A polymer electrolyte and its preparation method and application

By introducing imidazole-type ionic liquid and uniformly dispersed lithium salt in the polymer electrolyte, the problems of insufficient conductivity, migration number and strength in lithium secondary batteries are solved, and the performance of the battery is significantly improved.

CN118610575BActive Publication Date: 2024-10-29BYD CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411075813.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-29
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

Existing polyoxyethylene-based solid electrolytes in lithium secondary batteries have problems such as low ionic conductivity, low lithium ion migration number, and poor mechanical strength, resulting in poor rate performance, cycle performance, and safety performance of the battery.

Method used

By introducing imidazole ionic liquid into the polymer electrolyte for block copolymerization modification, a cross-linked body is formed, which increases the uniform dispersion of lithium salt and improves the ionic conductivity, lithium ion migration number and mechanical strength of the electrolyte.

Benefits of technology

It achieves the excellent ionic conductivity, lithium ion migration number and mechanical strength of the polymer electrolyte, and improves the rate performance, cycle performance and safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118610575B_ABST
    Figure CN118610575B_ABST
Patent Text Reader

Abstract

The present invention provides a polymer electrolyte and a preparation method and application thereof, wherein the polymer electrolyte comprises a polymer and a lithium salt, wherein the polymer comprises a cross-linked body obtained by polymerization of a compound represented by formula I, wherein R is selected from bis(trifluoromethylsulfonyl)imide, bis(fluorosulfonyl)imide, perchlorate, tetrafluoroborate, dioxalate borate, difluorooxalate borate or trifluoromethylsulfonate; m is selected from an integer between 10 and 50, and n is selected from an integer between 4 and 30. The polymer electrolyte of the present invention has excellent ionic conductivity, lithium ion transference number and mechanical strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries and relates to a polymer electrolyte and a preparation method and application thereof. Background Art

[0002] With the widespread application of smart electronic devices, electric vehicles and large-scale energy storage equipment, lithium secondary batteries with higher energy density and cycle life are urgently needed. Electrolyte is an important component of lithium secondary batteries, which plays the role of transporting ions and conducting current between the positive and negative electrodes. Compared with liquid electrolytes, solid electrolytes have higher mechanical strength and stability, can effectively inhibit the growth of lithium dendrites, and reduce the risk of battery short circuit. In addition, they can maintain good performance in a wide temperature range and have good temperature stability. In addition, solid electrolytes have good chemical stability and are not easy to react with electrodes, which is conducive to extending the cycle life of the battery. Polymer solid electrolytes are a widely used solid electrolyte with good flexibility and processability, and have been widely studied. Polyethylene oxide (PEO) has a wide range of sources and good compatibility with lithium salts. It is usually used as the main raw material of polymer solid electrolytes. However, the existing polyethylene oxide solid electrolytes still have problems such as low ionic conductivity, low lithium ion migration number, and poor mechanical strength during use, resulting in poor rate performance, cycle performance and safety performance of the battery. Summary of the invention

[0003] The present invention provides a polymer electrolyte having excellent ion conductivity, lithium ion transference number and mechanical strength.

[0004] The present invention also provides a method for preparing a polymer electrolyte, which includes adding a lithium salt before cross-linking the compound represented by initiation formula I so that the lithium salt is uniformly dispersed in the cross-linked body, thereby obtaining a polymer electrolyte with excellent ionic conductivity, lithium ion migration number and mechanical strength.

[0005] The present invention also provides a battery, which comprises the polymer electrolyte and thus has excellent rate performance, cycle performance and safety performance.

[0006] The present invention also provides an electronic device. Since the electronic device comprises the battery, the electronic device also has excellent rate performance, cycle performance and safety performance during use.

[0007] The present invention provides a polymer electrolyte, comprising a polymer and a lithium salt, wherein the polymer comprises a cross-linked body obtained by polymerizing a compound represented by formula I:

[0008]

[0009] In formula I, R is selected from bistrifluoromethylsulfonyl imide, bisfluorosulfonyl imide, perchlorate, tetrafluoroborate, dioxalatoborate, difluorooxalatoborate or trifluoromethylsulfonate; m is selected from an integer between 10 and 50, and n is selected from an integer between 4 and 30.

[0010] The polymer electrolyte as described above, wherein 15≤m≤30, and / or 8≤n≤25.

[0011] The polymer electrolyte as described above, wherein 100≤m×n≤750.

[0012] The polymer electrolyte as described above, wherein the molar ratio of the polyethylene glycol structural unit in the compound of Formula I to the lithium salt is (10-25):1.

[0013] The polymer electrolyte as described above, wherein the lithium salt includes one or more of lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium dioxalatoborate, and lithium perchlorate.

[0014] The present invention also provides a method for preparing the polymer electrolyte as described above, which comprises the following steps:

[0015] A free radical initiator is added to a mixed system of the compound shown in formula I and a lithium salt to initiate a polymerization reaction to obtain the polymer electrolyte.

[0016] The preparation method as described above, wherein the compound represented by formula I is prepared by a method comprising the following steps:

[0017] 1) reacting the compound represented by formula II, formaldehyde and glyoxal under the action of protonic acid HA to obtain a compound represented by formula III;

[0018]

[0019] 2) reacting the compound represented by formula III, allylamine, formaldehyde and glyoxal under the action of protonic acid HA to obtain the compound represented by formula IV;

[0020]

[0021] 3) subjecting the compound represented by formula IV to an ion exchange reaction with LiR to obtain the compound represented by formula I;

[0022] .

