411077674.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-07
AI Technical Summary
The existing perfluorosulfonic acid proton exchange membranes are difficult to maintain high vanadium ion barrier properties while improving the proton conduction ability, resulting in low conductivity and low energy efficiency, limiting their application in all vanadium oxidation and reduction flow batteries.
Long-branched and short-branched perfluorosulfonic acid resins are respectively coated and molded by hot pressing to form a composite perfluorosulfonic acid proton exchange membrane to enhance proton conduction capacity and block vanadium ion penetration.
The proton conduction ability and energy efficiency of the composite membrane are significantly improved, the electrochemical performance of the flow cell, especially the energy efficiency, and the morphological stability of the membrane is maintained.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of proton exchange membranes, and in particular relates to a composite perfluorosulfonic acid proton exchange membrane and a preparation method thereof. Background Art
[0002] Since renewable clean energy such as wind energy and solar energy is discontinuous and unstable, it is necessary to equip it with a high-performance energy storage system to improve the effective utilization of energy. All-vanadium redox flow battery (VRBS) has many advantages such as long life and high charge and discharge efficiency, making it an ideal choice. Perfluorosulfonic acid proton exchange membrane, as a key material in the VRBS system, plays the role of conducting protons. The proton exchange membrane separates the half-cell, prevents the mixing of electrolytes, and transfers protons between electrodes. The ideal characteristics of the membrane are low permeability to vanadium ions, high proton conductivity, and mechanical and chemical stability. Perfluoro Nafion membrane is commonly used in VRB because it meets most of the above characteristics, but it is expensive. In order to reduce costs, it is technically necessary to operate at high electrical density, so the proton membrane needs to have higher proton conductivity, but still maintain good vanadium ion barrier performance. Therefore, how to obtain an ion exchange membrane with both high ion conductivity and ion selectivity, as well as high energy efficiency, is a difficult problem and focus of current research. Summary of the invention
[0003] In order to overcome the defects of the prior art perfluorosulfonic acid proton exchange membrane that cannot simultaneously have excellent proton conductivity and vanadium ion permeation barrier performance, and has low conductivity and low energy efficiency, the present invention provides a composite perfluorosulfonic acid proton exchange membrane and a preparation method thereof. The composite perfluorosulfonic acid membrane prepared by the present invention not only improves proton conductivity but also blocks vanadium ion permeation, and greatly improves conductivity and energy efficiency.
[0004] The first aspect of the present invention provides a method for preparing a composite perfluorosulfonic acid proton exchange membrane, the method comprising the following steps:
[0005] (1) dissolving a long-chain branched perfluorosulfonic acid resin in a first organic solvent to obtain a first membrane-forming solution; dissolving a short-chain branched perfluorosulfonic acid resin in a second organic solvent to obtain a second membrane-forming solution;
[0006] (2) applying the first film-forming solution prepared in step (1) on a first substrate to obtain a first wet film attached to the first substrate; applying the second film-forming solution prepared in step (1) on a second substrate to obtain a second wet film attached to the second substrate;
[0007] (3) drying the first wet film and peeling it off from the first substrate to obtain a first perfluorosulfonic acid film; drying the second wet film and peeling it off from the second substrate to obtain a second perfluorosulfonic acid film;
[0008] (4) The first perfluorosulfonic acid membrane and the second perfluorosulfonic acid membrane are hot-pressed to obtain a composite perfluorosulfonic acid proton exchange membrane.
[0009] In one or more embodiments, in step (1), the side chain molecular structure of the long-chain branched perfluorosulfonic acid resin is -OCF2CF(CF3)OCF2CF2SO3H. Preferably, the long-chain branched perfluorosulfonic acid resin is Nafion resin and / or DH1120 resin.
[0010] In one or more embodiments, in step (1), the side chain molecular structure of the short-chain branched perfluorosulfonic acid resin is one of -OCF2CF2SO3H, -OCF2CF2CF2SO3H, and -OCF2SO3H.
[0011] In one or more embodiments, the short-chain branched perfluorosulfonic acid resin is IC154 resin and / or Aquivion D79-25BS resin.
[0012] In one or more embodiments, in step (1), the first organic solvent and the second organic solvent are each independently selected from one or more of N,N-dimethylformamide, N-methylpyrrolidone, dimethyl sulfoxide and dimethylacetamide.
[0013] In one or more embodiments, in step (1), the long-chain branched perfluorosulfonic acid resin is dissolved in the organic solvent by heating and stirring, and the heating temperature is 50-80°C.
