A method for preparing rare earth ion embedded vanadium-based nanofiber membrane

By embedding rare earth ions into vanadium-based nanofiber membranes, using the dissolution-recrystallization process of vanadium oxides, the problem of strict temperature pressure control of metal ions embedded in the prior art is solved, and the structural stability of the material and zinc ion storage are achieved. The improvement of space reduces production costs and energy consumption.

CN118600645BActive Publication Date: 2024-11-29JIANGXI UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411035670.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-29
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

When the prior art embeds metal ions into vanadium-based materials, the temperature and pressure control is strict and costly, making it difficult to achieve performance improvement under mild conditions.

Method used

By preparing vanadium-based nanofiber membrane and immersing it in rare earth element chloride solution, the rare earth ions are embedded in the vanadium oxygen layer, and the dissolution-recrystallization process of vanadium oxide is used to adjust the crystal structure, realize the embedding of rare earth ions and improve the material structural stability and storage space of zinc ions.

Benefits of technology

Under mild conditions, the embeddedness of rare earth ions is achieved, which improves the structural stability of the vanadium oxygen layer and the diffusion capacity of zinc ions, reduces energy consumption and cost, and improves the cycling performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118600645B_ABST
    Figure CN118600645B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a vanadium-based nanofiber membrane embedded with rare earth ions. First, a spinning carrier, vanadium acetylacetonate, terephthalic acid and isophthalic acid are dissolved in an organic solvent to prepare a vanadium-based nanofiber electrostatic spinning solution; then, the vanadium-based nanofiber electrostatic spinning solution is used as a raw material for electrostatic spinning, and then the primary electrostatic spinning nanofiber membrane is subjected to high-temperature calcination to obtain a vanadium-based nanofiber membrane; then, the vanadium-based nanofiber membrane is immersed in a rare earth element chloride salt solution and allowed to stand, so that the rare earth ions are fully embedded in the vanadium oxide layer; then, the product is taken out, and the chloride ions on the surface are removed by washing with deionized water; then, high-temperature calcination is performed to remove structural water, and a vanadium-based nanofiber membrane embedded with rare earth ions is obtained. The present invention embeds rare earth ions into the vanadium oxide layer through the process of dissolving and recrystallizing vanadium oxide, thereby expanding the interlayer spacing, stabilizing the vanadium oxide layer, and improving the structural stability of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of nano materials and electrochemistry, and in particular is a method for preparing a rare earth ion embedded vanadium-based nanofiber membrane. Background Art

[0002] In recent years, the environmental pollution and energy shortage caused by the extensive use of fossil fuels have become increasingly serious, causing people to turn to cleaner and more sustainable renewable energy, such as wind energy, solar energy, tidal energy, etc. Due to the intermittent and extensive characteristics of wind energy, solar energy and other energy sources, the development of effective energy storage systems is imminent. As an advanced energy storage system with high energy density, good cycle performance and high voltage platform, lithium-ion batteries dominate the energy market. However, due to problems such as the shortage of lithium resources, scientists are still working hard to find alternatives.

[0003] Aqueous zinc-ion batteries have attracted widespread attention as an emerging energy storage system that is inexpensive, safe, and environmentally friendly. They have high mass specific capacity and volume specific capacity. Currently, manganese-based materials, vanadium-based materials, Prussian blue and its analogs, and polyanion compounds are considered to be ideal positive electrode materials. However, manganese-based and Prussian blue exhibit low capacity and poor cycle performance as positive electrode materials. Vanadium-based materials have become a research hotspot in the field of positive electrode materials for zinc-ion batteries due to their unique VO octahedral structure and multiple oxidation states of the V element. Vanadium-based materials can provide a large amount of storage space for the extraction and embedding of zinc ions. However, after repeated extraction and embedding, the weak interaction force between the layers cannot maintain the stability of their structure. Therefore, embedding an appropriate amount of metal ions can reinforce the VO layer.