[0023] The preparation method as described above, wherein the polymerization reaction temperature is 60-100° C. and the time is 4-12 hours.

[0024] The present invention also provides a battery, comprising a positive electrode, a negative electrode and an electrolyte layer located between the positive electrode and the negative electrode, wherein the electrolyte layer comprises the polymer electrolyte as described above.

[0025] In the battery as described above, the thickness of the electrolyte layer is 20-50 μm.

[0026] The present invention also provides an electronic device, comprising the battery as described above.

[0027] The implementation of the present invention has at least the following beneficial effects:

[0028] 1) The polymer electrolyte of the present invention includes a crosslinked body obtained by polymerization of the compound shown in Formula I. The crosslinked body is modified by block copolymerization of the polyethylene glycol matrix through an imidazole-type ionic liquid, which destroys the order of the polyethylene glycol chain segment, reduces the crystallinity of the electrolyte, and improves the ionic conductivity of the polymer electrolyte. The imidazole-type ionic liquid unit can also adsorb anions in the lithium salt through electrostatic action, thereby increasing the lithium ion migration number, reducing concentration polarization, and improving the rate performance of the battery. In addition, compared with the linear molecular structure, the crosslinked body can significantly improve the mechanical strength of the polymer electrolyte, avoid short circuits between the positive and negative electrodes, and improve the safety performance of the battery. In summary, the polymer electrolyte of the present invention has excellent ionic conductivity, lithium ion migration number, and mechanical strength.

[0029] 2) The preparation method of the polymer electrolyte provided by the present invention comprises adding a lithium salt before cross-linking the compound represented by formula I, so that the lithium salt is evenly dispersed in the cross-linked body, thereby obtaining a polymer electrolyte with excellent ionic conductivity, lithium ion migration number and mechanical strength.

[0030] 3) Since the battery provided by the present invention includes the above-mentioned polymer electrolyte with excellent ionic conductivity, lithium ion transference number and mechanical strength, the battery has excellent cycle performance, rate performance and safety performance. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] PEO molecular chains have a high dielectric constant and can dissolve many lithium salts. They are recognized as a matrix suitable for preparing all-solid-state electrolytes. However, pure PEO polymers are easy to crystallize, resulting in less amorphous phase structures that can conduct lithium ions, which in turn makes the ionic conductivity of solid electrolytes low. In order to improve its ionic conductivity, the operating temperature can be increased to reduce the crystallinity of PEO polymers, but after the crystallinity decreases, the mechanical strength of the electrolyte also decreases, resulting in easy contact and short circuit between the positive and negative electrodes. In addition, the principle of PEO conducting lithium ions is to coordinate with lithium ions through the lone pair of electrons in the oxygen atoms of the molecular chain, thereby realizing the transmission of lithium ions, but the anions in the lithium salts will not interact with the polymers, so the transmission ability of anions under the electric field is stronger than that of lithium ions, resulting in a lower migration number of lithium ions. Accordingly, the battery is prone to concentration polarization and uneven lithium ion deposition during the charge and discharge process, which ultimately makes the battery's safety performance, rate performance and cycle performance poor.

[0033] Based on this, the present invention provides a polymer electrolyte, comprising a polymer and a lithium salt, wherein the polymer comprises a cross-linked body obtained by polymerization of a compound represented by Formula I:

[0034]

[0035] In formula I, R is selected from bistrifluoromethylsulfonyl imide, bisfluorosulfonyl imide, perchlorate, tetrafluoroborate, dioxalatoborate, difluorooxalatoborate or trifluoromethylsulfonate; m is selected from an integer between 10 and 50, and n is selected from an integer between 4 and 30.

[0036] The compound shown in formula I is obtained by introducing an imidazole-type ionic liquid into a polyethylene glycol matrix and performing block copolymerization modification on the same. The terminal groups all contain allyl groups, and under the initiation of a free radical initiator, the compound can self-crosslink to form a crosslinked body with a network structure, wherein by limiting the values ​​of m and n within the above range, a suitable amount of polyethylene glycol segments and imidazole-type ionic liquid units can be distributed in the crosslinked body, wherein the polyethylene glycol segments are used to promote the conduction of lithium ions, and at the same time, the electrolyte can have good flexibility, maintain good compatibility with the positive and negative electrodes, reduce the interface impedance, and improve the cycle performance of the battery; the imidazole-type ionic liquid unit can, on the one hand, destroy the orderliness of the polyethylene glycol segments, reduce the crystallinity of the electrolyte, and improve its ionic conductivity, and on the other hand, can adsorb anions in the lithium salt through electrostatic action, further increase the lithium ion migration number, reduce concentration polarization, and improve the rate performance of the battery. In addition, the cross-linked body has a three-dimensional network structure, which has higher mechanical strength than the linear molecular structure. Even when it is used in lithium metal solid-state batteries with a high surface density positive electrode, it is not easy to cause a short circuit between the positive and negative electrodes, so that the battery has both excellent energy density and safety performance.

[0037] In summary, the polymer electrolyte of the present invention, by including a cross-linked body of the compound represented by Formula I, can make the polymer electrolyte have higher ionic conductivity, lithium ion migration number and mechanical strength, thereby enabling the battery to have excellent energy density, rate performance, cycle performance and safety performance.

[0038] Further, 15≤m≤30, and / or, 8≤n≤25. Among them, the role of n is to control the ratio of ethoxy repeating units and imidazole units, and m controls the length of the chain segment in the middle of the cross-linked network, that is, the length of the chain segment between two vinyl groups, which will affect the strength of the network. When m is small, the rigidity is too strong after cross-linking, the electrolyte is brittle and the contact with the positive and negative electrodes is not good. When m is large, the strength after cross-linking will not be very good. Based on the above considerations, further controlling the values ​​of m and n within the above range is conducive to making the cross-linked body have both good flexibility and mechanical strength.