[0014] In one or more embodiments, in step (1), the short-chain branched perfluorosulfonic acid resin is dissolved in the organic solvent by heating and stirring, and the heating temperature is 50-80°C.
[0015] In one or more embodiments, in step (1), the solid content of the first membrane-forming solution is 5%-30%, preferably 10%-20%.
[0016] In one or more embodiments, in step (1), the solid content of the second membrane-forming solution is 5%-30%, preferably 10%-20%.
[0017] In one or more embodiments, in step (2), the materials of the first substrate and the second substrate are independently selected from one or more of polyimide, polyethylene terephthalate and polyethylene naphthalate.
[0018] In one or more embodiments, in step (2), the first film-forming solution is coated on the first substrate with a coating gap of 200-400 μm.
[0019] In one or more embodiments, in step (2), the coating speed of coating the first film-forming solution on the first substrate is 8-15 mm / s.
[0020] In one or more embodiments, in step (2), the second film-forming solution is coated on the second substrate with a coating gap of 200-400 μm.
[0021] In one or more embodiments, in step (2), the coating speed of coating the second film-forming liquid on the second substrate is 8-15 mm / s.
[0022] In one or more embodiments, in step (3), the drying temperature is 120-160°C.
[0023] In one or more embodiments, in step (3), the thickness of the first perfluorosulfonic acid membrane is 9-27 μm.
[0024] In one or more embodiments, in step (3), the thickness of the second perfluorosulfonic acid membrane is 9-27 μm.
[0025] In one or more embodiments, in step (4), the hot pressing temperature is 180-240°C.
[0026] In one or more embodiments, in step (4), the hot pressing pressure is 0.8-1.2 MPa.
[0027] In one or more embodiments, in step (4), the hot pressing speed is 0.8-1.2 m / min.
[0028] In one or more embodiments, in step (4), the thickness of the composite perfluorosulfonic acid proton exchange membrane is 30-40 μm.
[0029] In one or more embodiments, in step (1), the long-chain branched perfluorosulfonic acid resin is obtained by evaporating a long-chain branched perfluorosulfonic acid resin dispersion.
[0030] In one or more embodiments, in step (1), the short-chain branched perfluorosulfonic acid resin is obtained by evaporating a short-chain branched perfluorosulfonic acid resin dispersion.
[0031] The second aspect of the present invention provides a composite perfluorosulfonic acid proton exchange membrane prepared by the method described in any embodiment of the present invention.
[0032] The third aspect of the present invention provides a liquid flow battery, which comprises the composite perfluorosulfonic acid proton exchange membrane as described in any embodiment of the present invention. Preferably, the liquid flow battery is an all-vanadium redox liquid flow battery. DETAILED DESCRIPTION
[0033] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in this article. Unless otherwise specified, all technical and scientific terms used in this article are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definitions in this article shall prevail.
[0034] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0035] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.
[0036] In this document, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible sub-ranges and individual values within the range (including integers and fractions).
[0037] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.
[0038] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope limited by the claims.
[0039] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0040] In the present invention, long-chain branched perfluorosulfonic acid resin has a good effect of blocking vanadium ions. Short-chain branched perfluorosulfonic acid resin contains more sulfonate groups, so it has stronger proton conductivity, but at the same time its vanadium ion penetration is also increased accordingly, and the coulomb efficiency is low, which limits its use in all-vanadium flow batteries. In order to have high conductivity and block vanadium ion penetration at the same time, the inventors of the present invention consider using short-chain branched perfluorosulfonic acid resin in combination with long-chain branched perfluorosulfonic acid resin with better barrier to prepare proton exchange membrane. However, the inventors found in the study that if the short-chain branched perfluorosulfonic acid resin and the long-chain branched perfluorosulfonic acid resin are directly blended, there will still be more short-chain branched ion channels in the system, which cannot play a good role in blocking vanadium ions. If the direct coating method is adopted in the process, the solvent of the second coating will dissolve or swell the first layer, resulting in the appearance defects and uneven thickness of the obtained membrane. By coating the short-chain perfluorosulfonic acid resin and the long-chain perfluorosulfonic acid resin separately to obtain two single membranes, and then combining them by hot pressing, they can be well fused without producing an interface. The resulting composite perfluorosulfonic acid membrane not only improves the proton conductivity but also blocks the penetration of vanadium ions and greatly improves the energy efficiency.