[0004] The current driving force for the introduction of metal ion embedding is mainly based on the crystal phase transformation or reorganization growth during the hydrothermal process, which has strict temperature and pressure control and high cost. Therefore, it is urgent to explore a metal ion with better performance and embed it into the vanadium oxide layer through a mild and simple reaction method to improve the performance of vanadium-based materials. Summary of the invention

[0005] In view of the deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a method for preparing a rare earth ion embedded vanadium-based nanofiber membrane.

[0006] The technical solution of the present invention to solve the technical problem is to provide a method for preparing a rare earth ion embedded vanadium-based nanofiber membrane, characterized in that the method comprises the following steps:

[0007] (1) Preparation of vanadium-based nanofiber electrospinning solution: dissolving a spinning carrier, vanadyl acetylacetonate, terephthalic acid and isophthalic acid in an organic solvent to prepare a vanadium-based nanofiber electrospinning solution;

[0008] (2) Preparation of vanadium-based nanofiber membrane: electrospinning is performed using vanadium-based nanofiber electrospinning liquid as a raw material to form a primary electrospun nanofiber membrane; the primary electrospun nanofiber membrane is then calcined at a high temperature to decompose organic matter in the membrane to obtain a vanadium-based nanofiber membrane;

[0009] (3) Preparation of rare earth ion embedded vanadium-based nanofiber membrane: The vanadium-based nanofiber membrane is immersed in a rare earth element chloride salt solution and allowed to stand to allow the rare earth ions to fully embed into the vanadium oxide layer until the color of the vanadium-based nanofiber membrane no longer changes; the product is then taken out and washed with deionized water to remove the chloride ions on the surface; and then high-temperature calcination is performed to remove structural water, thereby increasing the crystallinity to obtain a rare earth ion embedded vanadium-based nanofiber membrane.

[0010] Compared with the prior art, the present invention has the following beneficial effects:

[0011] (1) The present invention utilizes the fact that vanadium oxide can be partially dissolved in aqueous solution, and improves its chemical environment through a suitable salt solution to promote its crystal interface confined adsorption and crystal growth. Through the process of vanadium oxide dissolution-recrystallization, rare earth ions are embedded into the vanadium oxide layer under mild conditions, which effectively adjusts the crystal structure of vanadium oxide, expands the interlayer spacing, improves the storage space of zinc ions, stabilizes the vanadium oxide layer, and improves the structural stability of the material. At the same time, the electrostatic interaction between zinc ions and the vanadium oxide layer is alleviated, providing an undisturbed internal environment for the embedding / de-embedding of ions, which is beneficial to the diffusion of zinc ions between the vanadium oxide layers.

[0012] (2) The present invention embeds rare earth ions whose size, charge and chemical properties are different from those of other elements in the vanadium-based nanofiber membrane. When the rare earth ions are introduced into the crystal structure of the vanadium-based nanofiber membrane, on the one hand, they interact with the atoms or ions in the vanadium-based nanofiber membrane, causing the crystal structure to change, which is beneficial to the rapid diffusion of zinc ions between the vanadium oxide layers. On the other hand, the rare earth ions can fill the gaps in the crystal structure of the vanadium-based nanofiber membrane or provide additional connection points to prevent the structure from collapsing after the zinc ions escape, thereby enhancing the structural stability of the vanadium-based nanofiber membrane.

[0013] (3) The present invention is simple and easy to implement. Compared with the high temperature and high pressure environment required for traditional metal ion embedding, the environment and technology required for this method are relatively mild and can be implemented at room temperature and pressure, with low energy consumption and cost.

[0014] (4) The rare earth ion embedded vanadium-based nanofiber membrane prepared by the present invention has broad application prospects in energy storage fields such as aqueous and organic embedded secondary batteries, and its nanostructure can provide more reaction sites for redox reactions during the charging and discharging process. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is an electron microscope image of the vanadium-based nanofiber membrane prepared in Example 1 of the present invention;

[0016] Figure 2 This is an electron microscope image of the rare earth ion embedded vanadium-based nanofiber membrane prepared in Example 1 of the present invention;

[0017] Figure 3 The electrochemical performance of the rare earth ion embedded vanadium-based nanofiber membrane prepared in Example 1 of the present invention as an electrode. DETAILED DESCRIPTION

[0018] The specific embodiments of the present invention are given below. The specific embodiments are only used to further illustrate the present invention in detail and do not limit the protection scope of the present invention.