[0039] Furthermore, 100≤m×n≤750. Studies have shown that when the value of m×n is within the above-defined range, the polymer electrolyte can have excellent lithium ion transference number, ionic conductivity and mechanical strength.

[0040] As mentioned above, the polyethylene glycol segment can promote the conduction of lithium ions. Based on this, the dosage ratio of the polyethylene glycol structural unit and the lithium salt in the compound shown in Formula I was studied, and it was found that when the molar ratio of the polyethylene glycol structural unit to the lithium salt in the compound shown in Formula I is (10-25):1, the electrolyte can have a higher ion conductivity. Exemplarily, the molar ratio of the polyethylene glycol structural unit to the lithium salt can be 10:1, 13:1, 15:1, 18:1, 20:1, 23:1, 25:1 or a range consisting of any two of the above molar ratios.

[0041] The present invention does not specifically limit the type of lithium salt, which can be selected from lithium salts commonly used in polymer electrolytes. Preferably, the lithium salt includes one or more of lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium dioxalatoborate, and lithium perchlorate.

[0042] The present invention also provides a method for preparing the polymer electrolyte as described above, comprising the following steps:

[0043] A free radical initiator is added to a mixed system of the compound shown in formula I and a lithium salt to initiate a polymerization reaction to obtain a polymer electrolyte.

[0044] The preparation method of the present invention adds a free radical initiator to a mixed system of the compound shown in formula I and a lithium salt to initiate a polymerization reaction, so that the lithium salt can be evenly distributed in the cross-linked body while the cross-linked body is formed, thereby obtaining a polymer electrolyte with excellent ionic conductivity, lithium ion migration number and mechanical strength.

[0045] The present invention does not particularly limit the preparation method of the compound represented by formula I, and it can be prepared by referring to conventional methods in the art.

[0046] In an optional embodiment, the compound represented by formula I can be prepared by a method comprising the following steps:

[0047] 1) reacting the compound represented by formula II, formaldehyde and glyoxal under the action of protonic acid HA to obtain a compound represented by formula III;

[0048]

[0049] 2) reacting the compound represented by formula III, allylamine, formaldehyde and glyoxal under the action of protonic acid HA to obtain the compound represented by formula IV;

[0050]

[0051] 3) subjecting the compound represented by formula IV to an ion exchange reaction with LiR to obtain the compound represented by formula I;

[0052] .

[0053] In the compounds of formula III and formula IV, the definitions and value ranges of m and n are the same as those for m and n in the compounds of formula I.

[0054] In the reaction of step 1), theoretically, 1 mol of formaldehyde, 1 mol of the compound shown in formula II and 1 mol of the acid radical of the protonic acid are required for every 1 mol of glyoxal, so that the imidazolium ionic liquid groups are connected to each other through the diamine compound shown in formula II. In the actual reaction, in order to allow both ends to be amino-terminated, the acid radicals in the compound shown in formula II and the protonic acid are usually excessive compared to glyoxal. Specifically, the degree of polymerization m can be adjusted by controlling the substrate concentration, reaction temperature, reaction time and other factors of the reaction solution.

[0055] Specifically, the protonic acid HA can be selected from protonic acids commonly used in the field of organic chemistry, including but not limited to acetic acid, hydrochloric acid, sulfuric acid, nitric acid or phosphoric acid.

[0056] The reaction in step 1) is preferably carried out in a solvent system, wherein the solvent can be selected from one or more of water, N-methylpyrrolidone, N-methylformamide, N-methylacetamide, N,N-dimethylformamide, sulfolane, and dimethyl sulfoxide.

[0057] After the reaction in step 1) is completed, the reaction solution needs to be purified. The purification process includes: distilling the reaction solution under reduced pressure and washing it to obtain the compound shown in formula III.

[0058] Then in step 2), allylamine, glyoxal, formaldehyde and protonic acid are added to the solvent system of the compound represented by formula III. Theoretically, 1 mol of formaldehyde, 0.5 mol of the compound represented by formula III, 1 mol of allylamine and 1 mol of the acid radical of the protonic acid are required for every 1 mol of glyoxal. In order to make the reaction more complete, the amount of allylamine and protonic acid can be appropriately excessive.

[0059] After the reaction in step 2) is completed, the reaction solution needs to be purified. The purification process includes: performing reduced pressure distillation and washing on the reaction solution to obtain the ionic liquid shown in formula VI.

[0060] The reaction in step 3) can be specifically carried out by referring to the following operation: the compound represented by formula VI is dissolved in water, and then added dropwise into an aqueous solution containing LiR, and stirred sufficiently to allow the A anion in formula IV to exchange with the R anion in the lithium salt LiR. After the precipitate is fully precipitated, the reaction is stopped, and the precipitate is washed with water and dried to obtain the compound represented by formula I.

[0061] The definition of R in LiR is consistent with the definition of R in the compound shown in Formula I.

[0062] The present invention does not specifically limit the free radical initiator used in the polymerization reaction, which can be selected from free radical initiators conventionally used in the art, including but not limited to peroxy free radical initiators, azo initiators or photoinitiators.

[0063] Furthermore, the amount of the free radical initiator can be 0.5% to 5% of the total mass of the compound represented by Formula I.