[0041] The present invention provides a method for preparing a composite perfluorosulfonic acid proton exchange membrane, the method comprising the following steps:
[0042] (1) dissolving a long-chain branched perfluorosulfonic acid resin in a first organic solvent to obtain a first membrane-forming solution; dissolving a short-chain branched perfluorosulfonic acid resin in a second organic solvent to obtain a second membrane-forming solution; wherein the order of preparing the first membrane-forming solution and the second membrane-forming solution is not particular;
[0043] (2) coating a first film-forming liquid on a first substrate to obtain a first wet film attached to the first substrate; coating a second film-forming liquid on a second substrate to obtain a second wet film attached to the second substrate; wherein the order of preparing the first wet film and the second wet film is not particular;
[0044] (3) drying the first wet film and peeling it off from the first substrate to obtain a first perfluorosulfonic acid film; drying the second wet film and peeling it off from the second substrate to obtain a second perfluorosulfonic acid film;
[0045] (4) The first perfluorosulfonic acid membrane and the second perfluorosulfonic acid membrane prepared in step (3) are hot-pressed to obtain a composite perfluorosulfonic acid proton exchange membrane.
[0046] In step (1), the side chain molecular structure of the long-chain branched perfluorosulfonic acid resin is -OCF2CF(CF3)OCF2CF2SO3H. In some embodiments, the long-chain branched perfluorosulfonic acid resin is Nafion resin (e.g., Nafion D520 resin) and / or DH1120 resin. In the present invention, Nafion resin is a perfluorosulfonic acid resin in a Nafion resin dispersion (e.g., Nafion D520 resin dispersion), and DH1120 resin is a perfluorosulfonic acid resin in a DH1120 resin dispersion.
[0047] In step (1), the side chain molecular structure of the short-chain branched perfluorosulfonic acid resin is one of -OCF2CF2SO3H, -OCF2CF2CF2SO3H, and -OCF2SO3H. In some embodiments, the short-chain branched perfluorosulfonic acid resin may be FORBLUE IC154 resin and / or Aquivion D79-25BS resin. In the present invention, FORBLUE IC154 resin is a perfluorosulfonic acid resin in a FORBLUE IC154 resin dispersion, and Aquivion D79-25BS resin is a perfluorosulfonic acid resin in an Aquivion D79-25BS resin dispersion.
[0048] In step (1), the perfluorosulfonic acid resin can be dissolved in the organic solvent by heating and stirring. The heating temperature and time are not particularly limited, and the perfluorosulfonic acid resin can be dissolved. An exemplary heating temperature for dissolving the short-chain perfluorosulfonic acid resin in the first organic solvent can be 50-80°C. The stirring time can be 2-6h. The stirring speed can be 200-400 rpm. An exemplary heating temperature for dissolving the short-chain perfluorosulfonic acid resin in the organic solvent can be 50-80°C. The stirring time can be 2-6h. The stirring speed can be 200-400 rpm.
[0049] In step (1), the solid contents of the first membrane-forming liquid and the second membrane-forming liquid may be 5%-30%, preferably 10%-20%, for example, 8%, 12%, 15%, 18%, 22%, and 26%, respectively.
[0050] In some embodiments, the perfluorosulfonic acid resin is obtained by evaporating a perfluorosulfonic acid resin dispersion. Commercially available perfluorosulfonic acid resin dispersions can be used, such as Nafion D520 dispersion, FORBLUE IC154 dispersion, DH1120 dispersion, Aquivion D79-25BS dispersion. Nafion D520 dispersion and DH1120 dispersion are long-chain branched perfluorosulfonic acid resin dispersions. FORBLUE IC154 dispersion and Aquivion D79-25BS dispersion are short-chain branched perfluorosulfonic acid resin dispersions. The temperature and time of evaporating the perfluorosulfonic acid resin dispersion can be determined according to the properties of the resin dispersion itself, such as the type of solvent, to obtain a perfluorosulfonic acid resin. An exemplary temperature can be 60-120°C, for example 80°C. An exemplary evaporation time can be 8-12h, for example 10h.
[0051] In step (2), the materials of the first substrate and the second substrate can be independently selected from one or more of polyimide, polyethylene terephthalate (PET) and polyethylene naphthalate (PEN). The materials of the first substrate and the second substrate used to prepare the first wet film and the second wet film can be the same or different.
[0052] In step (2), the coating gap between the first film-forming liquid and the second film-forming liquid applied to the first substrate and the second substrate can be 200-400 μm, for example, 250 μm, 300 μm, 350 μm. The coating speed can be 8-15 mm / s, for example, 9 mm / s, 10 mm / s, 12 mm / s, 14 mm / s. The coating setting distance can be 300-500 mm, for example, 350 mm, 400 mm, 450 mm.