[0019] The present invention provides a method for preparing a rare earth ion embedded vanadium-based nanofiber membrane (hereinafter referred to as the method), characterized in that the method comprises the following steps:

[0020] (1) Preparation of vanadium-based nanofiber electrospinning solution: Spinning carrier, vanadium acetylacetonate (VO(acac) 2 ), terephthalic acid (PTA) and isophthalic acid (PIA) are dissolved in an organic solvent to prepare a vanadium-based nanofiber electrospinning solution;

[0021] Preferably, in step (1), the spinning carrier is polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PVA) or polyvinylidene fluoride (PVDF); and the organic solvent is dimethylformamide (DMF), dimethylacetamide (DMAC) or methyl pyrrolidone (NMP).

[0022] Preferably, in step (1), the molecular weight of PVP is in the range of 400,000 to 1,000,000.

[0023] Preferably, in step (1), the mass ratio of the spinning carrier to the vanadyl acetylacetonate is 1-3:1, the mass of terephthalic acid is 10-15% of the mass of the spinning carrier, the mass of isophthalic acid is 2-5% of the mass of the spinning carrier, and the concentration of the spinning carrier is 10-15wt%.

[0024] Preferably, in step (1), the dissolution process is: stirring thoroughly at room temperature until each component is completely dissolved in the organic solvent.

[0025] (2) Preparation of vanadium-based nanofiber membrane: electrospinning is performed using vanadium-based nanofiber electrospinning liquid as a raw material to form a primary electrospun nanofiber membrane; the primary electrospun nanofiber membrane is then calcined at a high temperature to decompose organic matter in the membrane to obtain a vanadium-based nanofiber membrane;

[0026] Preferably, in step (2), the electrospinning process is: the electric field strength is 15-40 kV, the flow rate of the propulsion pump is 0.5-3 ml / h, the distance from the needle tip to the receiving device is 15-25 cm, the air humidity is 30-60%, and the temperature is 20-40 ° C.

[0027] Preferably, in step (2), the calcination temperature is 300-600°C, the heating rate is 0.5-3°C / min, the holding time is 1-3h, and the calcination environment is an oxygen-containing environment; the oxygen-containing environment is an air atmosphere or an oxygen atmosphere.

[0028] (3) Preparation of rare earth ion embedded vanadium-based nanofiber membrane: The vanadium-based nanofiber membrane is immersed in a rare earth element chloride salt solution and allowed to stand to allow the rare earth ions to fully embed into the vanadium oxide layer until the color of the vanadium-based nanofiber membrane no longer changes; the product is then taken out and washed with deionized water to remove the chloride ions on the surface; and then high-temperature calcination is performed to remove structural water (including water molecules introduced when the rare earth ions are embedded), thereby increasing the crystallinity to obtain a rare earth ion embedded vanadium-based nanofiber membrane.

[0029] Preferably, in step (3), the rare earth element chloride solution is prepared by: dissolving rare earth chloride in deionized water to prepare a rare earth element chloride solution; the rare earth chloride is yttrium chloride (YCl 3 ), europium chloride (EuCl 3 )、Lanthanum chloride(LaCl 3 ) or cerium chloride (CeCl 3 ).

[0030] Preferably, in step (3), the concentration of the rare earth element chloride salt solution is 0.5-3 mol / l.

[0031] Preferably, in step (3), the standing condition is normal temperature and pressure (preferably standard atmospheric pressure, temperature of 20-60° C.), and the standing time is 24-48 h.

[0032] Preferably, in step (3), the calcination temperature is 200-500°C, the heating rate is 1-2°C / min, the holding time is 1-3h, and the calcination environment is an oxygen-containing environment; the oxygen-containing environment is an air atmosphere or an oxygen atmosphere.