[0064] The above-mentioned polymerization reaction can be cross-linked and cured by heating the compound shown in Formula I, or can be cross-linked and cured by ultraviolet light irradiation. Preferably, the cross-linking and curing is achieved under heating conditions, and the heating temperature can be 60~100°C for 4~12h.

[0065] The present invention also provides a battery, comprising a positive electrode, a negative electrode and an electrolyte layer located between the positive electrode and the negative electrode, wherein the electrolyte layer comprises the polymer electrolyte as described above.

[0066] Since the polymer electrolyte of the present invention has high ionic conductivity, lithium ion transference number and mechanical strength, the battery also has excellent rate performance, cycling performance and safety performance.

[0067] The electrolyte layer of the present invention can be a solid electrolyte including only the above polymer electrolyte, or a semi-solid electrolyte in a gel state obtained by injecting an electrolyte solution into the above polymer electrolyte as a framework. Correspondingly, the obtained battery can be either a semi-solid battery or a solid battery.

[0068] It can be understood that the greater the thickness of the electrolyte layer, the better the safety performance of the battery. However, a larger thickness will also increase the resistance of lithium ion transmission, resulting in an increase in battery impedance, a deterioration in the rate performance of the battery, and a decrease in the energy density of the battery. Based on the above considerations, the thickness of the electrolyte layer is preferably 20~50μm. Exemplarily, the thickness of the electrolyte layer can be 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm or a range value composed of any two of the above numerical values.

[0069] Both the positive electrode and the negative electrode of the present invention can refer to the conventional positive and negative electrode compositions in the art.

[0070] Specifically, the positive electrode includes a positive electrode current collector and a positive electrode active material layer provided on at least one surface of the positive electrode current collector.

[0071] The present invention does not specifically limit the composition of the positive electrode current collector, which can be selected from the positive electrode current collectors commonly used in the art, such as aluminum foil.

[0072] In a specific embodiment, the positive electrode active material layer includes a positive electrode active material, a conductive agent, a binder, a lithium salt and a plasticizer.

[0073] The present invention does not specifically limit the types of the positive electrode active material, the conductive agent, the binder, the lithium salt and the plasticizer, and they can all be selected from the substances commonly used in the art.

[0074] Specifically, the positive electrode active material can be selected from lithium cobaltate (LiCoO2), lithium nickelate (LiNiO2), lithium iron phosphate (LiFePO4), lithium cobalt phosphate (LiCoPO4), lithium manganese phosphate (LiMnPO4), lithium nickel phosphate (LiNiPO4), lithium manganate (LiMnO2), binary material LiNi x A (1-x) O2 (A is selected from one of Co and Mn, 0<x<1), ternary material LiNi m B n C (1-m-n)One or more of O2 (B and C are independently selected from at least one of Co, Al, and Mn, and B and C are different, 0 < m < 1, 0 < n < 1).

[0075] The conductive agent can be selected from one or more of acetylene black, Super P, Super S, graphene, carbon fiber, carbon nanotube, and Ketjen black.

[0076] The binder can be selected from one or more of polyvinylidene fluoride, vinylidene fluoride - hexafluoropropylene copolymer, polytetrafluoroethylene, polyacrylonitrile, polypropylene carbonate, styrene - butadiene rubber, nitrile rubber, sodium carboxymethyl cellulose, polyethylene oxide, and ethylene oxide - propylene oxide copolymer.

[0077] The plasticizer can be selected from one or more of ethylene glycol dimethyl ether, ethylene glycol diethyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol diethyl ether, tetraethylene glycol diethyl ether, dipropylene glycol dimethyl ether, tripropylene glycol dimethyl ether, tetrapropylene glycol dimethyl ether, dipropylene glycol diethyl ether, tripropylene glycol diethyl ether, tetrapropylene glycol diethyl ether, 1,3 - dioxolane, 1,4 - dioxane, propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, butanedinitrile, and adiponitrile.

[0078] The selection of the lithium salt can refer to the types of lithium salts in polymer electrolytes, which will not be elaborated here.

[0079] In a preferred embodiment, the mass ratio of the cathode active material, conductive agent, binder, lithium salt, and plasticizer in the cathode active material layer is (50 - 90):(1 - 10):(9 - 20):(0 - 10):(0 - 10).

[0080] The anode includes an anode current collector and an anode active material layer provided on at least one surface of the anode current collector.

[0081] The present invention does not specifically limit the composition of the anode current collector, which can be selected from the anode current collectors commonly used in the art, such as copper foil.

[0082] In a specific embodiment, the anode active material layer includes an anode active material, a conductive agent, a binder, a lithium salt, and a plasticizer.

[0083] The present invention does not specifically limit the types of the anode active material, conductive agent, binder, lithium salt, and plasticizer, and they can all be selected from the substances commonly used in the art.

[0084] Specifically, the negative electrode active material can be selected from lithium metal, lithium metal alloy, graphite, silicon, silicon oxide, silicon carbon composite or silicon alloy. When the negative electrode active material is selected from lithium metal and lithium metal alloy, the negative electrode active material layer does not contain components such as conductive agent, binder, lithium salt and plasticizer.

[0085] The types of the conductive agent, binder, lithium salt and plasticizer in the negative electrode active material layer can refer to the selection of the conductive agent, binder, lithium salt and plasticizer in the positive electrode active material layer, and will not be repeated here.

[0086] In a preferred embodiment, the mass ratio of the negative electrode active material, the conductive agent, the binder, the lithium salt and the plasticizer in the negative electrode active material layer is (50-90): (1-10): (9-20): (0-10): (0-10).

[0087] The present invention does not impose any particular limitation on the method for preparing the battery, and the battery can be prepared by referring to conventional methods in the art.