[0053] In step (3), the drying temperature for drying the first wet film and the second wet film can be 120-160° C., such as 130° C., 140° C., 150° C. The drying time can be 15-40 min, such as 18 min, 20 min, 25 min, 30 min, 35 min.
[0054] In the present invention, the thickness of the first perfluorosulfonic acid film is preferably controlled to be 9-27 μm, for example, 9 μm, 18 μm, 22 μm, or 27 μm.
[0055] In the present invention, the thickness of the second perfluorosulfonic acid film is preferably controlled to be 9-27 μm, for example, 9 μm, 18 μm, 22 μm, or 27 μm.
[0056] In step (4), the first perfluorosulfonic acid film and the second perfluorosulfonic acid film are bonded together by hot pressing. The hot pressing temperature can be 180-240°C, for example, 190°C, 200°C, 220°C. The hot pressing pressure can be 0.8-1.2 MPa, for example, 0.9 MPa, 1.0 MPa, 1.1 MPa. The hot pressing speed can be 0.8-1.2 m / min, for example, 0.9 m / min, 1.0 m / min, 1.1 m / min.
[0057] In the present invention, the heat pressing does not change the thickness of the first perfluorosulfonic acid film and the second perfluorosulfonic acid film.
[0058] In the present invention, the thickness of the composite perfluorosulfonic acid proton exchange membrane can be 30-40 μm, for example, 28 μm, 30 μm, 32 μm, 36 μm, 38 μm. The thickness ratio of the first perfluorosulfonic acid membrane to the second perfluorosulfonic acid membrane can be (0.2-5):1, for example, 1:3, 1:1, 3:1.
[0059] In some embodiments, the composite perfluorosulfonic acid proton exchange membrane of the present invention is obtained by a method comprising the following steps:
[0060] (1) evaporating a long-chain branched perfluorosulfonic acid resin dispersion to obtain a dry long-chain branched perfluorosulfonic acid resin, dissolving the long-chain branched perfluorosulfonic acid resin in an organic solvent, heating and stirring, and obtaining a first membrane-forming solution;
[0061] Evaporating the short-chain perfluorosulfonic acid resin dispersion to obtain a dry short-chain perfluorosulfonic acid resin, dissolving the short-chain perfluorosulfonic acid resin in an organic solvent, heating and stirring to obtain a second membrane-forming solution;
[0062] (2) applying the first film-forming solution prepared in step (1) on a first substrate to obtain a first wet film attached to the first substrate; applying the second film-forming solution prepared in step (1) on a second substrate to obtain a second wet film attached to the second substrate;
[0063] (3) drying the first wet film and peeling it off from the first substrate to obtain a first perfluorosulfonic acid film; drying the second wet film and peeling it off from the second substrate to obtain a second perfluorosulfonic acid film;
[0064] (4) The first perfluorosulfonic acid membrane and the second perfluorosulfonic acid membrane prepared in step (3) are laminated and hot-pressed to obtain a composite perfluorosulfonic acid proton exchange membrane.
[0065] The invention also provides a composite perfluorosulfonic acid proton exchange membrane prepared by the preparation method of the invention.
[0066] The beneficial effects of the present invention compared with the prior art include:
[0067] The composite perfluorosulfonic acid proton exchange membrane of the present invention adopts a two-layer membrane structure prepared by combining a long-chain branched perfluorosulfonic acid resin and a short-chain branched perfluorosulfonic acid resin, so that the proton exchange membrane has a strong proton conductivity and excellent vanadium ion permeation barrier performance, thereby improving the electrochemical performance, especially the energy efficiency, of the liquid flow battery prepared by the composite perfluorosulfonic acid proton exchange membrane. In addition, by utilizing the winding characteristics and flexibility of the long-chain branched perfluorosulfonic acid resin, the proton exchange membrane of the present invention can maintain the membrane morphology well.
[0068] The present invention will be described below in the form of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The methods, reagents and materials used in the examples are, unless otherwise stated, conventional methods, reagents and materials in the art. The raw material compounds in the examples can all be purchased through commercial routes.
[0069] The Nafion D520 resin dispersion in the examples and comparative examples was purchased from Thermo Fisher Scientific. The DH1120 resin dispersion was purchased from Shandong Dongyue Future Hydrogen Energy Materials Co., Ltd. The Aquivion D79-25BS resin dispersion was purchased from Solvay Group. The FORBLUE IC154 resin dispersion was purchased from Aijiexu Chemical Technology Co., Ltd.
