A composite graphite sealing material and its preparation method and application

By alkali activation and hydrothermal reaction of expandable graphite to generate graphite-hydrotalcite-titanium dioxide composite material, combined with modified carbon fiber, the problem of insufficient environmental stress cracking and flame retardant performance of epoxy resin sealing materials is solved, and the composite is improved Flame retardant and mechanical properties of graphite sealing materials.

CN118599267BActive Publication Date: 2024-12-06YANCHENG CHAOGE SEALING MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410836682.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-12-06
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

Traditional epoxy resin sealing materials may experience environmental stress cracking in certain environments and do not have sufficient flame retardant properties, which limits their application.

Method used

The composite graphite material is used to generate graphite-hydrotalcite-titanium dioxide composite material by alkali activation and hydrothermal reaction of expandable graphite, and modified with silane coupling agent, combined with modified carbon fibers, to improve the flame retardant and mechanical properties of the material. .

Benefits of technology

Improves the flame retardant and wear resistance of sealing materials, and enhances their fire safety and mechanical properties in specific applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004913368180000121
    Figure BDA0004913368180000121
Patent Text Reader

Abstract

The invention discloses a composite graphite sealing material and a preparation method and application thereof. The invention promotes carbonization and forms a dense carbonaceous layer through the joint action of nano titanium dioxide, hydrotalcite and graphite, improves the strength and stability of the carbon layer, improves the flame retardant performance of the sealing material, and improves the problem of poor wear resistance of graphite by loading nano titanium dioxide, thereby improving the wear resistance of the sealing material; subsequently, a silane coupling agent KH560 is used to treat the surface of the composite graphite material, and epoxy groups are introduced to increase the compatibility between the composite graphite material and other raw materials, thereby improving the mechanical properties of the sealing material; and simultaneously, carbon fibers are modified, and amino groups in the modified carbon fibers undergo cross-linking reaction with epoxy groups, thereby enhancing the bonding strength between the carbon fibers and a base material, thereby further improving the mechanical properties of the sealing material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sealing material preparation, and in particular to a composite graphite sealing material and a preparation method and application thereof. Background Art

[0002] Epoxy resin, as a high-performance thermosetting plastic, has been widely used in the field of sealing materials due to its excellent bonding properties, mechanical properties and chemical corrosion resistance. With the development of science and technology and the increase in industrial demand, the application of epoxy resin sealing materials in the fields of electronics, automobiles, aerospace, construction, etc. has been continuously expanded, and the requirements for the performance of epoxy resin sealing materials have been further improved. Traditional epoxy resin sealing materials may suffer from environmental stress cracking in certain environments, especially in the presence of chemical media, which will reduce its performance as a sealing material; at the same time, epoxy resin sealing materials do not have sufficient flame retardant properties and do not meet the fire safety requirements of specific application fields. These defects limit the application occasions of epoxy resin sealing materials.

[0003] Expanded graphite is an excellent new sealing material due to its special loose and porous structure and good compression performance. When expanded graphite is used to fill epoxy resin, the dispersion performance of expanded graphite in the epoxy resin system is poor and the overall improvement of the comprehensive performance of epoxy resin cannot be achieved. Therefore, it is necessary to modify the expanded graphite to achieve an overall improvement in the comprehensive performance of the composite sealing material. Summary of the invention

[0004] In view of the deficiencies of the prior art, the object of the present invention is to provide a composite graphite sealing material and a preparation method and application thereof.

[0005] In order to achieve the above object, the present invention adopts the following technical scheme:

[0006] In a first aspect, the present invention provides a composite graphite sealing material, which comprises the following raw materials, measured in parts by weight: 60-80 parts of epoxy resin, 8-12 parts of maleic anhydride grafted POE, 10-15 parts of composite graphite material, 4-8 parts of modified carbon fiber, 1-3 parts of zinc stearate, and 5-10 parts of curing agent.