[0088] For example, in a specific embodiment, a battery can be prepared by the following steps:

[0089] 1) dispersing a positive electrode active material, a conductive agent, a binder, a lithium salt and a plasticizer in a solvent according to a specific mass ratio to form a positive electrode active material layer slurry, then coating the positive electrode active material layer slurry on a positive electrode current collector, and drying to obtain a positive electrode;

[0090] 2) Compounding metallic lithium on the negative electrode current collector to obtain a negative electrode;

[0091] 3) The positive electrode, polymer electrolyte, and negative electrode are assembled in order to obtain a cell, and the battery is obtained after the cell is packaged.

[0092] The present invention also provides an electronic device, comprising the battery as described above. The present invention does not specifically limit the electronic device, which can be any electrical device comprising the battery, including but not limited to mobile phones, laptop computers, electric bicycles, electric cars, electric toys, energy storage devices, etc.

[0093] The polymer electrolyte provided by the present invention and its preparation method and application will be further described in detail below through specific examples.

[0094] Unless otherwise specified, the reagents, materials and instruments used in the following examples are conventional reagents, conventional materials and conventional instruments in the art and can be obtained commercially. The reagents involved can also be synthesized by conventional methods in the art.

[0095] In the following examples, the compounds represented by Formula II-1 to Formula II-7 were all purchased from Sigma-Aldrich.

[0096] Example 1

[0097] This embodiment provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is as follows:

[0098] 1. Preparation of polymer electrolyte

[0099] 1) Add acetic acid (1.1 mol) to an aqueous solution of the compound (1.1 mol) of formula II-1 to obtain a mixed solution; add a mixed solution of formaldehyde and glyoxal (1 mol of formaldehyde and 1 mol of glyoxal in the mixed solution) dropwise to the mixed solution under ice bath conditions; after the addition is complete, heat to 80°C and react for 2 hours to obtain a first reaction solution; cool the first reaction solution to room temperature, distill under reduced pressure, and wash with water to obtain a compound of formula III-1.

[0100]

[0101] 2) Add acetic acid (1.1 mol) to an aqueous solution of the compound represented by formula III-1 (0.5 mol) and allylamine (1.1 mol) to obtain a mixed solution; under ice bath conditions, add a mixed solution of formaldehyde and glyoxal (in the mixed solution, formaldehyde is 1 mol and glyoxal is 1 mol), and after the addition is completed, heat to 80°C and react for 0.5h to obtain a second reaction solution; after cooling the second reaction solution to room temperature, distill under reduced pressure and wash with water to obtain the compound represented by formula IV-1.

[0102]

[0103] 3) The compound represented by formula IV-1 (1 mol) is dissolved in water, and its aqueous solution is added to an aqueous solution of LiTFSI (1.2 mol) to react and generate a precipitate. The precipitate is washed and dried to obtain the compound represented by formula I-1.

[0104]

[0105] 4) The compound represented by formula I-1 and LiTFSI were mixed in a molar ratio of polyethylene glycol structural unit to LiTFSI of 18:1, and 0.5% of AIBN based on the mass of the compound represented by formula I-1 was added as an initiator, and the mixture was heated to 60° C. for polymerization for 4 hours to obtain a polymer electrolyte.

[0106] 2. Preparation of all-solid-state batteries

[0107] 1) Lithium iron phosphate, Super P, polyethylene oxide with a molecular weight of 600,000, lithium bis(trifluoromethylsulfonyl)imide and succinonitrile were mixed in N,N-dimethylformamide at a mass ratio of 78:2:10:5:5 to obtain a positive electrode active material layer slurry, and then the positive electrode active material layer slurry was applied on an aluminum current collector with a thickness of 15 μm with a scraper, and then dried at 60 ° C for 1 h and at 80 ° C for 3 h to obtain a positive electrode with a thickness of 75 μm, in which the surface loading of lithium iron phosphate was 15 mg / cm 2 .

[0108] 2) Cut the positive electrode prepared above into 4.5×6cm 2 , a 25 μm thick lithium-copper composite strip (lithium layer thickness 15 μm, copper layer thickness 10 μm) was used as the negative electrode and cut into 4.7×6.2 cm 2 The polymer electrolyte prepared above was cut into 4.8×6.3cm 2 , with a thickness of 40μm. In a glove box filled with argon (O2 content ≤ 0.5ppm, H2O content ≤ 0.5ppm), the battery cell is assembled in the order of positive electrode, polymer electrolyte, and lithium copper composite tape, and an all-solid-state battery is obtained after packaging.

[0109] Example 2

[0110] This embodiment provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that of Embodiment 1, except that, in the preparation of the polymer electrolyte, the compound represented by formula II-1 in step 1) is replaced by the compound represented by formula II-2, and correspondingly, the compound represented by formula I-2 is obtained in step 3), and the compound represented by formula I-1 is also replaced by the compound represented by formula I-2 in step 4).

[0111]

[0112] Example 3

[0113] This embodiment provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that of Embodiment 1, except that, in the preparation of the polymer electrolyte, the compound represented by formula II-3 in step 1) is replaced by the compound represented by formula II-2, and correspondingly, the compound represented by formula I-3 is obtained in step 3), and the compound represented by formula I-1 is also replaced by the compound represented by formula I-3 in step 4).

[0114]

[0115] Example 4

[0116] This embodiment provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that of Embodiment 1, except that, in the preparation of the polymer electrolyte, the compound represented by formula II-1 in step 1) is replaced by the compound represented by formula II-4, and correspondingly, the compound represented by formula I-4 is obtained in step 3), and the compound represented by formula I-1 is also replaced by the compound represented by formula I-4 in step 4).