[0070] Example 1
[0071] Step (1): First, pour the purchased Nafion D520 dispersion into an evaporating dish, adjust the oven to 80°C, and place the evaporating dish in the oven for 10 hours to obtain a dry Nafion resin. Add 20g of the obtained Nafion resin and 80g of DMF solvent into a reactor, stir at 80°C for 4 hours, and set the stirring speed to 300 rpm. Stop stirring after observing that the Nafion resin is completely dissolved, and obtain a first membrane-forming solution with a mass fraction (i.e., solid content) of 20wt%.
[0072] The purchased FORBLUE IC154 dispersion was first evaporated at 80°C for 10 h to obtain dry FORBLUE IC154 resin. 20 g of the obtained FORBLUE IC154 resin and 80 g of DMF solvent were added to the reactor and stirred at 80°C for 4 h. The stirring speed was set to 300 rpm. Stirring was stopped after the IC154 resin was observed to be completely dissolved, and a second film-making solution with a mass fraction of 20 wt% (i.e., solid content) was obtained.
[0073] Step (2): coating the first film-forming liquid on the polyimide substrate, setting the gap of the casting coater to 300 μm, the running speed to 10 mm / s, and the setting distance to 400 mm, to obtain a first wet film attached to the substrate.
[0074] The second film-forming liquid was coated on the polyimide substrate, and the gap of the casting coater was set to 300 μm, the running speed was set to 10 mm / s, and the setting distance was 400 mm to obtain a second wet film attached to the substrate.
[0075] Step (3): Place the first wet film attached to the substrate and the second wet film attached to the substrate obtained in the previous step in a 140° C. oven for 20 minutes to remove the solvent, and then peel them off from the substrate to obtain a first perfluorosulfonic acid film and a second perfluorosulfonic acid film both with a thickness of 18 μm.
[0076] Step (4): The first perfluorosulfonic acid membrane and the second perfluorosulfonic acid membrane are bonded together by a hot pressing device, the hot pressing temperature is 200°C, the hot pressing speed is 1m / min, and the hot pressing pressure is 1MPa. The total thickness of the prepared composite perfluorosulfonic acid proton exchange membrane is 36μm, and the thickness ratio of the first perfluorosulfonic acid membrane and the second perfluorosulfonic acid is 1:1.
[0077] Example 2
[0078] The difference between Example 2 and Example 1 is that in step (3), the thickness of the first perfluorosulfonic acid membrane obtained is 9 μm, the thickness of the second perfluorosulfonic acid membrane obtained is 27 μm, and finally a composite perfluorosulfonic acid proton exchange membrane with a total thickness of 36 μm is obtained, wherein the thickness ratio of the first perfluorosulfonic acid membrane to the second perfluorosulfonic acid is 1:3. The other operating conditions are the same as those of Example 1.
[0079] Example 3
[0080] The difference between Example 3 and Example 1 is that in step (3), the thickness of the first perfluorosulfonic acid membrane obtained is 27 μm, the thickness of the second perfluorosulfonic acid membrane obtained is 9 μm, and finally a composite perfluorosulfonic acid proton exchange membrane with a total thickness of 36 μm is obtained, wherein the thickness ratio of the first perfluorosulfonic acid membrane to the second perfluorosulfonic acid is 3:1. The other operating conditions are the same as those of Example 1.
[0081] Example 4
[0082] The difference between Example 4 and Example 1 is that the solvent DMF used in step (1) is replaced with DMSO of equal mass. Other operating conditions and steps are the same as those in Example 1.
[0083] Example 5
[0084] The difference between Example 5 and Example 1 is that the DH1120 resin dispersion is dried to obtain dried DH1120 resin, and the Nafion resin is replaced with an equal mass of DH1120 resin. Other operating conditions and steps are the same as those in Example 1.
[0085] Example 6
[0086] The difference between Example 6 and Example 1 is that the Aquivion D79-25BS resin dispersion is dried to obtain dried Aquivion D79-25BS resin, and the FORBLUE IC154 resin is replaced with an equal mass of Aquivion D79-25BS resin. Other operating conditions and steps are the same as those in Example 1.
[0087] Comparative Example 1
[0088] Step (1): First, pour the purchased Nafion D520 dispersion into an evaporating dish, adjust the oven to 80°C, and place the evaporating dish in the oven for 10 hours to obtain a dry Nafion resin. Add 20g of the obtained Nafion resin and 80g of DMF solvent into a reactor, stir at 80°C for 4 hours, and set the stirring speed to 300 rpm. Stop stirring after observing that the Nafion resin is completely dissolved, and obtain a first membrane-forming solution with a mass fraction (i.e., solid content) of 20wt%.