[0033] Embodiment 1:

[0034] (1) Preparation of vanadium-based nanofiber electrospinning solution: At room temperature, 10.5 g of PVP powder and 10.5 g of VO(acac) were mixed. 2 powder, 1.05 g of PTA powder and 0.3 g of PIA powder were dissolved in DMF to prepare the vanadium-based nanofiber electrospinning solution;

[0035] (2) Preparation of vanadium-based nanofiber membrane: Electrospinning was performed using vanadium-based nanofiber electrospinning liquid as raw material to form a primary electrospun nanofiber membrane; the primary electrospun nanofiber membrane was then heated to 300°C at a heating rate of 0.5°C / min and calcined for 1 h to decompose the organic matter in the membrane to obtain V 2 O 5 Vanadium-based nanofiber membranes;

[0036] The electrospinning process was as follows: the electric field strength was 15 kV, the flow rate of the propulsion pump was 0.5 ml / h, the distance from the needle tip to the receiving device was 15 cm, the air humidity was 30%, and the temperature was 20 °C;

[0037] (3) Preparation of rare earth ion embedded vanadium-based nanofiber membrane: 9.78 g of YCl 3 Dissolve in deionized water to prepare 0.5 mol / L YCl 3 Solution; then V 2 O 5 Vanadium-based nanofiber membrane impregnated with YCl 3 The solution was allowed to stand at standard atmospheric pressure and temperature of 20°C for 24 hours to allow the rare earth ions to be fully embedded in the vanadium oxide layer until the color of the vanadium-based nanofiber membrane no longer changed; the product was then taken out and washed with deionized water to remove the chloride ions on the surface; the temperature was then increased to 200°C in a muffle furnace at a heating rate of 1°C / min and calcined for 2 hours to remove structural water, thereby increasing the crystallinity to obtain a vanadium-based nanofiber membrane embedded with rare earth ions.

[0038] Depend on Figure 1 It can be seen that the fiber diameter of the vanadium-based nanofiber membrane prepared in Example 1 is about 200 nm and exhibits good continuity.

[0039] Depend on Figure 2 It can be seen that after rare earth ions are embedded in the vanadium-based nanofiber membrane, the continuity of the entire nanofiber increases and the diameter of the fiber is reduced to about 100 nm.

[0040] Depend on Figure 3 It can be seen that after assembling an aqueous zinc ion battery by embedding rare earth ions into a vanadium-based nanofiber membrane as the positive electrode material, the initial discharge capacity of the battery is 320 mAh / g at a current density of 0.3 A / g, and the discharge capacity is 288 mAh / g after 100 cycles. The capacity retention rate is 90%, and the coulombic efficiency is close to 100% during the charge and discharge process.

[0041] Embodiment 2:

[0042] (1) Preparation of vanadium-based nanofiber electrospinning solution: At room temperature, 12.9 g of PVA powder and 12.9 g of VO(acac) were mixed. 2powder, 1.29 g of PTA powder and 0.4 g of PIA powder were dissolved in DMF to prepare the vanadium-based nanofiber electrospinning solution;

[0043] (2) Preparation of vanadium-based nanofiber membrane: Electrospinning was performed using vanadium-based nanofiber electrospinning liquid as raw material to form a primary electrospun nanofiber membrane; the primary electrospun nanofiber membrane was then heated to 400°C at a heating rate of 1°C / min and calcined for 2 h to decompose the organic matter in the membrane to obtain V 2 O 5 Vanadium-based nanofiber membranes;

[0044] The electrospinning process was as follows: the electric field strength was 20 kV, the flow rate of the propulsion pump was 1 ml / h, the distance from the needle tip to the receiving device was 20 cm, the air humidity was 30%, and the temperature was 20 °C;

[0045] (3) Preparation of rare earth ion embedded vanadium-based nanofiber membrane: 24.64 g of CeCl 3 Dissolve in deionized water to prepare 1 mol / L CeCl 3 Solution; then V 2 O 5 Vanadium-based nanofiber membranes impregnated in CeCl 3 The solution was allowed to stand at standard atmospheric pressure and 35°C for 24 hours to allow the rare earth ions to be fully embedded in the vanadium oxide layer until the color of the vanadium-based nanofiber membrane no longer changed; the product was then taken out and washed with deionized water to remove the chloride ions on the surface; the temperature was then increased to 350°C in a muffle furnace at a heating rate of 1°C / min and calcined for 2 hours to remove structural water, thereby increasing the crystallinity to obtain a vanadium-based nanofiber membrane embedded with rare earth ions.