[0007] Specifically, in some embodiments of the present invention, the epoxy resin can be selected to be 60 parts, 62 parts, 65 parts, 68 parts, 70 parts, 72 parts, 74 parts, 75 parts, 76 parts, 78 parts, and 80 parts, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0008] Specifically, in some embodiments of the present invention, the maleic anhydride grafted POE can be selected to be 8 parts, 9 parts, 10 parts, 11 parts, or 12 parts, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0009] Specifically, in some embodiments of the present invention, the composite graphite material can be selected to be 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, or 15 parts, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0010] More specifically, the preparation method of the composite graphite material is as follows:

[0011] S1, ultrasonically dispersing expandable graphite powder in an alkaline solution, drying, and then calcining in an ammonia atmosphere to obtain pretreated graphite;

[0012] S2, dissolving zinc nitrate, aluminum nitrate and urea in water to prepare a mixed salt solution, then adding pretreated graphite, tetrabutyl titanate and sodium dodecylbenzene sulfonate thereto, stirring and dispersing them evenly, then transferring them into a reactor for hydrothermal reaction, and after the reaction is completed, centrifuging, washing and drying to obtain a graphite-hydrotalcite-titanium dioxide composite material;

[0013] S3, dispersing the graphite-hydrotalcite-titanium dioxide composite material in an ethanol aqueous solution, then adding a silane coupling agent KH560 thereto, stirring for reaction, and after the reaction is completed, centrifuging, washing, and drying to obtain a composite graphite material.

[0014] In step S1, the alkaline solution can be selected as sodium hydroxide solution or potassium hydroxide solution, and the mass fraction of the alkaline solution is 25-40%, for example, 25%, 30%, 35%, 40% can be selected, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0015] In step S1, the calcination temperature is 350-450°C. In some embodiments of the present invention, for example, 350°C, 360°C, 380°C, 400°C, 410°C, 420°C, 440°C, and 450°C can be selected; the calcination time is 30-60s, for example, 30s, 35s, 40s, 45s, 50s, 55s, and 60s can be selected, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0016] In step S2, the mass ratio of zinc nitrate, aluminum nitrate, urea, pretreated graphite, tetrabutyl titanate and sodium dodecylbenzene sulfonate is 4-8:3-5:4-6:5-10:3-5:0.4-0.8, and more preferably 5-6:3-4:4-5:6-8:3-4:0.5-0.6.

[0017] In step S2, the temperature of the hydrothermal reaction is 150-180°C. In some embodiments of the present invention, for example, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, and 180°C can be selected; the time of the hydrothermal reaction is 12-18h. For example, 12h, 13h, 14h, 15h, 16h, 17h, and 18h ​​can be selected, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0018] In step S3, the mass ratio of the graphite-hydrotalcite-titanium dioxide composite material and the silane coupling agent KH560 is 5-10:1-2. In some embodiments of the present invention, for example, 5:1, 5:2, 8:1, 8:2, 10:1, 10:2 can be selected, but it is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable.

[0019] Specifically, in some embodiments of the present invention, the modified carbon fiber can be selected to be 4 parts, 5 parts, 6 parts, 7 parts, or 8 parts, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0020] More specifically, the preparation method of the modified carbon fiber is as follows: dopamine hydrochloride is added to Tris-HCl buffer, the pH is adjusted to 8-10, and then carbon fiber is added and soaked for 18-24 hours. After soaking, the carbon fiber is taken out and washed with water and vacuum dried to obtain the modified carbon fiber.