[0089] The purchased FORBLUE IC154 dispersion was first evaporated at 80°C for 10 h to obtain a dry IC154 resin. 20 g of the obtained IC154 resin and 80 g of DMF solvent were added to a reactor and stirred at 80°C for 4 h. The stirring speed was set to 300 rpm. Stirring was stopped after the IC154 resin was observed to be completely dissolved, and a second film-making solution with a mass fraction of 20 wt% (i.e., solid content) was obtained.
[0090] Step (2): coating the first film-forming liquid on the polyimide substrate, setting the gap of the casting coater to 300 μm, the running speed to 10 mm / s, and the setting distance to 400 mm, to obtain a first wet film attached to the substrate. The first wet film attached to the substrate is placed in a 140° C. oven for 10 minutes to dry and remove the solvent, thereby obtaining a substrate having a first perfluorosulfonic acid film on the surface.
[0091] Step (3): Coat the second film-forming liquid on the surface of the first perfluorosulfonic acid film on the substrate, and set the gap of the casting coater to 300 μm, the running speed to 10 mm / s, and the setting distance to 400 mm. At this time, the coated film has a large number of defects. The surface of the film coated with the second film-forming liquid has circular and hexagonal shrinkage holes, and the first perfluorosulfonic acid film is swollen by the second film-forming liquid, resulting in uneven thickness.
[0092] Comparative Example 2
[0093] Step (1): First, pour the purchased Nafion D520 dispersion into an evaporating dish, adjust the oven to 80°C, and place the evaporating dish in the oven for 10 hours to obtain a dry Nafion resin. Add 20g of the obtained Nafion resin and 80g of DMF solvent into a reactor, stir at 80°C for 4 hours, and set the stirring speed to 300 rpm. Stop stirring after observing that the Nafion resin is completely dissolved, and obtain a first membrane-forming solution with a mass fraction (i.e., solid content) of 20wt%.
[0094] The purchased FORBLUE IC154 dispersion was first evaporated at 80°C for 10 h to obtain a dry IC154 resin. 20 g of the obtained IC154 resin and 80 g of DMF solvent were added to a reactor and stirred at 80°C for 4 h. The stirring speed was set to 300 rpm. Stirring was stopped after the IC154 resin was observed to be completely dissolved, and a second film-making solution with a mass fraction of 20 wt% (i.e., solid content) was obtained.
[0095] Step (2): The first film-forming liquid and the second film-forming liquid are mixed together at a solid mass content ratio of 1:1 to form a composite film-forming liquid.
[0096] Step (3): The composite film-forming liquid obtained in step 2 is coated on a polyimide substrate, and a wet film attached to the substrate is obtained by setting the gap of the casting coater to 600 μm, the running speed to 10 mm / s, and the setting distance to 400 mm.
[0097] Step (4): The wet film attached to the substrate obtained in step (3) was placed in an oven at 140° C. for 20 minutes to remove the solvent, and then peeled off from the substrate to obtain a perfluorosulfonic acid membrane proton exchange membrane with a thickness of 36 μm.
[0098] Comparative Example 3
[0099] Step (1): Pour the purchased Nafion D520 dispersion into an evaporating dish, adjust the oven to 80°C, and place the evaporating dish in the oven for 10 hours to obtain a dry Nafion resin. Add 20 g of the obtained Nafion resin and 80 g of DMF solvent into a reactor, stir at 80°C for 4 hours, and set the stirring speed to 300 rpm. Stop stirring after observing that the Nafion resin is completely dissolved, and obtain a membrane-making solution with a mass fraction (i.e., solid content) of 20 wt%.
[0100] Step (2): coating the film-forming liquid on the polyimide substrate, setting the gap of the casting coater to 600 μm, the running speed to 10 mm / s, and the setting distance to 400 mm, to obtain a wet film attached to the substrate.
[0101] Step (3): The wet film attached to the substrate obtained in the previous step was placed in a 140° C. oven for 20 minutes to remove the solvent, and then peeled off from the substrate to obtain a perfluorosulfonic acid film with a thickness of 36 μm.
[0102] Comparative Example 4
[0103] Step (1): The purchased FORBLUE IC154 dispersion was first evaporated at 80°C for 10 h to obtain a dry IC154 resin. 20 g of the obtained IC154 resin and 80 g of DMF solvent were added to a reactor and stirred at 80°C for 4 h. The stirring speed was set to 300 rpm. Stirring was stopped after the IC154 resin was observed to be completely dissolved, and a film-making solution with a mass fraction of 20 wt% (i.e., solid content) was obtained.