[0117]

[0118] Example 5

[0119] This embodiment provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that of Embodiment 1, except that, in the preparation of the polymer electrolyte, the compound represented by formula II-1 in step 1) is replaced by the compound represented by formula II-5, and correspondingly, the compound represented by formula I-5 is obtained in step 3), and the compound represented by formula I-1 is also replaced by the compound represented by formula I-5 in step 4).

[0120]

[0121] Example 6

[0122] This embodiment provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that of Embodiment 1, except that, in the preparation of the polymer electrolyte, the reaction time of step 1) is adjusted to 1 h so that the compound obtained in step 3) is the compound represented by formula I-6, and in step 4), the compound represented by formula I-1 is replaced by the compound represented by formula I-6.

[0123]

[0124] Example 7

[0125] This embodiment provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that of Embodiment 1, except that, in the preparation of the polymer electrolyte, the reaction time of step 1) is adjusted to 3h so that the compound obtained in step 3) is the compound represented by formula I-7, and in step 4), the compound represented by formula I-1 is replaced by the compound represented by formula I-7.

[0126]

[0127] Example 8

[0128] This embodiment provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that of Embodiment 1, except that, in the preparation of the polymer electrolyte, the reaction time of step 1) is adjusted to 5 h so that the compound obtained in step 3) is the compound represented by formula I-8, and in step 4), the compound represented by formula I-1 is replaced by the compound represented by formula I-8.

[0129]

[0130] Example 9

[0131] This embodiment provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that of Example 1, except that, in the preparation of the polymer electrolyte, in step 4), the compound represented by formula I-1 and LiTFSI are replaced by a mixture of polyethylene glycol structural units and LiTFSI in a molar ratio of 10:1.

[0132] Example 10

[0133] This embodiment provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that of Example 1, except that, in the preparation of the polymer electrolyte, in step 4), the compound represented by formula I-1 and LiTFSI are replaced by a mixture of polyethylene glycol structural units and LiTFSI in a molar ratio of 25:1.

[0134] Embodiment 11

[0135] This embodiment provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that of Example 1, except that, in the preparation of the polymer electrolyte, in step 4), the compound represented by formula I-1 and LiTFSI are replaced by a mixture of polyethylene glycol structural units and LiTFSI in a molar ratio of 8:1.

[0136] Example 12

[0137] This embodiment provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that of Example 1, except that, in the preparation of the polymer electrolyte, in step 4), the compound represented by formula I-1 and LiTFSI are replaced by a mixture of polyethylene glycol structural units and LiTFSI in a molar ratio of 30:1.

[0138] Embodiment 13

[0139] This embodiment provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is substantially the same as that of Embodiment 1, except that, in the preparation of the all-solid-state battery, the thickness of the polymer electrolyte is replaced with 20 μm.

[0140] Embodiment 14

[0141] This embodiment provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that of Embodiment 1, except that in the preparation of the all-solid-state battery, the thickness of the polymer electrolyte is replaced with 50 μm.

[0142] Embodiment 15

[0143] This embodiment provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is substantially the same as that of Embodiment 1, except that, in the preparation of the all-solid-state battery, the thickness of the polymer electrolyte is replaced with 15 μm.

[0144] Example 16

[0145] This embodiment provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that of Embodiment 1, except that in the preparation of the all-solid-state battery, the thickness of the polymer electrolyte is replaced with 60 μm.

[0146] Embodiment 17

[0147] This embodiment provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is substantially the same as that of Embodiment 1, except that, in the preparation of the polymer electrolyte, LiTFSI in step 3) and step 4) is replaced by lithium perchlorate.

[0148] Comparative Example 1

[0149] This comparative example provides a polymer electrolyte and an all-solid-state battery. The polymer electrolyte used is obtained by mixing polyethylene oxide with a molecular weight of 600,000 and lithium bis(trifluoromethylsulfonyl)imide in a molar ratio of 18:1. The preparation process of the all-solid-state battery is basically the same as that in Example 1.

[0150] Comparative Example 2

[0151] This comparative example provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that in Example 1, except that, in the preparation of the polymer electrolyte, the compound represented by Formula I-1 is replaced by the compound represented by Formula A, and the obtained polymer is a cross-linked body of the compound represented by Formula A.

[0152]

[0153] Comparative Example 3

[0154] This comparative example provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that in Example 1, except that, in the preparation of the polymer electrolyte, the compound represented by formula II-1 in step 1) is replaced by the compound represented by formula II-6, and correspondingly, the compound represented by formula I-9 is obtained in step 3), and the compound represented by formula I-1 is also replaced by the compound represented by formula I-9 in step 4).

[0155]

[0156] Comparative Example 4

[0157] This comparative example provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that in Example 1, except that, in the preparation of the polymer electrolyte, the compound represented by formula II-1 in step 1) is replaced by the compound represented by formula II-7, and correspondingly, the compound represented by formula I-10 is obtained in step 3), and the compound represented by formula I-1 is also replaced by the compound represented by formula I-10 in step 4).

[0158]

[0159] Comparative Example 5

[0160] This comparative example provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that in Example 1, except that, in the preparation of the polymer electrolyte, the reaction time of step 1) is adjusted to 0.5 h so that the compound obtained in step 3) is the compound represented by formula I-11, and in step 4), the compound represented by formula I-1 is replaced by the compound represented by formula I-11.