[0021] Among them, the dosage ratio of dopamine hydrochloride, Tris-HCl buffer and carbon fiber is 1-3g:50mL:1-3g, for example, 1g:50mL:1g, 1g:50mL:2g, 1g:50mL:3g, 2g:50mL:1g, 2g:50mL:2g, 2g:50mL:3g, 3g:50mL:1g, 3g:50mL:2g, 3g:50mL:3g can be selected, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0022] Specifically, in some embodiments of the present invention, the zinc stearate can be selected to be 1 part, 1.5 parts, 2 parts, 2.5 parts, or 3 parts, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0023] Specifically, in some embodiments of the present invention, the curing agent can be selected to be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, or 10 parts, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] More specifically, the curing agent may be an amine curing agent or an acid anhydride curing agent, for example, ethylenediamine, hexamethylenediamine, maleic anhydride or phthalic anhydride.

[0025] In a second aspect, the present invention provides a method for preparing the above-mentioned composite graphite sealing material, comprising the following steps: according to the formula amount, epoxy resin, maleic anhydride grafted POE, composite graphite material, modified carbon fiber, zinc stearate and curing agent are stirred and mixed evenly, and cured to obtain the composite graphite sealing material.

[0026] In a third aspect, the present invention also provides application of the composite graphite sealing material in a sealing gasket.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The present invention first performs an alkali activation treatment on expandable graphite, and then roasts it in an ammonia atmosphere to obtain pretreated graphite, thereby increasing the number of active groups on the graphite surface, and also increasing the porosity and specific surface area of ​​the graphite, which is beneficial to the subsequent loading of hydrotalcite and nano-titanium dioxide; then the pretreated graphite, tetrabutyl titanate and a mixed salt solution are blended and subjected to a hydrothermal reaction, and the generated hydrotalcite is attached to the surface and pore structure of the graphite, and at the same time, the nano-titanium dioxide is attached to the interlayer of the hydrotalcite and the surface and pore structure of the graphite. The nano-titanium dioxide, hydrotalcite and graphite work together to promote carbonization and form a dense carbonaceous layer, thereby improving the strength and stability of the carbon layer, and improving the flame retardant performance of the sealing material. At the same time, by loading the nano-titanium dioxide, the problem of poor wear resistance of the graphite is improved, thereby improving the wear resistance of the sealing material; then the surface is treated with a silane coupling agent KH560, and by introducing epoxy groups, the compatibility between the composite graphite material and other raw materials is increased, thereby improving the mechanical properties of the sealing material.

[0029] (2) The present invention utilizes dopamine to modify carbon fiber and deposits a layer of polydopamine on the surface of the carbon fiber. After the carbon fiber is modified with polydopamine, amino active functional groups are introduced, thereby improving the dispersion performance of the carbon fiber in the epoxy resin. At the same time, the amino groups in the modified carbon fiber undergo a cross-linking reaction with the epoxy groups, thereby enhancing the bonding strength between the carbon fiber and the base material, and further improving the mechanical properties of the sealing material. In addition, polydopamine has excellent flame retardant properties. When it is introduced into the sealing material and works together with the composite graphite material, the flame retardant properties of the sealing material are further improved. DETAILED DESCRIPTION

[0030] The present invention is further described in detail below through specific preferred embodiments, but the present invention is not limited to the following embodiments.

[0031] It should be noted that, unless otherwise specified, the chemical reagents involved in the present invention were purchased through commercial channels.

[0032] The model of the epoxy resin used in the embodiment of the present invention is E44, purchased from Wanqing Chemical Technology Co., Ltd.; the brand of maleic anhydride grafted POE is MA8510; the mesh number of the expandable graphite powder is 100 mesh, purchased from Qingdao Yuchen Graphite Co., Ltd.; the carbon fiber is chopped carbon fiber with a length of 1-3 mm, purchased from Toray New Materials (Guangdong) Co., Ltd.