[0104] Step (2): coating the film-forming liquid on the polyimide substrate, setting the gap of the casting coater to 600 μm, the running speed to 10 mm / s, and the setting distance to 400 mm, to obtain a wet film attached to the substrate.
[0105] Step (3): The wet film attached to the substrate obtained in the previous step was placed in a 140° C. oven for 20 minutes to remove the solvent, and then peeled off from the substrate to obtain a perfluorosulfonic acid film with a thickness of 36 μm.
[0106] Comparative Example 5
[0107] Step (1): First, pour the purchased Solvay Aquivion D79-25BS dispersion into an evaporating dish, adjust the oven to 80°C, and place the evaporating dish in the oven for 10 hours to obtain dry Aquivion resin (short-chain branched perfluorosulfonic acid resin). Add 20g of the obtained Aquivion resin and 80g of DMF solvent into a reactor, stir at 80°C for 4 hours, and set the stirring speed to 300 rpm. Stop stirring after observing that the resin is completely dissolved, and obtain a membrane-forming solution with a mass fraction of 20wt%.
[0108] Step (2): The film-forming solution obtained in step (1) is coated on a polyimide substrate, and a wet film attached to the substrate is obtained by setting the gap of the casting coater to 600 μm, the running speed to 10 mm / s, and the setting distance to 400 mm.
[0109] Step (3): The wet film attached to the substrate obtained in the previous step was placed in an oven at 140° C. for 20 min to dry and remove the solvent, then removed from the substrate and annealed at 200° C. to obtain a perfluorosulfonic acid proton exchange membrane with a thickness of 36 μm.
[0110] Test Example 1
[0111] The performance of the all-vanadium redox flow battery prepared using the perfluorosulfonic acid proton exchange membrane of Examples 1-6 and Comparative Examples 2-5 was tested. The test conditions were as follows: at a current density of 80 mA / cm 2 -200mA / cm 2 The charge and discharge experiments were carried out under the following conditions: charging to 1.55V and discharging to 1.00V, and the effective working area of the electrode was 48cm 2 The positive and negative electrolytes are VO 2+ / VO2 + and V 2+ / V 3+ of sulfuric acid solution, the battery operating temperature is 30°C.
[0112] The energy efficiency results of the all-vanadium redox flow batteries prepared using the perfluorosulfonic acid proton exchange membranes of Examples 1-6 and Comparative Examples 2-5 are shown in Table 1.
[0113] Table 1: Performance test of proton membrane vanadium redox flow battery at different current densities
[0114] Current density <![CDATA[80mA / cm 2 ]]> <![CDATA[120mA / cm 2 ]]> <![CDATA[160mA / cm 2 ]]> <![CDATA[200mA / cm 2 ]]> efficiency Energy efficiency Energy efficiency Energy efficiency Energy efficiency Example 1 90.89 88.34 85.57 82.71 Example 2 90.64 88.21 85.56 82.67 Example 3 90.6 87.67 84.67 81.43 Example 4 90.61 88.22 85.56 82.62 Example 5 90.65 88.18 85.52 82.66 Example 6 90.64 88.31 85.53 82.67 Comparative Example 2 88.82 85.85 82.99 80.13 Comparative Example 3 89.48 86.54 83.29 80.04 Comparative Example 4 89.13 87.13 84.55 81.27 Comparative Example 5 88.73 86.44 84.26 81.08
[0115] It can be seen from Table 1 that when long- and short-chain branched resins are used together through the hot pressing process, the energy efficiency of the battery can be improved, especially when the ratio is 1:1, the effect is most obvious. When the hot pressing process is used to prepare a double-layer membrane, the long-chain branched resin has good vanadium resistance and the short-chain branch has low resistance.
[0116] Test Example 2
[0117] The conductivity of the perfluorosulfonic acid proton exchange membranes of Examples 1-6 and Comparative Examples 2-3 was tested. The prepared perfluorosulfonic acid proton exchange membrane was clamped by a test module, and then laid flat and overlapped between two parallel electrodes. The test piece was immersed in ultrapure water, and the conductivity of the proton exchange membrane was tested using a CHI760 electrochemical workstation. The conductivity results are shown in Table 2.