[0046] After rare earth ions were embedded in vanadium-based nanofiber membrane as the positive electrode material and an aqueous zinc ion battery was assembled, the capacity retention rate was 92% after 200 cycles at a current density of 0.5A / g.

[0047] Embodiment 3:

[0048] (1) Preparation of vanadium-based nanofiber electrospinning solution: 10.5 g of PVDF powder and 5.25 g of VO(acac) were mixed at room temperature. 2 powder, 1.58 g of PTA powder and 0.4 g of PIA powder were dissolved in DMAC to prepare the electrospinning solution for vanadium-based nanofibers;

[0049] (2) Preparation of vanadium-based nanofiber membrane: Electrospinning was performed using vanadium-based nanofiber electrospinning liquid as raw material to form a primary electrospun nanofiber membrane. The primary electrospun nanofiber membrane was then heated to 450°C at a heating rate of 1°C / min and calcined for 2 h to decompose the organic matter in the membrane to obtain V2 O 5 Vanadium-based nanofiber membranes;

[0050] The electrospinning process was as follows: the electric field strength was 20 kV, the flow rate of the propulsion pump was 0.5 ml / h, the distance from the needle tip to the receiving device was 20 cm, the air humidity was 30%, and the temperature was 20 °C;

[0051] (3) Preparation of rare earth ion embedded vanadium-based nanofiber membrane: 25.83 g of EuCl 3 Dissolve in deionized water to prepare 1 mol / L EuCl 3 Solution; then V 2 O 5 Vanadium-based nanofiber membrane impregnated with EuCl 3 The solution was allowed to stand at standard atmospheric pressure and 45°C for 36 hours to allow the rare earth ions to be fully embedded in the vanadium oxide layer until the color of the vanadium-based nanofiber membrane no longer changed; the product was then taken out and washed with deionized water to remove the chloride ions on the surface; the temperature was then increased to 350°C in a muffle furnace at a heating rate of 2°C / min and calcined for 3 hours to remove structural water, thereby increasing the crystallinity to obtain a vanadium-based nanofiber membrane embedded with rare earth ions.

[0052] After rare earth ions were embedded in vanadium-based nanofiber membrane as the positive electrode material and an aqueous zinc ion battery was assembled, the capacity retention rate was 95% after 100 cycles at a current density of 0.5A / g.

[0053] Embodiment 4:

[0054] (1) Preparation of vanadium-based nanofiber electrospinning solution: At room temperature, 17.46 g of PVDF powder and 8.73 g of VO(acac) were added. 2 powder, 1.9 g of PTA powder and 0.6 g of PIA powder were dissolved in DMF to prepare the vanadium-based nanofiber electrospinning solution;

[0055] (2) Preparation of vanadium-based nanofiber membrane: Electrospinning was performed using vanadium-based nanofiber electrospinning liquid as raw material to form a primary electrospun nanofiber membrane; the primary electrospun nanofiber membrane was then heated to 500°C at a heating rate of 3°C / min and calcined for 3 h to decompose the organic matter in the membrane to obtain V 2 O 5 Vanadium-based nanofiber membranes;

[0056] The electrospinning process was as follows: the electric field strength was 30 kV, the flow rate of the propulsion pump was 2 ml / h, the distance from the needle tip to the receiving device was 20 cm, the air humidity was 30%, and the temperature was 35 °C;

[0057] (3) Preparation of rare earth ion embedded vanadium-based nanofiber membrane: 49.05 g of LaCl3 Dissolve in deionized water to prepare 2 mol / L LaCl 3 Solution; then V 2 O 5 Vanadium-based nanofiber membrane impregnated with LaCl 3 The solution was allowed to stand at standard atmospheric pressure and 55°C for 36 hours to allow the rare earth ions to be fully embedded in the vanadium oxide layer until the color of the vanadium-based nanofiber membrane no longer changed; the product was then taken out and washed with deionized water to remove the chloride ions on the surface; the temperature was then increased to 450°C in a muffle furnace at a heating rate of 1.5°C / min and calcined for 2 hours to remove structural water, thereby increasing the crystallinity to obtain a vanadium-based nanofiber membrane embedded with rare earth ions.