[0033] Example 1

[0034] A method for preparing a composite graphite sealing material comprises the following steps:

[0035] 60 parts of epoxy resin, 10 parts of maleic anhydride grafted POE, 10 parts of composite graphite material, 5 parts of modified carbon fiber, 2 parts of zinc stearate and 8 parts of curing agent ethylenediamine were stirred and mixed evenly, and cured at 80° C. to obtain a composite graphite sealing material;

[0036] Wherein, the preparation method of the composite graphite material is as follows:

[0037] S1. Ultrasonic dispersion of 10 g expandable graphite powder in 100 mL of 30 wt % sodium hydroxide solution, drying, and then calcining in an ammonia atmosphere at a calcination temperature of 400° C. for 45 s to obtain pretreated graphite;

[0038] S2, 4g zinc nitrate, 4g aluminum nitrate and 5g urea were dissolved in 100mL water to prepare a mixed salt solution, and then 8g pretreated graphite, 4g tetrabutyl titanate and 0.5g sodium dodecylbenzene sulfonate were added thereto, stirred and dispersed evenly, and then transferred to a reactor for hydrothermal reaction, the temperature of the hydrothermal reaction was 150°C, and the time of the hydrothermal reaction was 18h. After the reaction was completed, the graphite-hydrotalcite-titanium dioxide composite material was obtained by centrifugation, washing and drying;

[0039] S3. Disperse 5 g of graphite-hydrotalcite-titanium dioxide composite material in 100 mL of 80 wt% ethanol aqueous solution, then add 1 g of silane coupling agent KH560, stir and react for 3 h, and after the reaction is completed, centrifuge, wash and dry to obtain a composite graphite material.

[0040] The preparation method of the modified carbon fiber is as follows: 2 g of dopamine hydrochloride is added to 50 mL of Tris-HCl buffer, the pH is adjusted to 10, and then 2 g of carbon fiber is added and soaked for 24 hours. After soaking, the carbon fiber is taken out and washed with water and vacuum dried to obtain the modified carbon fiber.

[0041] Example 2

[0042] A method for preparing a composite graphite sealing material comprises the following steps:

[0043] 80 parts of epoxy resin, 12 parts of maleic anhydride grafted POE, 15 parts of composite graphite material, 4 parts of modified carbon fiber, 1 part of zinc stearate and 5 parts of curing agent phthalic anhydride were stirred and mixed evenly, and cured at 80° C. to obtain a composite graphite sealing material;

[0044] Wherein, the preparation method of the composite graphite material is as follows:

[0045] S1, ultrasonically dispersing 10 g of expandable graphite powder in 100 mL of 30 wt% sodium hydroxide solution, drying, and then calcining in an ammonia atmosphere at a calcination temperature of 450° C. for 30 s to obtain pretreated graphite;

[0046] S2, 8g zinc nitrate, 5g aluminum nitrate and 6g urea were dissolved in 100mL water to prepare a mixed salt solution, and then 10g pretreated graphite, 5g tetrabutyl titanate and 0.8g sodium dodecylbenzene sulfonate were added thereto, stirred and dispersed evenly, and then transferred to a reactor for hydrothermal reaction at a temperature of 180°C for 12h. After the reaction was completed, the graphite-hydrotalcite-titanium dioxide composite material was obtained by centrifugation, washing and drying;

[0047] S3. Disperse 10 g of graphite-hydrotalcite-titanium dioxide composite material in 100 mL of 80 wt% ethanol aqueous solution, then add 2 g of silane coupling agent KH560, stir and react for 3 h, and after the reaction is completed, centrifuge, wash and dry to obtain a composite graphite material.

[0048] The preparation method of the modified carbon fiber is as follows: 1 g of dopamine hydrochloride is added to 50 mL of Tris-HCl buffer, the pH is adjusted to 10, and then 1 g of carbon fiber is added and soaked for 18 hours. After soaking, the carbon fiber is taken out, washed with water, and vacuum dried to obtain the modified carbon fiber.