[0161]

[0162] Comparative Example 6

[0163] This comparative example provides a polymer electrolyte and an all-solid-state battery, and the preparation method thereof is basically the same as that in Example 1, except that, in the preparation of the polymer electrolyte, the reaction time of step 1) is adjusted to 5h so that the compound obtained in step 3) is the compound represented by formula I-12, and in step 4), the compound represented by formula I-1 is replaced by the compound represented by formula I-12.

[0164]

[0165] Comparative Example 7

[0166] The solid electrolyte is obtained by mixing the compound represented by formula I-1 and LiTFSI in a molar ratio of 18:1.

[0167] Test Case

[0168] 1. The following properties of the polymer electrolytes prepared in the above examples and comparative examples were tested:

[0169] 1. Lithium ion migration number

[0170] Test method: Use a lithium sheet with a diameter of 16 mm as an electrode, cut the polymer electrolyte into a disc with a diameter of 19 mm, assemble it into a Li||Li symmetric battery, and test the lithium ion migration number and ion conductivity of the Li||Li symmetric battery. Use an electrochemical workstation to apply a polarization voltage of 10 mV to the battery, and the polarization time is 2 hours. Test the current and impedance of the symmetric battery before and after polarization, and calculate the lithium ion migration number according to the following formula.

[0171]

[0172] Among them, t + is the lithium ion migration number, I0 and I ss are the current before polarization begins and the current after polarization stabilizes, R0 and R ss are the impedance before polarization begins and the impedance after polarization stabilizes, and ∆V is the polarization voltage.

[0173] 2. Ionic conductivity

[0174] Test method: Use a punching machine to cut stainless steel sheets with a diameter of 16 mm and a thickness of 200 μm, and a polymer electrolyte membrane with a diameter of 19 mm; stack the stainless steel sheets and polymer electrolyte membrane in order, so that the polymer electrolyte membrane is between the stainless steel sheets, and assemble a stainless steel symmetrical battery. Put the stainless steel symmetrical battery in a 60°C oven for 10 minutes and then test the impedance of the stainless steel symmetrical battery.

[0175] The ionic conductivity of the polymer electrolyte was calculated according to the following formula:

[0176]

[0177] Where σ is the ionic conductivity of the electrolyte, L is the thickness of the polymer electrolyte membrane, S is the area of ​​the stainless steel sheet, and R is the impedance of the stainless steel symmetric cell.

[0178] The above test results are shown in Table 1.

[0179] 2. The following performance tests were performed on the all-solid-state batteries prepared in the above embodiments and comparative examples:

[0180] 1. Cycle performance

[0181] Test method: At 60℃, charge the battery to 3.8V at a constant current rate of 0.05C, let it stand for 5 minutes, and then discharge it to 2.5V at a constant current rate of 0.05C, and repeat the above process 3 times. Then charge it to 3.8V at a constant current rate of 0.2C, and charge it to 0.01C at a constant voltage of 3.8V, let it stand for 5 minutes, and finally discharge it to 2.5V at a rate of 0.2C, and let it stand for 5 minutes. The cycle is terminated when the specific capacity of the battery is 80% of the initial capacity, and the number of cycles at this time is recorded.

[0182] 2. Rate performance

[0183] Test method: At 60°C, charge the battery to 3.8V at a constant current of 0.05C, let it stand for 5 minutes, and then discharge it to 2.5V at a constant current of 0.05C. Repeat the above process 3 times. Then charge it to 3.8V at a rate of 0.1C, let it stand for 5 minutes, then discharge it to 2.5V at a rate of 0.1C, let it stand for 5 minutes, then charge it to 3.8V at a rate of 0.5C, record the charging capacity of 0.5C and 0.1C, and calculate the 0.5C / 0.1C rate charging capacity retention rate by 0.5C charging capacity / 0.1C charging capacity.

[0184] The test results of the above values ​​are listed in Table 1.

[0185] Table 1

[0186]

[0187] The following conclusions can be drawn from Table 1:

[0188] 1) From the comparison of Examples 1 to 8 and Comparative Examples 3 to 6, it can be seen that the proportion of imidazolium ionic liquid units in the polymer electrolyte has a significant effect on the lithium ion migration number. The greater the proportion of imidazolium ionic liquid units, the higher the lithium ion migration number. The content of polyethylene glycol chain segments has a significant effect on the ionic conductivity of the polymer electrolyte. Among them, the cycle performance of the battery is related to the ionic conductivity and the lithium ion migration number, and the rate performance of the battery is mainly related to the ionic conductivity.

[0189] Specifically, the larger n is (Comparative Example 4), the smaller the proportion of the imidazolium ionic liquid unit is, the corresponding lithium ion migration number will decrease, and the polyethylene glycol structural unit will be easy to crystallize, thereby making the ionic conductivity of the polymer electrolyte worse. If n is too small (Comparative Example 3), there will be too few polyethylene glycol segments, making it difficult to transport lithium ions, and thus causing the ionic conductivity to deteriorate. m will affect the length of the segment between the two terminal vinyl groups. If m is too large (Comparative Example 6), the mechanical strength of the polymer electrolyte will be reduced, making the battery prone to short circuit and the cycle performance to deteriorate. If m is too small (Comparative Example 5), the polymer electrolyte will be too rigid, with poor compatibility with the positive and negative electrode interfaces, poor contact, and will not be conducive to the battery's cycle performance and rate performance.

[0190] Embodiments 1 to 8 have suitable n and m values, so the polymer electrolyte has both excellent lithium ion migration number and ionic conductivity, and accordingly, the battery has both excellent cycle performance and rate performance; especially when m is in the range of 15 to 30, n is in the range of 8 to 25, and the product of m and n is 100 to 750, the performance of embodiments 1, 3, 4, 5, 7, and 8 is more excellent.