[0118] Table 2: Conductivity test results
[0119] name Conductivity (ms / cm) Example 1 33.8 Example 2 42.4 Example 3 31.6 Example 4 32.9 Example 5 33.2 Example 6 33.5 Comparative Example 2 28.8 Comparative Example 3 27.9
[0120] It can be found from Table 2 that the conductivity of the proton exchange membrane prepared by hot pressing is significantly higher than that of the membrane prepared by direct blending, and as the proportion of short-chain branched resin increases, the conductivity will increase accordingly. High membrane conductivity means that the internal resistance of the membrane itself is low, thereby improving the energy efficiency of the flow battery.
Claims
1. A method for preparing a composite perfluorosulfonic acid proton exchange membrane, characterized in that: The method comprises the following steps: (1) dissolving a long-chain branched perfluorosulfonic acid resin in a first organic solvent to obtain a first membrane-forming solution; dissolving a short-chain branched perfluorosulfonic acid resin in a second organic solvent to obtain a second membrane-forming solution; wherein the long-chain branched perfluorosulfonic acid resin is Nafion resin and / or DH1120 resin, and the short-chain branched perfluorosulfonic acid resin is FORBLUE IC154 resin and / or Aquivion D79-25BS resin; (2) applying the first film-forming solution prepared in step (1) on a first substrate to obtain a first wet film attached to the first substrate; applying the second film-forming solution prepared in step (1) on a second substrate to obtain a second wet film attached to the second substrate; (3) drying the first wet film and peeling it off from the first substrate to obtain a first perfluorosulfonic acid film; drying the second wet film and peeling it off from the second substrate to obtain a second perfluorosulfonic acid film; the thickness of the first perfluorosulfonic acid film is 9-27 μm; the thickness of the second perfluorosulfonic acid film is 9-27 μm; (4) Hot pressing the first perfluorosulfonic acid membrane and the second perfluorosulfonic acid membrane to obtain a composite perfluorosulfonic acid proton exchange membrane; the hot pressing temperature is 180-240°C.
2. The method according to claim 1, characterized in that The method has one or more of the following features: In step (1), the first organic solvent and the second organic solvent are each independently selected from one or more of N,N-dimethylformamide, N-methylpyrrolidone, dimethyl sulfoxide and dimethylacetamide; In step (1), the long-chain branched perfluorosulfonic acid resin is dissolved in the first organic solvent by heating and stirring, and the heating temperature is 50-80° C.; In step (1), the short-chain branched perfluorosulfonic acid resin is dissolved in the second organic solvent by heating and stirring, and the heating temperature is 50-80°C.
3. The method according to claim 1, characterized in that In step (1), the solid content of the first membrane-forming solution is 5wt%-30wt%; and / or In step (1), the solid content of the second membrane-forming solution is 5wt%-30wt%.
4. The method according to claim 1, wherein: In step (1), the solid content of the first membrane-forming solution is 10wt%-20wt%; and / or In step (1), the solid content of the second membrane-forming solution is 10wt%-20wt%.
5. The method according to claim 1, characterized in that The method has one or more of the following features: In step (2), the materials of the first substrate and the second substrate are independently selected from one or more of polyimide, polyethylene terephthalate and polyethylene naphthalate; In step (2), the first film-forming solution is coated on the first substrate with a coating gap of 200-400 μm; In step (2), the first film-forming liquid is coated on the first substrate at a coating speed of 8-15 mm / s; In step (2), the second film-forming liquid is coated on the second substrate with a coating gap of 200-400 μm; In step (2), the coating speed of coating the second film-forming liquid on the second substrate is 8-15 mm / s.
6. The method according to claim 1, characterized in that In step (3), the drying temperature is 120-160°C.
7. The method according to claim 1, characterized in that In step (4), the hot pressing pressure is 0.8-1.2 MPa; and / or In step (4), the hot pressing speed is 0.8-1.2 m / min.
8. The method according to claim 1, wherein In step (4), the thickness of the composite perfluorosulfonic acid proton exchange membrane is 30-40 μm.
9. The method according to claim 1, characterized in that In step (1), the long-chain branched perfluorosulfonic acid resin is obtained by evaporating a long-chain branched perfluorosulfonic acid resin dispersion; and / or The short-chain branched perfluorosulfonic acid resin is obtained by evaporating a short-chain branched perfluorosulfonic acid resin dispersion.
10. A composite perfluorosulfonic acid proton exchange membrane prepared by the method according to any one of claims 1 to 9.
11. A liquid flow battery, characterized in that: It comprises the composite perfluorosulfonic acid proton exchange membrane as claimed in claim 10.
12. The flow battery according to claim 11, wherein: The liquid flow battery is an all-vanadium redox liquid flow battery.