[0049] Example 3

[0050] A method for preparing a composite graphite sealing material comprises the following steps:

[0051] 65 parts of epoxy resin, 8 parts of maleic anhydride grafted POE, 12 parts of composite graphite material, 8 parts of modified carbon fiber, 3 parts of zinc stearate and 10 parts of curing agent ethylenediamine were stirred and mixed uniformly, and cured at 80° C. to obtain a composite graphite sealing material;

[0052] Wherein, the preparation method of the composite graphite material is as follows:

[0053] S1, ultrasonically dispersing 10 g of expandable graphite powder in 100 mL of 30 wt% sodium hydroxide solution, drying, and then calcining in an ammonia atmosphere at a calcination temperature of 450° C. for 30 s to obtain pretreated graphite;

[0054] S2, 5g zinc nitrate, 5g aluminum nitrate and 6g urea were dissolved in 100mL water to prepare a mixed salt solution, and then 5g pretreated graphite, 3g tetrabutyl titanate and 0.4g sodium dodecylbenzene sulfonate were added thereto, stirred and dispersed evenly, and then transferred to a reactor for hydrothermal reaction, the temperature of the hydrothermal reaction was 160°C, and the time of the hydrothermal reaction was 12h. After the reaction was completed, the graphite-hydrotalcite-titanium dioxide composite material was obtained by centrifugation, washing and drying;

[0055] S3. Disperse 8 g of graphite-hydrotalcite-titanium dioxide composite material in 100 mL of 80 wt% ethanol aqueous solution, then add 2 g of silane coupling agent KH560, stir and react for 3 h, and after the reaction is completed, centrifuge, wash and dry to obtain a composite graphite material.

[0056] The preparation method of the modified carbon fiber is as follows: 2 g of dopamine hydrochloride is added to 50 mL of Tris-HCl buffer, the pH is adjusted to 10, and then 3 g of carbon fiber is added and soaked for 24 hours. After soaking, the carbon fiber is taken out, washed with water, and vacuum dried to obtain the modified carbon fiber.

[0057] Example 4

[0058] A method for preparing a composite graphite sealing material comprises the following steps:

[0059] 75 parts of epoxy resin, 10 parts of maleic anhydride grafted POE, 12 parts of composite graphite material, 5 parts of modified carbon fiber, 2 parts of zinc stearate and 8 parts of curing agent phthalic anhydride were stirred and mixed uniformly, and cured at 80° C. to obtain a composite graphite sealing material;

[0060] Wherein, the preparation method of the composite graphite material is as follows:

[0061] S1, ultrasonically dispersing 10 g of expandable graphite powder in 100 mL of 30 wt% sodium hydroxide solution, drying, and then calcining in an ammonia atmosphere at a calcination temperature of 450° C. for 30 s to obtain pretreated graphite;

[0062] S2, 4g zinc nitrate, 5g aluminum nitrate and 5g urea were dissolved in 100mL water to prepare a mixed salt solution, and then 6g pretreated graphite, 4g tetrabutyl titanate and 0.6g sodium dodecylbenzene sulfonate were added thereto, stirred and dispersed evenly, and then transferred to a reactor for hydrothermal reaction, the temperature of the hydrothermal reaction was 160°C, and the time of the hydrothermal reaction was 15h. After the reaction was completed, the graphite-hydrotalcite-titanium dioxide composite material was obtained by centrifugation, washing and drying;

[0063] S3. Disperse 6 g of graphite-hydrotalcite-titanium dioxide composite material in 100 mL of 80 wt% ethanol aqueous solution, then add 2 g of silane coupling agent KH560, stir and react for 3 h, and after the reaction is completed, centrifuge, wash and dry to obtain a composite graphite material.

[0064] The preparation method of the modified carbon fiber is as follows: 3 g of dopamine hydrochloride is added to 50 mL of Tris-HCl buffer, the pH is adjusted to 10, and then 3 g of carbon fiber is added and soaked for 24 hours. After soaking, the carbon fiber is taken out and washed with water and vacuum dried to obtain the modified carbon fiber.