[0191] 2) From the comparison of Examples 1 and 9 to 12, it can be seen that when the molar ratio of the compound represented by Formula I-1 and LiTFSI is in the range of (10 to 25): 1, the polymer electrolyte has excellent lithium ion migration number and ionic conductivity, and the battery also has excellent cycle performance and rate performance. However, when the molar ratio of the two is outside the above range, such as 8: 1 and 30: 1, respectively, the lithium salt content is too much or too little. When the lithium salt content is too much, the lithium salt cannot be dissociated, resulting in a small number of lithium ions that can be dissociated and transmitted. When the lithium salt content is too little, it will also lead to a small number of lithium ions transmitted, which in turn leads to a low lithium ion migration number and ionic conductivity of the polymer electrolyte, and the battery cycle performance and rate performance are also relatively poor.

[0192] 3) From the comparison of Examples 1 and 13 to 16, it can be seen that the thickness of the polymer electrolyte layer has a certain influence on the cycle performance and rate performance of the battery. When the thickness of the polymer electrolyte is within 20 to 50 μm, the battery can have both relatively excellent cycle performance and rate performance. When the thickness of the polymer electrolyte is low (15 μm), the transmission path of lithium ions is shorter, and the battery has a more excellent rate performance, but the battery is more prone to short circuit, resulting in poor cycle performance. When the thickness of the polymer electrolyte is high (60 μm), the battery is not prone to short circuit and has better cycle performance, but the transmission path of lithium ions is longer, resulting in poor rate performance of the battery.

[0193] 4) From the comparison between Examples 1 and 17, it can be seen that different types of lithium salts and R anions can make the polymer electrolyte have both excellent lithium ion transference number and ion conductivity, and the battery has both excellent cycle performance and rate performance.

[0194] 5) From the comparison between Example 1 and Comparative Example 1, it can be seen that the lithium ion transfer number and ion conductivity of the polymer electrolyte obtained by mixing unmodified polyethylene oxide with LiTFSI are poor, and the cycle performance and rate performance of the battery are also poor.

[0195] 6) From the comparison between Example 1 and Comparative Example 2, it can be seen that when the polymerized monomer does not contain imidazolium ionic liquid units, excessive polyethylene glycol structural units are prone to crystallization, resulting in poor lithium ion migration number and ionic conductivity of the electrolyte, and thus poor cycle performance and rate performance.

[0196] 7) From the comparison between Example 1 and Comparative Example 7, it can be seen that the cycle performance of the electrolyte prepared by using only the lithium salt obtained by mixing the compound represented by Formula I-1 and LiTFSI is significantly poor. The reason is that when the compound represented by Formula I-1 is not cross-linked, the mechanical strength of the obtained electrolyte is low and it is easy to short-circuit, which leads to poor battery cycle performance.

[0197] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments may still be modified, or some or all of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A polymer electrolyte comprising a polymer and a lithium salt, characterized in that: The polymer includes a cross-linked product obtained by polymerizing the compound shown in Formula I: , In formula I, R is selected from bistrifluoromethylsulfonyl imide, bisfluorosulfonyl imide, perchlorate, tetrafluoroborate, dioxalatoborate, difluorooxalatoborate or trifluoromethylsulfonate; m is selected from an integer between 10 and 50, and n is selected from an integer between 4 and 30.

2. The polymer electrolyte according to claim 1, characterized in that 15≤m≤30, and / or, 8≤n≤25.

3. The polymer electrolyte according to claim 1 or 2, characterized in that 100≤m×n≤750.

4. The polymer electrolyte according to claim 1, characterized in that The molar ratio of the polyethylene glycol structural unit to the lithium salt in the compound of formula I is (10-25):

1.

5. The polymer electrolyte according to claim 1 or 4, characterized in that The lithium salt includes one or more of lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium dioxalatoborate, and lithium perchlorate.

6. A method for preparing a polymer electrolyte according to any one of claims 1 to 5, characterized in that: The following steps are involved: A free radical initiator is added to a mixed system of the compound shown in formula I and a lithium salt to initiate a polymerization reaction to obtain the polymer electrolyte.

7. The preparation method according to claim 6, characterized in that: The compound represented by formula I is prepared by a method comprising the following steps: 1) reacting the compound represented by formula II, formaldehyde and glyoxal under the action of protonic acid HA to obtain a compound represented by formula III; , 2) reacting the compound represented by formula III, allylamine, formaldehyde and glyoxal under the action of protonic acid HA to obtain the compound represented by formula IV; , 3) subjecting the compound represented by formula IV to an ion exchange reaction with LiR to obtain the compound represented by formula I; 。 8. The preparation method according to claim 6, characterized in that: The polymerization reaction temperature is 60-100° C. and the reaction time is 4-12 hours.

9. A battery comprising a positive electrode, a negative electrode and an electrolyte layer between the positive electrode and the negative electrode, characterized in that: The electrolyte layer comprises the polymer electrolyte according to any one of claims 1 to 5.

10. The battery according to claim 9, characterized in that The thickness of the electrolyte layer is 20-50 μm.

11. An electronic device, characterized in that: A battery comprising the battery of claim 9 or 10.

Citation Information

Patent Citations

  • Novel ionic liquid and preparation method thereof

    CN105261786A

  • Bi-imidazole ring functional ionic liquid, preparing method thereof, electrolyte and lithium secondary battery

    CN109776423A