[0058] After rare earth ions were embedded in vanadium-based nanofiber membrane as the positive electrode material and an aqueous zinc ion battery was assembled, the capacity retention rate was 92% after 100 cycles at a current density of 0.5A / g.

[0059] Embodiment 5:

[0060] (1) Preparation of vanadium-based nanofiber electrospinning solution: At room temperature, 18.96 g of PVP powder and 6.32 g of VO(acac) were added. 2 powder, 2.84 g of PTA powder and 0.4 g of PIA powder were dissolved in NMP to prepare the vanadium-based nanofiber electrospinning solution;

[0061] (2) Preparation of vanadium-based nanofiber membrane: Electrospinning was performed using vanadium-based nanofiber electrospinning liquid as raw material to form a primary electrospun nanofiber membrane. The primary electrospun nanofiber membrane was then heated to 600°C at a heating rate of 3°C / min and calcined for 3 h to decompose the organic matter in the membrane to obtain V 2 O 5 Vanadium-based nanofiber membranes;

[0062] The electrospinning process was as follows: the electric field strength was 30 kV, the flow rate of the propulsion pump was 2 ml / h, the distance from the needle tip to the receiving device was 20 cm, the air humidity was 30%, and the temperature was 35 °C;

[0063] (3) Preparation of rare earth ion embedded vanadium-based nanofiber membrane: 58.5 g of YCl 3 Dissolve in deionized water to prepare 3 mol / L YCl 3 Solution; then V 2 O 5 Vanadium-based nanofiber membrane impregnated with YCl 3The solution was allowed to stand at standard atmospheric pressure and 60°C for 48 hours to allow the rare earth ions to be fully embedded in the vanadium oxide layer until the color of the vanadium-based nanofiber membrane no longer changed; the product was then taken out and washed with deionized water to remove the chloride ions on the surface; the temperature was then increased to 500°C in a muffle furnace at a heating rate of 2°C / min and calcined for 3 hours to remove structural water, thereby increasing the crystallinity to obtain a vanadium-based nanofiber membrane embedded with rare earth ions.

[0064] After rare earth ions were embedded in vanadium-based nanofiber membrane as the positive electrode material and an aqueous zinc ion battery was assembled, the capacity retention rate was 90% after 1000 cycles at a current density of 2A / g.

[0065] Comparative Example 1:

[0066] (1) Embedding rare earth ions into vanadium oxide by hydrothermal method: 0.9 g oxalic acid (H 2 C 2 O 4 ) and 0.9g of V 2 O 5 Add to 80 mL of deionized water and stir at 50 °C until the suspension turns dark blue. Then add 8.18 g of CeCl 3 Then, 10 mL of 0.15 mol / L urea precipitant was added, and after sufficient stirring, the mixture was transferred to a sealed polytetrafluoroethylene reactor and kept at 190 °C for 72 h. After the reaction, the product was filtered and washed to obtain VO 2 Precursor;

[0067] (2) VO 2 The precursor was placed in a tubular furnace for heat treatment. Nitrogen was passed through for 30 minutes before heating to expel air and water vapor in the tube and create an inert atmosphere. The nitrogen flow rate was 0.4L / min, and the heating rate of the tubular furnace was 5℃ / min. The temperature was raised to 800℃ and maintained for 5 hours. After that, the heating was stopped and the sample was cooled with the furnace to obtain rare earth ion embedded vanadium oxide.

[0068] After assembling an aqueous zinc-ion battery by embedding rare earth ions into vanadium oxide as the positive electrode material, the capacity retention rate was 52% after 1,000 cycles at a current density of 2A / g.

[0069] Any matters not described in the present invention are applicable to the prior art.