[0065] Comparative Example 1

[0066] A method for preparing a composite graphite sealing material comprises the following steps:

[0067] 60 parts of epoxy resin, 10 parts of maleic anhydride grafted POE, 10 parts of composite graphite material, 5 parts of modified carbon fiber, 2 parts of zinc stearate and 8 parts of curing agent ethylenediamine were stirred and mixed evenly, and cured at 80° C. to obtain a composite graphite sealing material;

[0068] Wherein, the preparation method of the composite graphite material is as follows:

[0069] S1. Ultrasonic dispersion of 10 g expandable graphite powder in 100 mL of 30 wt % sodium hydroxide solution, drying, and then calcining in an ammonia atmosphere at a calcination temperature of 400° C. for 45 s to obtain pretreated graphite;

[0070] S2, 4g zinc nitrate, 4g aluminum nitrate and 5g urea were dissolved in 100mL water to prepare a mixed salt solution, and then 8g pretreated graphite and 0.5g sodium dodecylbenzene sulfonate were added thereto, stirred and dispersed evenly, and then transferred to a reactor for hydrothermal reaction, the temperature of the hydrothermal reaction was 150°C, and the time of the hydrothermal reaction was 18h. After the reaction was completed, the graphite-hydrotalcite composite material was obtained by centrifugation, washing and drying;

[0071] S3. Disperse 5 g of graphite-hydrotalcite composite material in 100 mL of 80 wt% ethanol aqueous solution, then add 1 g of silane coupling agent KH560, stir and react for 3 h, and after the reaction is completed, centrifuge, wash and dry to obtain a composite graphite material.

[0072] The preparation method of the modified carbon fiber is as follows: 2 g of dopamine hydrochloride is added to 50 mL of Tris-HCl buffer, the pH is adjusted to 10, and then 2 g of carbon fiber is added and soaked for 24 hours. After soaking, the carbon fiber is taken out and washed with water and vacuum dried to obtain the modified carbon fiber.

[0073] Compared with Example 1, Comparative Example 1 does not load nano titanium dioxide in the composite graphite material.

[0074] Comparative Example 2

[0075] A method for preparing a composite graphite sealing material comprises the following steps:

[0076] 60 parts of epoxy resin, 10 parts of maleic anhydride grafted POE, 10 parts of composite graphite material, 5 parts of carbon fiber, 2 parts of zinc stearate and 8 parts of curing agent ethylenediamine were stirred and mixed uniformly, and cured at 80° C. to obtain a composite graphite sealing material;

[0077] Wherein, the preparation method of the composite graphite material is as follows:

[0078] S1. Ultrasonic dispersion of 10 g expandable graphite powder in 100 mL of 30 wt % sodium hydroxide solution, drying, and then calcining in an ammonia atmosphere at a calcination temperature of 400° C. for 45 s to obtain pretreated graphite;

[0079] S2, 4g zinc nitrate, 4g aluminum nitrate and 5g urea were dissolved in 100mL water to prepare a mixed salt solution, and then 8g pretreated graphite, 4g tetrabutyl titanate and 0.5g sodium dodecylbenzene sulfonate were added thereto, stirred and dispersed evenly, and then transferred to a reactor for hydrothermal reaction, the temperature of the hydrothermal reaction was 150°C, and the time of the hydrothermal reaction was 18h. After the reaction was completed, the graphite-hydrotalcite-titanium dioxide composite material was obtained by centrifugation, washing and drying;

[0080] S3. Disperse 5 g of graphite-hydrotalcite-titanium dioxide composite material in 100 mL of 80 wt% ethanol aqueous solution, then add 1 g of silane coupling agent KH560, stir and react for 3 h, and after the reaction is completed, centrifuge, wash and dry to obtain a composite graphite material.

[0081] Compared with Example 1, Comparative Example 2 does not perform modification treatment on the carbon fiber.