Claims

1. A method for preparing a rare earth ion embedded vanadium-based nanofiber membrane, characterized in that: The method comprises the following steps: (1) Preparation of vanadium-based nanofiber electrospinning solution: dissolving a spinning carrier, vanadyl acetylacetonate, terephthalic acid and isophthalic acid in an organic solvent to prepare a vanadium-based nanofiber electrospinning solution; The spinning carrier is polyvinyl pyrrolidone, polyvinyl alcohol or polyvinylidene fluoride; the organic solvent is dimethylformamide, dimethylacetamide or methylpyrrolidone; The mass ratio of the spinning carrier to the vanadyl acetylacetonate is 1-3:1, the mass of terephthalic acid is 10-15% of the mass of the spinning carrier, the mass of isophthalic acid is 2-5% of the mass of the spinning carrier, and the concentration of the spinning carrier is 10-15wt%; (2) Preparation of vanadium-based nanofiber membrane: electrospinning is performed using vanadium-based nanofiber electrospinning liquid as a raw material to form a primary electrospun nanofiber membrane; the primary electrospun nanofiber membrane is then calcined at a high temperature to decompose organic matter in the membrane to obtain a vanadium-based nanofiber membrane; (3) Preparation of rare earth ion embedded vanadium-based nanofiber membrane: The vanadium-based nanofiber membrane is immersed in a rare earth element chloride salt solution and allowed to stand to allow the rare earth ions to be fully embedded in the vanadium oxide layer until the color of the vanadium-based nanofiber membrane no longer changes; the product is then taken out and washed with deionized water to remove the chloride ions on the surface; and then high-temperature calcination is performed to remove structural water, thereby increasing the crystallinity, to obtain a rare earth ion embedded vanadium-based nanofiber membrane; The preparation of rare earth element chloride salt solution is as follows: rare earth chloride is dissolved in deionized water to prepare rare earth element chloride salt solution; the rare earth chloride is yttrium chloride, europium chloride, lanthanum chloride or cerium chloride.

2. The method for preparing rare earth ion embedded vanadium-based nanofiber membrane according to claim 1, characterized in that: In step (1), the molecular weight of polyvinyl pyrrolidone ranges from 400,000 to 1,000,000.

3. The method for preparing rare earth ion embedded vanadium-based nanofiber membrane according to claim 1, characterized in that: In step (2), the electrospinning process is as follows: the electric field strength is 15-40 kV, the flow rate of the propulsion pump is 0.5-3 ml / h, the distance from the needle tip to the receiving device is 15-25 cm, the air humidity is 30-60%, and the temperature is 20-40°C.

4. The method for preparing rare earth ion embedded vanadium-based nanofiber membrane according to claim 1, characterized in that: In step (2), the calcination temperature is 300-600°C, the heating rate is 0.5-3°C / min, the holding time is 1-3h, and the calcination environment is an oxygen-containing environment.

5. The method for preparing rare earth ion embedded vanadium-based nanofiber membrane according to claim 1, characterized in that: In step (3), the concentration of the rare earth element chloride solution is 0.5-3 mol / l.

6. The method for preparing rare earth ion embedded vanadium-based nanofiber membrane according to claim 1, characterized in that: In step (3), the standing condition is normal pressure, the temperature is 20-60°C, and the standing time is 24-48h.

7. The method for preparing rare earth ion embedded vanadium-based nanofiber membrane according to claim 1, characterized in that: In step (3), the calcination temperature is 200-500°C, the heating rate is 1-2°C / min, the holding time is 1-3h, and the calcination environment is an oxygen-containing environment.

Citation Information

Patent Citations

  • Preparation method of zinc vanadic acid nanofiber negative electrode material for lithium ion battery

    CN106159248A

  • Preparation method of vanadium-based nano material for positive electrode of aqueous zinc ion battery

    CN111952580A

  • Preparation method of vanadium pentoxide-based magnesium battery positive electrode material

    CN118343834A

  • Vanadium pentoxide / RGO-coated lithium nickel cobalt manganese oxide positive electrode material and preparation method therefor

    WO2022048346A1