[0082] The composite graphite sealing materials prepared in Examples 1-4 and Comparative Examples 1-2 were subjected to performance tests, wherein the tensile strength and elongation at break were measured according to the GB / T 2567-2021 method; the volume wear rate was measured according to the GB / T 3960-2016 method, with a load of 200N, a sliding speed of 0.43m / s in the reciprocating mode, and GCr15 bearing steel as the friction pair; the limiting oxygen index: tested according to GB / T 2406.2-2009, a sample size of type I was prepared, and the ignition method was A;

[0083] The test was conducted 3 times and the average value was taken. The test results are shown in the following table:

[0084]

[0085] Finally, it should be noted that the above embodiments do not limit the present invention in any form. For those skilled in the art, some modifications and improvements can be made to the present invention. Therefore, any modification or improvement made without departing from the spirit of the present invention belongs to the scope of protection claimed in the present invention.

Claims

1. A composite graphite sealing material, characterized in that: The raw materials include the following components in parts by weight: 60-80 parts of epoxy resin, 8-12 parts of maleic anhydride grafted POE, 10-15 parts of composite graphite material, 4-8 parts of modified carbon fiber, 1-3 parts of zinc stearate, and 5-10 parts of curing agent; Wherein, the preparation method of the composite graphite material is as follows: S1, ultrasonically dispersing expandable graphite powder in an alkaline solution, drying, and then calcining in an ammonia atmosphere to obtain pretreated graphite; S2, dissolving zinc nitrate, aluminum nitrate and urea in water to prepare a mixed salt solution, then adding pretreated graphite, tetrabutyl titanate and sodium dodecylbenzene sulfonate thereto, stirring and dispersing them evenly, then transferring them into a reactor for hydrothermal reaction, and after the reaction is completed, centrifuging, washing and drying to obtain a graphite-hydrotalcite-titanium dioxide composite material; S3, dispersing the graphite-hydrotalcite-titanium dioxide composite material in an ethanol aqueous solution, then adding a silane coupling agent KH560 thereto, stirring for reaction, and after the reaction is completed, centrifuging, washing, and drying to obtain a composite graphite material; The preparation method of the modified carbon fiber is as follows: dopamine hydrochloride is added to Tris-HCl buffer, the pH is adjusted to 8-10, and then carbon fiber is added and soaked for 18-24 hours, and after soaking, the modified carbon fiber is taken out, washed with water, and vacuum dried to obtain the modified carbon fiber.

2. The composite graphite sealing material according to claim 1, characterized in that: In step S1, the calcination temperature is 350-450° C., and the calcination time is 30-60 seconds.

3. The composite graphite sealing material according to claim 1, characterized in that: In step S2, the mass ratio of zinc nitrate, aluminum nitrate, urea, pretreated graphite, tetrabutyl titanate and sodium dodecylbenzene sulfonate is 4-8:3-5:4-6:5-10:3-5:0.4-0.

8.

4. The composite graphite sealing material according to claim 1, characterized in that: In step S2, the temperature of the hydrothermal reaction is 150-180° C., and the time of the hydrothermal reaction is 12-18 hours.

5. The composite graphite sealing material according to claim 1, characterized in that: In step S3, the mass ratio of the graphite-hydrotalcite composite material to the silane coupling agent KH560 is 5-10:1-2.

6. The composite graphite sealing material according to claim 1, characterized in that: The usage ratio of dopamine hydrochloride, Tris-HCl buffer and carbon fiber is 1-3g:50mL:1-3g.

7. The method for preparing the composite graphite sealing material according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: according to the formula, epoxy resin, maleic anhydride grafted POE, composite graphite material, modified carbon fiber, zinc stearate and curing agent are stirred and mixed evenly, and then cured to obtain the composite graphite sealing material.

8. Use of the composite graphite sealing material according to any one of claims 1 to 6 in sealing gaskets.

Citation Information

Patent Citations

  • Preparation method and application of chemical-bonded thermally-conductive insulation composite filling material

    CN106380630A

  • Silicone rubber composite graphite sealing material and preparation method and application thereof

    CN111995298A